A high-strength, long-lasting mildew-proof mortar material and its preparation method and application

A high-strength, long-lasting mildew-proof mortar material with tartaric acid-modified oyster shell powder and vanillin-hexacyclotetrafluoroethylene composite enhances mold inhibition and mechanical stability, overcoming the limitations of existing mortar materials.

CN118637873BActive Publication Date: 2024-12-06BEIJING ECO HOME (LETING) TECH DEV CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411102943.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-06
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing mildew-proof mortar materials exhibit low anti-mildew rates, poor mechanical properties, and short duration of anti-mildew effect, especially in humid environments.

Method used

A high-strength and long-lasting mildew-proof mortar material is prepared using cement, epoxy resin, tartaric acid-modified oyster shell powder, and vanillin-hexacyclotetrafluoroethylene composite material, combined with additives like water reducer and dispersant, to enhance mold inhibition and mechanical stability.

Benefits of technology

The mortar material achieves long-term, efficient mold resistance and maintains excellent mechanical properties in humid conditions, addressing the limitations of prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and specifically discloses a high-strength long-acting mildew-proof mortar material and its preparation method and application. The high-strength long-acting mildew-proof mortar material includes the following raw material components: cement, lime powder, quartz sand, water reducer, dispersant, stabilizer, tartaric acid modified oyster shell powder, vanillin-hexacyclic stone composite material, epoxy resin and water. The tartaric acid modified oyster shell powder and vanillin-hexacyclic stone composite material can inhibit the growth of mold efficiently and stably for a long time. Combined with other raw material components, the obtained mortar material can not only maintain a long-acting mildew-proof effect, but also has good compressive and flexural strength. The present invention can effectively solve the problems in the prior art that the mildew-proof mortar material has a low anti-mildew rate, poor mechanical properties and stability in a humid environment, and a short duration of anti-mildew effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and specifically discloses a high-strength and long-acting mildew-proof mortar material and a preparation method and application thereof. Background Art

[0002] Mortar is the most widely used material in building materials, including housing construction, bridges, tunnels, and urban infrastructure. Decorative mortar, in particular, as the exterior finish of a building, not only gives the building a rich appearance, but also forms a barrier to protect the wall from environmental damage. When mortar is in a humid environment or water seepage occurs, it is very easy to breed bacteria and mold, which not only seriously affects the appearance of the wall, causing the wall surface to be uneven, but also seriously affects environmental hygiene and shortens the service life of the mortar material. Therefore, how to improve the mildew resistance of mortar materials has become an important topic in the field of existing building materials research and development.

[0003] In order to enhance the mildew resistance of mortar in the prior art, the density of the raw materials of the mortar material can be adjusted or a hydrophobic agent can be introduced to enhance the hydrophobic function of the mortar material, thereby ensuring that its structure is dense and water vapor is difficult to enter, thereby inhibiting the growth of mold. However, this only slows down the growth rate of mold and cannot completely prevent the formation of mold. There are also reports that mildew inhibitors or bactericides are introduced into mortar materials, but the mildew resistance rate of the obtained mortar material is low, the mechanical properties and stability deteriorate in a humid environment, and the duration of the mildew resistance effect is short. Based on this, the development of a mortar material that can efficiently and stably resist mildew has great practical significance in the field of new building materials. Summary of the invention

[0004] In view of the problems in the prior art that the mildew-proof mortar materials have low anti-mildew rate, poor mechanical properties and stability in a humid environment, and short duration of anti-mildew effect, the present invention provides a high-strength and long-lasting mildew-proof mortar material and its preparation method and application. The high-strength and long-lasting mildew-proof mortar material is prepared with cement and epoxy resin as gelling materials; lime powder, quartz sand, tartaric acid-modified oyster shell powder and vanillin-hexacyclotetrafluoroethylene composite material as aggregates; water reducer, dispersant and stabilizer as additives. The tartaric acid-modified oyster shell powder and vanillin-hexacyclotetrafluoroethylene composite material can inhibit the growth of mold efficiently and stably for a long time. Combined with other raw material components, the obtained mortar material not only has excellent compressive and flexural strength, but also can maintain a long-lasting and stable mildew-proof effect.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The first aspect of the present invention provides a high-strength and long-lasting mildew-proof mortar material, comprising the following raw material components in parts by weight: 70-90 parts of cement, 40-60 parts of lime powder, 100-120 parts of quartz sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 1-2 parts of stabilizer, 20-30 parts of tartaric acid modified oyster shell powder, 10-20 parts of vanillin-hexacyclotetrafluoroethylene composite material, 30-50 parts of epoxy resin and 70-100 parts of water.

[0007] Oyster shells contain a large amount of calcium carbonate and part of chitin. The chitosan formed after chitin deacetylation has a strong bactericidal ability. Therefore, oyster shells are a low-cost antifungal material. However, oyster shells need to be calcined before use. During the calcination process, due to the decomposition of calcium carbonate, its original structure collapses and the pore structure is destroyed, which greatly reduces its antifungal ability. Based on this, the present invention uses tartaric acid to modify it. After tartaric acid modification, the total specific surface area, micropore specific surface area and total pore volume of oyster shells are significantly increased, and the number of micropores increases. This is because tartaric acid can slightly dissolve part of the calcium carbonate, etch the oyster shell, increase the number of pores and pore volume, and enhance the ability to adsorb and degrade mold. In addition, tartaric acid can also promote the deacetylation of chitin to form chitosan, thereby greatly improving the antifungal ability of oyster shells. In addition, oyster shells contain a large amount of calcium carbonate and have a high hardness, which can give the mortar material a higher compressive strength and flexural strength, allowing the mortar material to maintain excellent mechanical properties even in a relatively humid environment.

[0008] The present invention also designs a vanillin-six ring stone composite material, and the six ring stone has the ability to permanently release negative ions, can kill mold, and purify the air. However, the amount of negative ions released by the six ring stone is limited, and the amount of mold killing is also limited. In order to further improve the sterilization effect of the mortar material, the present invention loads vanillin on the surface of the six ring stone, and vanillin can destroy the mold cell membrane and the outer membrane of the mold mitochondria, and affect the transportation of substances inside and outside the mitochondria, thereby inhibiting the growth of mold, and combining the six ring stone that can release negative ions, greatly improving the antibacterial and sterilization effect of the vanillin-six ring stone composite material, thereby improving the long-term anti-mold ability of the mortar material. Further, the main components of the six ring stone are calcite and limonite, and the structure is dense, and it can be used as a filler to make up for the pores of the mortar material and improve the mechanical properties of the mortar material.

[0009] The present invention also adopts cement, lime powder, quartz sand and epoxy resin as main materials, combined with tartaric acid modified oyster shell powder, vanillin-hexacyclotetrafluoroethylene composite material and various additives. Through the synergistic effect of each component, the obtained mortar material not only has long-term stable and efficient mildew resistance, but also can maintain excellent mechanical properties in a humid environment, providing new ideas for new building materials.

[0010] Preferably, the method for preparing the tartaric acid modified oyster shell powder comprises the following steps:

[0011] S1, cleaning the oyster shells, immersing them in an alkaline solution, separating the solid and the liquid, washing, drying and then ball milling to obtain pretreated oyster shell powder;

[0012] S2, heating the oyster shell powder to 850° C.-950° C. for calcination, and grinding to obtain activated oyster shell powder;

[0013] S3, dispersing the activated oyster shell powder in an alcohol solution, adding tartaric acid, and performing a hydrothermal reaction at 100° C.-140° C. to obtain tartaric acid-modified oyster shell powder.

[0014] Further preferably, in S1, the alkaline solution is a 0.05 mol / L-0.1 mol / L sodium hydroxide solution.

[0015] Further preferably, in S1, the mass volume ratio of the oyster shell to the alkaline solution is 1g:5mL-1g:8mL.

[0016] Further preferably, in S1, the immersion time is 12h-20h.

[0017] Further preferably, in S1, the drying temperature is 90°C-120°C, and the drying time is 3h-6h.

[0018] Further preferably, in S1, the rotation speed of the ball mill is 800 rpm-1200 rpm, and the ball milling time is 30 min-50 min.

[0019] Further preferably, in S2, the temperature is increased by programmed temperature increase, and the rate of temperature increase is 15°C / min-25°C / min.

[0020] Further preferably, in S2, the calcination treatment time is 4h-6h.

[0021] Further preferably, in S3, the alcohol solution is a 65%-75% ethanol solution.

[0022] Further preferably, in S3, the mass volume ratio of the activated oyster shell powder to the alcohol solution is 1g:3mL-1g:5mL.

[0023] Further preferably, in S3, the mass ratio of the activated oyster shell powder to the tartaric acid is 1:0.5-1:0.8.

[0024] Further preferably, in S3, the hydrothermal reaction time is 2h-4h.

[0025] Preferably, the preparation method of the vanillin-hexacyclopentasiloxane composite material comprises the following steps:

[0026] Step a, ball-milling the hexacyclic stone, dispersing it in an amide solvent, adding a surfactant, and performing a coupling reaction at 60° C.-70° C. to obtain activated hexacyclic stone powder;

[0027] Step b, dispersing the activated hexacyclopaste powder in an alkaline solution, adding vanillin, carrying out a hydrothermal reaction at 90° C.-110° C., filtering, washing, and drying to obtain a vanillin-hexacyclopaste composite material.

[0028] Further preferably, in step a, the rotation speed of the ball mill is 500 rpm-700 rpm, and the ball milling time is 20 min-30 min.

[0029] Further preferably, in step a, the amide solvent is N'N-dimethylformamide.

[0030] Further preferably, in step a, the surfactant is 3-amino-1,2-propanediol.

[0031] Further preferably, in step a, the mass volume ratio of the hexacyclostone to the amide solvent is 1g:3mL-1g:5mL.

[0032] Further preferably, in step a, the mass ratio of the hexacyclostone to the surfactant is 1:0.8-1:1.2.

[0033] Further preferably, in step a, the coupling reaction time is 2h-4h.

[0034] Further preferably, in step b, the alkaline solution is a 0.1 mol / L-0.2 mol / L sodium hydroxide solution.

[0035] Further preferably, in step b, the mass volume ratio of the activated hexacyclic stone powder to the alkaline solution is 1g:2mL-1g:4mL.

[0036] Further preferably, in step b, the mass ratio of the activated hexacyclopentasiloxane powder to the vanillin is 1:0.4-1:0.7.

[0037] Further preferably, in step b, the hydrothermal reaction time is 2h-5h.

[0038] Preferably, the cement is Portland cement.

[0039] Preferably, the particle size of the lime powder is 0.1 mm-0.3 mm.

[0040] Preferably, the particle size of the quartz sand is 0.2 mm-0.5 mm.

[0041] Preferably, the water reducer is any one of a sodium lignin sulfonate water reducer, a naphthalene-based high-efficiency water reducer, an aliphatic high-efficiency water reducer, an amino high-efficiency water reducer or a polycarboxylic acid high-efficiency water reducer.

[0042] Preferably, the dispersant is a fatty acid dispersant.

[0043] Preferably, the stabilizer is any one of EL0002, TAB-2 or T-386.

[0044] The second aspect of the present invention provides a method for preparing the high-strength and long-lasting mildew-proof mortar material, comprising the following steps: weighing each raw material component according to the designed ratio, and mixing the weighed components evenly to obtain the high-strength and long-lasting mildew-proof mortar material.

[0045] The third aspect of the present invention provides the use of the high-strength and long-acting mildew-proof mortar material or the high-strength and long-acting mildew-proof mortar material prepared by the preparation method of the high-strength and long-acting mildew-proof mortar material in the field of building materials.

[0046] In summary, the present invention uses cement and epoxy resin as cementitious materials; lime powder, quartz sand, tartaric acid modified oyster shell powder and vanillin-hexacyclic stone composite material as aggregates; water reducer, dispersant and stabilizer are used as additives to prepare a high-strength and long-lasting mildew-proof mortar material. The tartaric acid modified oyster shell powder and vanillin-hexacyclic stone composite material can achieve long-term, efficient and stable inhibition of mold growth. Combined with other raw material components, the resulting mortar material not only has a long-term, stable and efficient mildew-proof effect, but also has excellent mechanical properties in a humid environment. The use of this mortar material can effectively solve the problems of low mildew-proof rate, poor mechanical properties and stability in a humid environment, and short duration of anti-mildew effect in mildew-proof mortar materials in the prior art. DETAILED DESCRIPTION

[0047] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] This embodiment provides a high-strength and long-lasting mildew-proof mortar material and a preparation method thereof, which specifically includes the following contents:

[0050] The high-strength and long-lasting mildew-proof mortar material comprises the following raw material components by weight: 80 parts of silicate cement, 50 parts of lime powder, 110 parts of quartz sand, 1.5 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 25 parts of tartaric acid modified oyster shell powder, 15 parts of vanillin-hexacyclic stone composite material, 1 part of EL0002 stabilizer, 40 parts of epoxy resin and 80 parts of water;

[0051] Weigh each raw material component according to the designed proportion, mix the weighed components evenly, and obtain a high-strength and long-lasting mildew-proof mortar material.

[0052] The preparation method of the tartaric acid modified oyster shell powder comprises the following steps:

[0053] S1. Clean 100 g of oyster shells, immerse them in 600 mL of 0.08 mol / L sodium hydroxide solution for 18 h, filter, wash the solid filtrate with water, dry it at 100 ° C for 4 h, and ball mill it at a speed of 1000 rpm for 40 min to obtain pretreated oyster shell powder;

[0054] S2, heating the oyster shell powder to 900° C. at a heating rate of 20° C. / min, calcining the powder for 5 h, and grinding the powder to obtain activated oyster shell powder;

[0055] S3, dispersing the activated oyster shell powder in 350 mL of 70% ethanol solution, adding 80 g of tartaric acid, and performing a hydrothermal reaction at 120° C. for 3 h to obtain tartaric acid-modified oyster shell powder.

[0056] The preparation method of the vanillin-hexacyclopentadienyl composite material comprises the following steps:

[0057] Step a, ball mill 100g of hexacyclolith at a speed of 600rpm for 25min, disperse it in 400mL N'N-dimethylformamide, add 100g of 3-amino-1,2-propanediol, and carry out coupling reaction at 65°C for 3h to obtain activated hexacyclolith powder;

[0058] Step b, dispersing the activated hexacyclolith powder in 250 mL of 0.15 mol / L sodium hydroxide solution, adding 60 g of vanillin, performing hydrothermal reaction at 100° C. for 4 h, filtering, washing, and drying at 90° C. for 6 h to obtain a vanillin-hexacyclolith composite material.

[0059] The particle size of the lime powder is 0.3 mm; the particle size of the quartz sand is 0.4 mm.

[0060] Example 2

[0061] This embodiment provides a high-strength and long-lasting mildew-proof mortar material and a preparation method thereof, which specifically includes the following contents:

[0062] The high-strength and long-lasting mildew-proof mortar material comprises the following raw material components in parts by weight: 90 parts of silicate cement, 40 parts of lime powder, 100 parts of quartz sand, 2 parts of polycarboxylic acid high-efficiency water reducing agent, 4 parts of fatty acid dispersant, 20 parts of tartaric acid-modified oyster shell powder, 15 parts of vanillin-hexacyclotetrafluoroethylene composite material, 1 part of EL0002 stabilizer, 40 parts of epoxy resin and 80 parts of water;

[0063] Weigh each raw material component according to the designed proportion, mix the weighed components evenly, and obtain a high-strength and long-lasting mildew-proof mortar material.

[0064] The preparation method of the tartaric acid modified oyster shell powder comprises the following steps:

[0065] S1. Clean 100 g of oyster shells, immerse them in 600 mL of 0.08 mol / L sodium hydroxide solution for 18 h, filter, wash the solid filtrate with water, dry it at 100 ° C for 4 h, and ball mill it at a speed of 1200 rpm for 30 min to obtain pretreated oyster shell powder;

[0066] S2, heating the oyster shell powder to 900° C. at a heating rate of 20° C. / min, calcining the powder for 5 h, and grinding the powder to obtain activated oyster shell powder;

[0067] S3, dispersing the activated oyster shell powder in 350 mL of 70% ethanol solution, adding 80 g of tartaric acid, and performing a hydrothermal reaction at 120° C. for 3 h to obtain tartaric acid-modified oyster shell powder.

[0068] The preparation method of the vanillin-hexacyclopentadienyl composite material comprises the following steps:

[0069] Step a, ball mill 100g of hexacyclolith at a speed of 600rpm for 25min, disperse it in 400mL N'N-dimethylformamide, add 100g of 3-amino-1,2-propanediol, and carry out coupling reaction at 65°C for 3h to obtain activated hexacyclolith powder;

[0070] Step b, dispersing the activated hexacyclolith powder in 250 mL of 0.15 mol / L sodium hydroxide solution, adding 60 g of vanillin, performing hydrothermal reaction at 100° C. for 4 h, filtering, washing, and drying at 90° C. for 6 h to obtain a vanillin-hexacyclolith composite material.

[0071] The particle size of the lime powder is 0.3 mm; the particle size of the quartz sand is 0.3 mm.

[0072] Example 3

[0073] This embodiment provides a high-strength and long-lasting mildew-proof mortar material and a preparation method thereof, which specifically includes the following contents:

[0074] The high-strength and long-lasting mildew-proof mortar material comprises the following raw material components by weight: 80 parts of silicate cement, 60 parts of lime powder, 120 parts of quartz sand, 1.5 parts of naphthalene-based high-efficiency water reducer, 4 parts of fatty acid dispersant, 30 parts of tartaric acid-modified oyster shell powder, 20 parts of vanillin-hexacyclotetrafluoroethylene composite material, 1 part of EL0002 stabilizer, 40 parts of epoxy resin and 90 parts of water;

[0075] Weigh each raw material component according to the designed proportion, mix the weighed components evenly, and obtain a high-strength and long-lasting mildew-proof mortar material.

[0076] The preparation method of the tartaric acid modified oyster shell powder comprises the following steps:

[0077] S1. Clean 100 g of oyster shells, immerse them in 600 mL of 0.08 mol / L sodium hydroxide solution for 18 h, filter, wash the solid filtrate with water, dry it at 100 ° C for 4 h, and ball mill it at a speed of 900 rpm for 50 min to obtain pretreated oyster shell powder;

[0078] S2, heating the oyster shell powder to 900° C. at a heating rate of 20° C. / min, calcining the powder for 5 h, and grinding the powder to obtain activated oyster shell powder;

[0079] S3, dispersing the activated oyster shell powder in 350 mL of 70% ethanol solution, adding 80 g of tartaric acid, and performing a hydrothermal reaction at 120° C. for 3 h to obtain tartaric acid-modified oyster shell powder.

[0080] The preparation method of the vanillin-hexacyclopentadienyl composite material comprises the following steps:

[0081] Step a, ball mill 100g of hexacyclolith at a speed of 600rpm for 25min, disperse it in 400mL N'N-dimethylformamide, add 100g of 3-amino-1,2-propanediol, and carry out coupling reaction at 65°C for 3h to obtain activated hexacyclolith powder;

[0082] Step b, dispersing the activated hexacyclolith powder in 250 mL of 0.15 mol / L sodium hydroxide solution, adding 60 g of vanillin, performing hydrothermal reaction at 100° C. for 4 h, filtering, washing, and drying at 90° C. for 6 h to obtain a vanillin-hexacyclolith composite material.

[0083] The particle size of the lime powder is 0.2 mm; the particle size of the quartz sand is 0.4 mm.

[0084] Comparative Example 1

[0085] This comparative example provides a high-strength and long-lasting mildew-proof mortar material and a preparation method thereof, which is different from Example 1 in that the tartaric acid-modified oyster shell powder is replaced with an equal amount of oyster shell powder, and other components and processes remain unchanged, specifically including the following contents:

[0086] The high-strength, long-lasting mildew-proof mortar material comprises the following raw material components by weight: 80 parts of silicate cement, 50 parts of lime powder, 110 parts of quartz sand, 1.5 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 25 parts of oyster shell powder, 15 parts of vanillin-hexacyclic stone composite material, 1 part of EL0002 stabilizer, 40 parts of epoxy resin and 80 parts of water;

[0087] Weigh each raw material component according to the designed proportion, mix the weighed components evenly, and obtain a high-strength and long-lasting mildew-proof mortar material.

[0088] The preparation method of the vanillin-hexacyclopentadienyl composite material comprises the following steps:

[0089] Step a, ball mill 100g of hexacyclolith at a speed of 600rpm for 25min, disperse it in 400mL N'N-dimethylformamide, add 100g of 3-amino-1,2-propanediol, and carry out coupling reaction at 65°C for 3h to obtain activated hexacyclolith powder;

[0090] Step b, dispersing the activated hexacyclolith powder in 250 mL of 0.15 mol / L sodium hydroxide solution, adding 60 g of vanillin, performing hydrothermal reaction at 100° C. for 4 h, filtering, washing, and drying at 90° C. for 6 h to obtain a vanillin-hexacyclolith composite material.

[0091] The particle size of the lime powder is 0.3 mm; the particle size of the quartz sand is 0.4 mm.

[0092] Comparative Example 2

[0093] This comparative example provides a high-strength and long-lasting mildew-proof mortar material and a preparation method thereof, which is different from Example 1 in that the vanillin-hexacyclotetrafluoroethylene composite material is replaced with an equal amount of hexacyclotetrafluoroethylene powder, and other components and processes remain unchanged, specifically including the following contents:

[0094] The high-strength, long-lasting, mildew-proof mortar material comprises the following raw material components by weight: 80 parts of Portland cement, 50 parts of lime powder, 110 parts of quartz sand, 1.5 parts of sodium lignin sulfonate water reducer, 4 parts of fatty acid dispersant, 25 parts of tartaric acid-modified oyster shell powder, 15 parts of hexacyclic stone powder, 1 part of EL0002 stabilizer, 40 parts of epoxy resin and 80 parts of water;

[0095] Weigh each raw material component according to the designed proportion, mix the weighed components evenly, and obtain a high-strength and long-lasting mildew-proof mortar material.

[0096] The preparation method of the tartaric acid modified oyster shell powder comprises the following steps:

[0097] S1. Clean 100 g of oyster shells, immerse them in 600 mL of 0.08 mol / L sodium hydroxide solution for 18 h, filter, wash the solid filtrate with water, dry it at 100 ° C for 4 h, and ball mill it at a speed of 1000 rpm for 40 min to obtain pretreated oyster shell powder;

[0098] S2, heating the oyster shell powder to 900° C. at a heating rate of 20° C. / min, calcining the powder for 5 h, and grinding the powder to obtain activated oyster shell powder;

[0099] S3, dispersing the activated oyster shell powder in 350 mL of 70% ethanol solution, adding 80 g of tartaric acid, and performing a hydrothermal reaction at 120° C. for 3 h to obtain tartaric acid-modified oyster shell powder.

[0100] The particle size of the lime powder is 0.3 mm; the particle size of the quartz sand is 0.4 mm.

[0101] In order to further reflect the technical effect of the present invention, the present invention conducted the following tests on the mortar materials obtained in Examples 1-3 and Comparative Examples 1-2: the flexural strength, compressive strength and bonding strength of the mortar samples were tested according to the standard JC / T2497-2018; the results are shown in Table 1.

[0102] Table 1 Performance test results of various mortar materials

[0103]

[0104] Anti-mildew effect test: According to GB / T 1741-2009, the mortar materials provided in each embodiment and the comparative example were subjected to an anti-mildew test, and were cultured for 28 days at 28°C and an ambient humidity of 90%. In order to further demonstrate the long-term anti-mildew effect of the present invention, the mortar materials provided in each embodiment and the comparative example were subjected to a long-term anti-mildew test according to GB / T 1741-2009 standard, and were cultured for 90 days at 28°C and an ambient humidity of 90%. The test results are shown in Table 2.

[0105] Table 2 Anti-mildew test results

[0106]

[0107] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength and long-lasting mildew-proof mortar material, characterized in that: The invention comprises the following raw material components in parts by weight: 70-90 parts of cement, 40-60 parts of lime powder, 100-120 parts of quartz sand, 1-2 parts of water reducer, 3-5 parts of dispersant, 1-2 parts of stabilizer, 20-30 parts of tartaric acid modified oyster shell powder, 10-20 parts of vanillin-hexacyclotetrafluoroethylene composite material, 30-50 parts of epoxy resin and 70-100 parts of water; The preparation method of the tartaric acid modified oyster shell powder comprises the following steps: S1, cleaning the oyster shells, immersing them in an alkaline solution, separating the solid and the liquid, washing, drying and then ball milling to obtain pretreated oyster shell powder; S2, heating the oyster shell powder to 850° C.-950° C. for calcination, and grinding to obtain activated oyster shell powder; S3, dispersing the activated oyster shell powder in an alcohol solution, adding tartaric acid, and performing a hydrothermal reaction at 100° C.-140° C. to obtain tartaric acid-modified oyster shell powder; The preparation method of the vanillin-hexacyclopentadienyl composite material comprises the following steps: Step a, grinding the hexacyclic stone, dispersing it in an amide solvent, adding a surfactant, and performing a coupling reaction at 60° C.-70° C. to obtain activated hexacyclic stone powder; Step b, dispersing the activated hexacyclopaste powder in an alkaline solution, adding vanillin, carrying out a hydrothermal reaction at 90° C.-110° C., solid-liquid separation, washing, and drying to obtain a vanillin-hexacyclopaste composite material.

2. The high-strength and long-lasting mildew-proof mortar material according to claim 1, characterized in that: In S1, the alkaline solution is a 0.05 mol / L-0.1 mol / L sodium hydroxide solution; and / or In S1, the mass volume ratio of the oyster shell to the alkaline solution is 1g:5mL-1g:8mL; and / or In S1, the immersion time is 12h-20h; and / or In S1, the rotation speed of the ball mill is 800 rpm-1200 rpm, and the ball milling time is 30 min-50 min.

3. The high-strength and long-lasting mildew-proof mortar material according to claim 1, characterized in that: In S2, the temperature is increased by programmed temperature increase, and the rate of temperature increase is 15°C / min-25°C / min; and / or In S2, the calcination treatment time is 4h-6h.

4. The high-strength and long-lasting mildew-proof mortar material according to claim 1, characterized in that: In S3, the alcohol solution is a 65%-75% ethanol solution; and / or In S3, the mass volume ratio of the activated oyster shell powder to the alcohol solution is 1g:3mL-1g:5mL; and / or In S3, the mass ratio of the activated oyster shell powder to the tartaric acid is 1:0.5-1:0.8; and / or In S3, the hydrothermal reaction time is 2h-4h.

5. The high-strength and long-lasting mildew-proof mortar material according to claim 1, characterized in that: In step a, the amide solvent is N'N-dimethylformamide; and / or In step a, the surfactant is 3-amino-1,2-propylene glycol; and / or In step a, the mass volume ratio of the hexacyclolith to the amide solvent is 1g:3mL-1g:5mL; and / or In step a, the mass ratio of the hexacyclolith to the surfactant is 1:0.8-1:1.2; and / or In step a, the coupling reaction time is 2h-4h.

6. The high-strength and long-lasting mildew-proof mortar material according to claim 1, characterized in that: In step b, the alkaline solution is a 0.1 mol / L-0.2 mol / L sodium hydroxide solution; and / or In step b, the mass volume ratio of the activated hexacyclic stone powder to the alkaline solution is 1g:2mL-1g:4mL; and / or In step b, the mass ratio of the activated hexacyclopentasiloxane powder to the vanillin is 1:0.4-1:0.7; and / or In step b, the hydrothermal reaction time is 2h-5h.

7. The method for preparing the high-strength and long-lasting mildew-proof mortar material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: weighing various raw material components according to the designed proportion, and uniformly mixing the weighed components to obtain a high-strength and long-lasting mildew-proof mortar material.

8. Use of the high-strength and long-acting mildew-proof mortar material according to any one of claims 1 to 6 or the high-strength and long-acting mildew-proof mortar material prepared by the preparation method of the high-strength and long-acting mildew-proof mortar material according to claim 7 in the field of building materials.

Citation Information

Patent Citations

  • High-strength sealing mortar and preparation method thereof

    CN104193236A

  • Antibacterial and environment-friendly mortar

    CN107365123A

  • Energy-saving environmental-protection mildew-resistant building material and preparation method thereof

    CN108911609A

  • Nano color wall decoration mortar

    CN109650833A

  • Ceramic coating material with effects of environmental protection, self-cleaning property, antibacterial property and scratch resistance, and preparation method thereof

    CN110183878A