A water-resistant starch-based degradable plastic with high elongation at break and preparation method thereof

Through the combination of silanized starch and epoxy soybean oil acrylate, the problems of low water resistance and low elongation of break of starch-based degraded plastics are solved, and the combination of high elongation of break and water resistance is achieved, and environmental protection is adopted. Low-cost water and ethanol solvents, suitable for large-scale production.

CN118638351BActive Publication Date: 2024-11-26DEZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104815.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Existing starch-based degraded plastics are difficult to meet the requirements of high water resistance and high elongation of break at the same time. The commonly used modifiers are highly toxic or expensive, and have poor compatibility with starch, resulting in performance limitations.

Method used

By hydrolyzing the aminosilane and starch in water, then stirring, drying, washing with ethanol aqueous solution, forming silanized starch, and then heating and stirring with epoxy soybean oil acrylate and reinforcement in water, curing reaction is carried out to form high break elongation, forming high break water-resistant starch-based degradation plastic.

Benefits of technology

It significantly improves the water resistance and mechanical properties of starch-based degraded plastics, with an elongation rate of break of more than 160%. It uses environmentally friendly, low-cost water and ethanol as solvents, and does not require toxic solvents or photosensitizers, which are suitable for large-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a high elongation at break water-resistant starch-based degradable plastic and a preparation method thereof, and belongs to the technical field of degradable polymer materials. The preparation method provided by the present invention comprises the following steps: after hydrolyzing aminosilane in water, starch and a strong base are added, the reaction is stirred and dried, and then washed with an ethanol aqueous solution, and the silanized starch is obtained after drying; the silanized starch, epoxy soybean oil acrylate and a reinforcing agent are heated and stirred in water, dried, and then placed at 110-140°C for curing reaction. The preparation method of the present invention is low in cost, green and environmentally friendly, and simple to operate, and is suitable for large-scale preparation. The prepared starch-based degradable plastic has excellent water resistance, and while maintaining a high tensile strength, the elongation at break can reach more than 160%, and has good application performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of degradable polymer materials, and in particular to a high-elongation-at-break water-resistant starch-based degradable plastic and a preparation method thereof. Background Art

[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Plastics are widely used in agriculture, life, medicine and other fields, and are important materials indispensable for economic and social development. Most petroleum-based plastics are difficult to degrade in the natural environment, causing serious pollution to the environment. Bio-based degradable plastics are one of the important ways to solve plastic pollution. Starch-based plastics are one of the lowest-cost and largest-volume degradable plastics in the world. However, starch molecules contain a large number of hydroxyl groups, which leads to poor water resistance and mechanical properties of plastics, limiting their scope of application. The development of water-resistant starch-based degradable plastics with high mechanical properties is a hot issue in the forefront of continuous research.

[0004] Adding reinforcing agents, polymers, and hydrophobic modification of starch are widely used to improve the performance of starch-based degradable plastics. Hydrogen bonds are formed between reinforcing agents or polymers and starch, which are easily destroyed in a high-humidity environment, resulting in poor water resistance of degradable plastics. Starch has a large number of hydroxyl groups and low activity, so starch modification requires the use of highly active modifiers such as acyl chlorides and acetic anhydride, but these modifiers are highly toxic or expensive.

[0005] Vegetable oils are widely available, low-cost, and highly hydrophobic. The double bonds of vegetable oils can be epoxidized and acrylated to form highly active epoxidized soybean oil acrylate (AESO). AESO has been reported to be used for hydrophobic coating of starch to prepare water-resistant starch films, but AESO coating films are easy to fall off and break, and are very brittle. In addition, AESO and starch have different polarities, poor compatibility, low reactivity, and the starch-based plastics obtained by the mixed reaction of the two often have a very low elongation at break, which limits their application. Therefore, how to provide a water-resistant starch-based degradable plastic with high elongation at break is an urgent problem to be solved. Summary of the invention

[0006] In view of this, the present invention provides a high elongation at break water-resistant starch-based degradable plastic and a preparation method thereof, which solves the problem that existing starch-based degradable plastics are difficult to simultaneously meet high water resistance and high elongation at break.

[0007] In a first aspect, the present invention provides a method for preparing a water-resistant starch-based degradable plastic with high elongation at break, comprising the following steps:

[0008] The aminosilane is hydrolyzed in water, starch and a strong base are added, the mixture is stirred for reaction, and then dried, and then washed with an ethanol aqueous solution, and dried to obtain silanized starch;

[0009] The silanized starch, epoxy soybean oil acrylate and reinforcing agent are heated and stirred in water, dried, and then placed at 110-140°C for curing reaction to obtain the product.

[0010] Preferably, the aminosilane is selected from 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane; the hydrolysis temperature is 10-40° C., and the hydrolysis time is 1-3 hours.

[0011] Preferably, the strong base is selected from sodium hydroxide or potassium hydroxide.

[0012] Preferably, after hydrolyzing the aminosilane in water, starch and a strong base are added, and in the drying step after stirring the reaction, the mass ratio of aminosilane, starch, a strong base and water is 1: (1.2~1.8): (0.1~0.15): (1.5~2.5); the stirring reaction temperature is 10~40°C and the time is 1~3h; the drying temperature is 70~90°C and the drying time is 20~30h.

[0013] Preferably, the volume fraction of the ethanol aqueous solution is 50-90%, the washing is performed 1-4 times, and the drying temperature of the silanized starch obtained after drying is 50-80° C., and the drying time is 10-30 hours.

[0014] Preferably, the usage ratio of the silanized starch, epoxy soybean oil acrylate, enhancer and water is (60~70)g: (25~40)g: (1~5)g: (800~1200)mL.

[0015] Preferably, the enhancer is selected from one or more of microcrystalline cellulose, chitosan or polyvinyl alcohol.

[0016] Preferably, in the step of heating and stirring the silanized starch, epoxy soybean oil acrylate and the enhancer in water, the heating and stirring steps are specifically: first heating and stirring at 80-90° C. for 20-40 minutes, and then heating and stirring at 60-80° C. for 1-3 hours.

[0017] Preferably, in the drying step after heating and stirring the silanized starch, epoxy soybean oil acrylate and the enhancer in water, the drying temperature is 60-80° C. and the drying time is 6-10 hours; and the curing reaction time is 1-5 hours.

[0018] In a second aspect, the present invention provides a water-resistant starch-based degradable plastic with high elongation at break prepared by the above-mentioned preparation method.

[0019] Compared with the prior art, the present invention has achieved the following beneficial effects:

[0020] (1) The present invention first synthesizes silanized starch, then uses epoxy soybean oil acrylate (AESO) as a plasticizer for starch-based plastics, and synthesizes a degradable plastic film by a solution casting method. The preparation method can significantly improve the water resistance and mechanical properties of starch-based degradable plastics. The prepared starch-based degradable plastics can maintain a high tensile strength while having an elongation at break of more than 160%, and have good application performance.

[0021] (2) The present invention uses aminosilane and strong alkali to modify starch, directly dries it, and then removes the unreacted aminosilane by alcohol washing. Compared with the previous technical solution of obtaining insoluble silanized modified starch by filtering first and then drying it, the present invention can obtain silanized starch with a high degree of substitution.

[0022] (3) The solvents used in the preparation process of the high elongation at break water-resistant starch-based degradable plastic of the present invention are water and ethanol, without the need to use toxic organic solvents or add other photosensitizers or catalysts. The process is low-cost, green and environmentally friendly, and easy to operate, making it suitable for large-scale preparation. DETAILED DESCRIPTION

[0023] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0024] The present invention provides a method for preparing a water-resistant starch-based degradable plastic with high elongation at break, comprising the following steps:

[0025] The aminosilane is hydrolyzed in water, starch and a strong base are added, the mixture is stirred for reaction, and then dried, and then washed with an ethanol aqueous solution, and dried to obtain silanized starch;

[0026] The silanized starch, epoxy soybean oil acrylate and reinforcing agent are heated and stirred in water, dried, and then placed at 110-140°C for curing reaction to obtain the product.

[0027] The present invention first uses aminosilane to silane-modify starch, so that starch is grafted with amino groups, which is easier to react with epoxy soybean oil acrylate later. During the starch silane modification process, aminosilane hydrolyzes to produce silanol groups, which can form hydrogen bonds with the hydroxyl groups of starch, and form Si-OC after heating, and successfully graft aminosilane onto starch. Starch has a large number of intermolecular and intramolecular hydrogen bonds, which makes it insoluble in cold water. Adding strong alkali can destroy its hydrogen bonds and promote starch dissolution, thereby improving the silane modification efficiency. After the reaction solution is dried, the presence of unreacted aminosilane will reduce the mechanical strength and water resistance of the plastic. The unreacted aminosilane can be removed with an ethanol aqueous solution.

[0028] The present invention heats and stirs silanized starch, plasticizer epoxy soybean oil acrylate (AESO) and a reinforcing agent in water. The heating and stirring process can fully mix the raw materials and gelatinize the starch. At the same time, the silanized starch and AESO undergo Michael addition reaction. Since the solvent for heating and stirring is water, the temperature of the heating and stirring process is below 100°C, and the reaction of the silanized starch and AESO is incomplete. Therefore, the temperature is increased after drying to perform a curing reaction. The double bonds of AESO and the amino groups of the silanized starch produce a strong interaction through the Michael addition reaction to form a compact structure. At the same time, the fatty acid chain of AESO produces a plasticizing effect on the silanized starch. AESO itself is hydrophobic. Therefore, the starch-based degradable plastic finally prepared has high strength, high elongation at break and high water resistance.

[0029] The present invention does not impose any particular restriction on the type and source of starch, and the starch may be selected from, for example, corn starch, potato starch, or tapioca starch.

[0030] In the present invention, the aminosilane is selected from 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane; the hydrolysis temperature is 10-40°C, more preferably 20-30°C, and the hydrolysis time is 1-3h, more preferably 1.5-2.5h. In the present invention, the strong base is selected from sodium hydroxide or potassium hydroxide.

[0031] In the present invention, the aminosilane is hydrolyzed in water, starch and a strong base are added, and in the drying step after stirring the reaction, the mass ratio of aminosilane, starch, a strong base and water is 1: (1.2-1.8): (0.1-0.15): (1.5-2.5); the stirring reaction temperature is 10-40°C, and the time is 1-3h. The present invention uses a high-concentration alkaline solution to dissolve starch to improve the starch silanization modification efficiency, the solution volume used is small, the starch solid content is high, and it is conducive to directly drying the mixed solution through an oven.

[0032] In the present invention, the volume fraction of the ethanol aqueous solution is 50-90%, and the number of washings is 1-4 times. The purpose of washing with the ethanol aqueous solution is to remove unreacted aminosilane. The present invention finds that if aminosilane is directly added to a mixture of starch, AESO, and a reinforcing agent and heated for reaction, the aminosilane reaction is incomplete, and its residue in the plastic will lead to a decrease in water resistance and mechanical properties.

[0033] The drying temperature of the silanized starch obtained after drying according to the present invention is 50-80°C, more preferably 50-70°C, and further preferably 55-65°C; the drying time is 10-30h, and more preferably 15-25h.

[0034] In the present invention, the usage ratio of the silanized starch, epoxy soybean oil acrylate, enhancer and water is (60-70) g: (25-40) g: (1-5) g: (800-1200) mL; more preferably (60-70) g: (25-35) g: (1-3) g: (900-1100) mL.

[0035] In the present invention, the reinforcing agent is selected from one or more of microcrystalline cellulose, chitosan or polyvinyl alcohol, more preferably microcrystalline cellulose. The reinforcing agent has strong mechanical strength, thereby improving the mechanical strength of the plastic. In the present invention, in the step of heating and stirring the silanized starch, epoxy soybean oil acrylate and the reinforcing agent in water, the heating and stirring step is specifically: first heating and stirring at 80-90°C for 20-40 minutes to gelatinize the silanized starch. Heating and stirring at too high a temperature in water may cause starch degradation or pot sticking; then heating and stirring at 60-80°C for 1-3 hours to promote the addition reaction of the silanized starch and AESO.

[0036] In the present invention, in the drying step after heating and stirring the silanized starch, epoxy soybean oil acrylate and the enhancer in water, the drying temperature is 60-80°C and the drying time is 6-10 hours; the curing reaction time is 1-5 hours, more preferably 1-3 hours; the curing reaction temperature is more preferably 110-130°C, and further preferably 115-125°C.

[0037] The present invention also provides a high-elongation-at-break water-resistant starch-based degradable plastic prepared by the above-mentioned preparation method. The high-elongation-at-break water-resistant starch-based degradable plastic prepared by the present invention has a tensile strength of more than 8MPa and an elongation at break of more than 160%, and a water solubility of less than 0.5% in a 24h immersion test, and has excellent water resistance.

[0038] The technical solution of the present invention is further described below in conjunction with specific embodiments. In the following embodiments, the "room temperature" is 25±2°C, the starch used is cassava starch, and the concentration percentage of the ethanol aqueous solution is the volume fraction of ethanol in the ethanol aqueous solution.

[0039] Example 1

[0040] This embodiment provides a method for preparing a water-resistant starch-based degradable plastic with high elongation at break.

[0041] (1) Preparation of silanized starch:

[0042] 11.07 g of 3-aminopropyltriethoxysilane was hydrolyzed in 22.14 g of distilled water at room temperature for 2 h, then 16.20 g of cassava starch and 1.30 g of NaOH were added, and stirring was continued for 2 h. The sample was reacted in an oven at 80 ° C for 24 h. The dried sample was washed and purified twice with 220 mL of 70% ethanol aqueous solution, and then dried at 60 ° C for 24 h to obtain silanized starch.

[0043] (2) Preparation of starch-based degradable plastics:

[0044] 6.50 g of silanized starch, 3.30 g of epoxy soybean oil acrylate and 0.20 g of microcrystalline cellulose were mixed and stirred in 100 mL of distilled water, heated to 85°C and stirred for 30 min, then cooled to 70°C and stirred for 2 h. 60.00 g of the solution was poured into a glass dish, dried in an oven at 60°C for 8 h, and then cured at 120°C for 2 h.

[0045] Example 2

[0046] This embodiment provides a method for preparing a water-resistant starch-based degradable plastic with high elongation at break.

[0047] (1) Preparation of silanized starch:

[0048] 11.07 g of 3-aminopropyltrimethoxysilane was hydrolyzed in 24.35 g of distilled water at room temperature for 2 h, then 18.80 g of starch and 1.50 g of NaOH were added, and stirring was continued for 2 h. The sample was reacted in an oven at 80 ° C for 24 h. The dried sample was washed and purified twice with 220 mL of 70% ethanol aqueous solution, and then dried at 60 ° C for 24 h to obtain silanized starch.

[0049] (2) Preparation of starch-based degradable plastics:

[0050] 6.80g of silanized starch, 2.90g of epoxy soybean oil acrylate and 0.30g of chitosan were mixed in 100mL of distilled water, heated to 80℃ and stirred for 30min, then cooled to 70℃ and stirred for 2h. 60.00g of the solution was poured into a glass dish, dried in an oven at 70℃ for 5h, and then placed in an oven at 130℃ for high temperature curing for 2h.

[0051] Example 3

[0052] This embodiment provides a method for preparing a water-resistant starch-based degradable plastic with high elongation at break.

[0053] (1) Preparation of silanized starch:

[0054] 11.07 g of 3-aminopropyltriethoxysilane was hydrolyzed in 22.14 g of distilled water at room temperature for 2 h, then 13.80 g of starch and 1.20 g of KOH were added, and stirring was continued for 2 h. The sample was reacted in an oven at 80 ° C for 24 h. The dried sample was washed and purified twice with 220 mL of 70% ethanol aqueous solution, and then dried at 60 ° C for 24 h to obtain silanized starch.

[0055] (2) Preparation of starch-based degradable plastics:

[0056] 6.20g of silanized starch, 3.60g of epoxy soybean oil acrylate and 0.20g of polyvinyl alcohol were mixed and stirred in 100mL of distilled water, heated to 90℃ and stirred for 30min, then cooled to 70℃ and stirred for 2h. 60.00g of the solution was poured into a glass dish, dried in an oven at 60℃ for 8h, and then placed in an oven at 120℃ for high temperature curing for 3h.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is that the starch is not subjected to silanization modification in this comparative example.

[0059] 6.50g starch, 3.30g epoxidized soybean oil acrylate and 0.20g microcrystalline cellulose were mixed and stirred in 100mL distilled water, heated to 90℃ and stirred for 30min, then cooled to 70℃ and stirred for 2h. 60.00g of the solution was poured into a glass dish, dried in an oven at 60℃ for 8h, and then placed in an oven at 120℃ for high temperature curing for 2h.

[0060] Comparative Example 2

[0061] The difference between this comparative example and Example 1 is that in this comparative example, the epoxy soybean oil acrylate is replaced by glycerol.

[0062] (1) Preparation of silanized starch:

[0063] 11.07 g of 3-aminopropyltriethoxysilane was hydrolyzed in 22.14 g of distilled water at room temperature for 2 h, then 16.20 g of starch and 1.30 g of NaOH were added, and stirring was continued for 2 h. The sample was reacted in an oven at 80 ° C for 24 h. The dried sample was washed and purified twice with 220 mL of 70% ethanol aqueous solution, and then dried at 60 ° C for 24 h to obtain silanized starch.

[0064] (2) Preparation of starch-based degradable plastics:

[0065] 6.50 g of silanized starch, 3.30 g of glycerol and 0.20 g of microcrystalline cellulose were mixed and stirred in 100 mL of distilled water, heated to 90°C and stirred for 30 min, then cooled to 70°C and stirred for 2 h. 60.00 g of the solution was poured into a glass dish, dried in an oven at 60°C for 8 h, and then placed in an oven at 120°C for high temperature curing for 2 h.

[0066] Comparative Example 3

[0067] Compared with Comparative Example 2, the present comparative example does not perform silanization modification on the starch.

[0068] 6.50g starch, 3.30g glycerol and 0.20g microcrystalline cellulose were mixed and stirred in 100mL distilled water, heated to 90℃ and stirred for 30min, then cooled to 70℃ and stirred for 2h. 60.00g solution was poured into a glass dish, dried in an oven at 60℃ for 8h, and then placed in an oven at 120℃ for high temperature curing for 2h.

[0069] Comparative Example 4

[0070] The difference between this comparative example and Example 1 is that in this comparative example, 3-aminopropyl triethoxysilane, starch, epoxy soybean oil acrylate, and microcrystalline cellulose are added to the reaction at the same time, the mass of starch is controlled to be 6.5 g, and the mass ratio of 3-aminopropyl triethoxysilane to starch is the same as that in Example 1.

[0071] 6.50g starch, 4.45g 3-aminopropyl triethoxysilane, 3.30g epoxy soybean oil acrylate and 0.20g microcrystalline cellulose were mixed and stirred in 100mL distilled water, heated to 90℃ and stirred for 30min, then cooled to 70℃ and stirred for 2h. 60.00g of the solution was poured into a glass dish, dried in an oven at 60℃ for 8h, and then placed in an oven at 120℃ for high temperature curing for 2h.

[0072] Test example

[0073] Water solubility test:

[0074] The starch-based degradable plastic samples of Examples 1 to 3 and Comparative Examples 1 to 4 were dried at 60°C for 24 h. Then, the samples were immersed in 100 mL of distilled water for 24 h. The insoluble particles were filtered, collected, and dried at 60°C for 24 h. The water solubility is the ratio of the mass of the dissolved sample to the dry weight of the initial sample, and the results are shown in Table 1.

[0075] Tensile strength and elongation at break test:

[0076] According to ASTM D882, the tensile strength and elongation at break of rectangular samples were measured using a tensile testing machine (Jinan Languang Electromechanical Technology Co., Ltd.). The results are shown in Table 1.

[0077] Table 1 Performance measurement of starch-based degradable plastic samples of Examples and Comparative Examples

[0078]

[0079] Compared with the comparative example, the starch-based degradable plastic sample of the embodiment has low water solubility and high elongation at break. From the comparison between the comparative example and Example 1, it can be seen that if the starch is not silanized or glycerol is used as a plasticizer, the degradable plastic will have poor water resistance and low elongation at break. In addition, when the starch is silanized, it is necessary to remove the unreacted silane, otherwise the unreacted silane will significantly reduce the water resistance and elongation at break of the degradable plastic.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a water-resistant starch-based degradable plastic with high elongation at break, characterized in that: The steps include: The aminosilane is hydrolyzed in water, starch and a strong base are added, the mixture is stirred for reaction, and then dried, and then washed with an ethanol aqueous solution, and dried to obtain silanized starch; The mass ratio of the aminosilane, starch, strong base and water is 1: (1.2-1.8): (0.1-0.15): (1.5-2.5); The silanized starch, epoxy soybean oil acrylate and reinforcing agent are heated and stirred in water, dried, and then placed at 110-140°C for curing reaction to obtain; The usage ratio of the silanized starch, epoxy soybean oil acrylate, reinforcing agent and water is (60-70) g: (25-40) g: (1-5) g: (800-1200) mL; The reinforcing agent is selected from one or more of microcrystalline cellulose, chitosan or polyvinyl alcohol.

2. The preparation method according to claim 1, characterized in that The aminosilane is selected from 3-aminopropyltriethoxysilane or 3-aminopropyltrimethoxysilane; the strong base is selected from sodium hydroxide or potassium hydroxide; the hydrolysis temperature is 10-40° C., and the hydrolysis time is 1-3 hours.

3. The preparation method according to claim 1, characterized in that: The aminosilane is hydrolyzed in water, starch and strong alkali are added, and in the drying step after stirring the reaction, the stirring reaction temperature is 10-40° C. and the time is 1-3 hours; the drying temperature is 70-90° C. and the drying time is 20-30 hours.

4. The preparation method according to claim 1, characterized in that: The volume fraction of the ethanol aqueous solution is 50-90%, the washing times are 1-4 times; the drying temperature of the silanized starch obtained after drying is 50-80° C., and the drying time is 10-30 hours.

5. The preparation method according to claim 1, characterized in that: In the step of heating and stirring the silanized starch, epoxy soybean oil acrylate and the enhancer in water, the heating and stirring steps are specifically: first heating and stirring at 80-90° C. for 20-40 minutes, and then heating and stirring at 60-80° C. for 1-3 hours.

6. The preparation method according to claim 1, characterized in that: In the drying step after heating and stirring the silanized starch, epoxy soybean oil acrylate and the enhancer in water, the drying temperature is 60-80° C. and the drying time is 6-10 hours; and the curing reaction time is 1-5 hours.

7. A water-resistant starch-based degradable plastic with high elongation at break prepared by the preparation method according to any one of claims 1 to 6.