A high-strength and high-toughness polyoxymethylene composite material and its preparation method and application

By introducing polylactic acid (PLA) and catalyst into the polyformaldehyde (POM)/ethylene glycidyl methacrylate (EGMA) blend system, the poor toughness and thermodynamic incompatibility of POM are solved. The preparation of polyformaldehyde composite materials with high strength and high toughness has been achieved, and the scope of application has been expanded.

CN118638384BActive Publication Date: 2024-11-08HANGZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128949.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-08
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Polyformaldehyde (POM) is prone to spherical crystals during molding, resulting in sensitivity to notches and poor toughness, limiting its application range, and is thermodynamic inconsistent with the blending system of ethylene glycidyl methacrylate copolymer (EGMA). Capacitance, it is difficult to achieve high performance.

Method used

Polylactic acid (PLA) and N,N-dimethyln-octadecamine catalysts were introduced into the POM/EGMA blend system. EGMA and PLA formed an elastomer linked by PLA in situ, increasing viscosity and inhibiting elastomer phase breakage. Reduce interfacial tension, improve interphase adhesion, and realize the preparation of polyformaldehyde composite materials with high strength and high toughness.

Benefits of technology

It significantly improves the impact strength and tensile properties of polyformaldehyde materials, enhances its toughness, reduces interface tension, achieves synergistic improvement of the comprehensive performance of incompatible blends, and expands its fields in automobiles, electrical, electronics, etc. Application possibilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118638384B_ABST
    Figure CN118638384B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polymer materials, specifically discloses a high-strength and high-toughness polyoxymethylene composite material and its preparation method and application, and its method includes the following: ethylene methacrylate glycidyl copolymer, polylactic acid, N, N-dimethyl n-octadecylamine are blended by a mixing device at 170-220 DEG C to obtain a uniform blend, then cooled to room temperature, then added to polyoxymethylene, mixed uniformly at room temperature to obtain a mixture A; or ethylene methacrylate glycidyl copolymer, polylactic acid, N, N-dimethyl n-octadecylamine catalyst are added to polyoxymethylene, mixed uniformly at room temperature to obtain a mixture B; Mixture A or B is added to a mixing device for melt blending to obtain modified polyoxymethylene. The polylactic acid used in the present invention is a typical biodegradable polymer material, green and environmentally friendly and pollution-free; its preparation process only needs to use commonly used melt mixing equipment, and industrial preparation is simple, which is conducive to large-scale industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, and in particular to a high-strength and high-toughness polyoxymethylene composite material and a preparation method and application thereof. Background Art

[0002] Polyoxymethylene (POM) is a widely used engineering plastic. POM has a regular chain structure, no side chains, high density, high tensile strength, high bending modulus, self-lubrication, creep resistance and other characteristics. It is widely used in the automotive, electrical, and electronic fields. However, due to the high crystallinity of POM, it is very easy to form large spherulites during the molding process. These spherulites are easy to form stress concentration points when the material is impacted, resulting in POM's shortcomings such as notch sensitivity and poor toughness, which greatly limits its application range. In response to this performance shortcoming of polyoxymethylene, a large number of studies in the past 20 years have shown that blending modification is the simplest and most effective way to toughen POM.

[0003] Ethylene glycidyl methacrylate copolymer (EGMA) is a linear elastomer with a low glass transition temperature (Tg) and a flexible molecular chain. It is widely used in toughening and modification of engineering plastics such as PPS, PLA, and PA6. However, according to the second law of thermodynamics, the components of the POM / EGMA blend system are thermodynamically incompatible. Simple physical blending will cause macroscopic phase separation of the material, making it difficult to achieve high performance, resulting in limited applications. Further improving the performance of the POM / EGMA blend system and increasing the compatibility of POM with other components remain the core scientific issues in polyoxymethylene blending research. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes to introduce polylactic acid (PLA) and N,N-dimethyl n-octadecylamine (DMSA) catalyst into a polyoxymethylene (POM) / ethylene glycidyl methacrylate copolymer (EGMA) blending system. During the reactive blending process, EGMA and PLA in situ form an elastomer linked by PLA, which significantly improves its viscosity, inhibits the breakage of the elastomer phase during the blending process, and fixes the structure. At the same time, a small amount of free PLA molecular chains are compatible with the POM matrix, thereby effectively reducing the interfacial tension, improving the interphase adhesion, and playing a compatibilizing role, thereby achieving a synergistic improvement in the comprehensive performance of the incompatible blend, and preparing a polyoxymethylene material with high strength and high toughness.

[0005] To achieve the above object, on the one hand, the present invention provides a method for preparing a high-strength and high-toughness polyoxymethylene composite material, which comprises the following steps:

[0006] S1. 5-20 wt% of ethylene methacrylate glycidyl copolymer pellets or powder, 1-30 wt% of polylactic acid pellets or powder, and 0.1-1.0 wt% of N,N-dimethyl n-octadecylamine catalyst are mixed at 170-220° C. by a mixing device to obtain a uniform blend, then cooled to room temperature, and then added to 60-90 wt% of polyoxymethylene pellets or powder, and mixed uniformly at room temperature to obtain a mixture A; or

[0007] 5-20 wt% of ethylene methacrylate glycidyl copolymer pellets or powder, 1-30 wt% of polylactic acid pellets or powder, and 0.01-1.0 wt% of N,N-dimethyl n-octadecylamine catalyst are added to 60-90 wt% of polyoxymethylene pellets or powder, and mixed uniformly in one step at room temperature to obtain a mixture B;

[0008] S2. Adding the mixture A or B into a mixing device for melt blending to obtain a high-strength and high-toughness polyoxymethylene composite material (also known as modified polyoxymethylene).

[0009] As a further preferred technical solution of the present invention, the step of drying the raw materials is also included, specifically:

[0010] The pellets or powders of polyoxymethylene and polylactic acid are vacuum dried at 60-80°C for 24-48 hours, and the pellets or powders of ethylene methacrylate copolymer are vacuum dried at 40-50°C for 24-48 hours.

[0011] As a further preferred technical solution of the present invention, in step S1, the mixing equipment is one of an internal mixer and an extruder, the rotation speed is 20-100 rpm, and the mixing time is 2-20 min.

[0012] As a further preferred technical solution of the present invention, in step S2, the mixing equipment is one of an internal mixer and an extruder. The temperature range of the internal mixer is 170-220 °C, the speed is 20-100 rpm, and the mixing time is 2-20 min. The temperature range of the extruder is 170-220 °C, and the mixing speed is 30-150 rpm.

[0013] As a further preferred technical solution of the present invention, the mass ratio of ethylene methacrylate glycidyl copolymer to polylactic acid is 2:1 to 1:3.

[0014] According to another aspect of the present invention, the present invention further provides a polyoxymethylene composite material, which is prepared by the above method.

[0015] According to another aspect of the present invention, the present invention also provides an application of the above-mentioned polyoxymethylene composite material as engineering plastics, so that the formaldehyde composite material is directly used as a masterbatch in the fields of automobiles, electrical and electronic fields.

[0016] The method for preparing the high-strength and high-toughness polyoxymethylene composite material of the present invention adopts the above technical scheme to achieve the following beneficial effects:

[0017] 1) The polylactic acid used in the present invention is a typical biodegradable polymer material, which is green, environmentally friendly and pollution-free;

[0018] 2) The present invention only requires the use of commonly used melt-mixing equipment, and the industrial preparation is simple, which is conducive to large-scale industrial production;

[0019] 3) The polyvinyl methacrylate glycidyl copolymer used in the present invention undergoes an epoxy ring-opening reaction with polylactic acid. When a small amount of N,N-dimethyl n-octadecylamine catalyst is used, the reactivity of carboxyl, hydroxyl and epoxy groups can be significantly increased, thereby greatly improving product performance;

[0020] 4) The present invention can obtain modified polyoxymethylene with adjustable mechanical properties by changing the mass ratio and addition amount of ethylene methacrylate copolymer / polylactic acid during melt blending, which provides new possibilities for expanding the application of polyoxymethylene in various fields. In addition, the composite material prepared by the present invention can also be used as a high-performance polymer alloy material. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0022] Figure 1 1 and 2 are SEM images of Comparative Example 1 and Example 1, wherein a and b represent the internal microstructure of each sample, respectively, and 1 and 2 represent SEM magnifications of 4 K and 10 K, respectively.

[0023] Figure 2 TEM images of Comparative Example 1 and Example 1, wherein a and b represent the internal microscopic morphology of each sample, respectively, and 1 and 2 represent TEM magnifications of 1.5 K and 6 K, respectively.

[0024] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0026] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0027] The number average molecular weight of the polyoxymethylene (POM) used in the following examples is in the range of 5000-200000; the number average molecular weight of the polylactic acid (PLA) is in the range of 5000-150000; the manufacturer of ethylene glycidyl methacrylate copolymer (EGMA) is: Arkema, France, brand: AX8900; the catalyst (DMSA) is N,N-dimethyl n-octadecylamine, molecular formula: C 18 H 36 (CH 3 ) 2 N.

[0028] Comparative Example 1: Preparation of a polyoxymethylene composite material POM / EGMA, wherein the mass ratio of the POM / EGMA raw materials is 70:10.

[0029] Step S1. The POM pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0030] Step S2. adding the EGMA pellets to the POM pellets, and mixing them evenly at room temperature to obtain a mixture;

[0031] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0032] Comparative Example 2: Preparation of a polyoxymethylene composite material POM / EGMA-PLA, wherein the mass ratio of the POM / EGMA / PLA raw materials is 70:10:20.

[0033] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0034] Step S2. EGMA pellets and PLA pellets are first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0035] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0036] Example 1: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of the POM / EGMA / PLA / DMSA raw materials is 70:10:20:0.3.

[0037] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0038] Step S2. adding EGMA pellets, PLA pellets, and DMSA catalyst to POM pellets, and mixing them uniformly at room temperature to obtain a mixture;

[0039] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0040] like Figure 1 As shown, Example 1 and Comparative Example 1 were subjected to SEM analysis, and we can see that the addition of PLA and DMSA catalysts has a significant effect on the micromorphology of the POM / EGMA blend. The interfacial tension is reduced, and the morphology is transformed from an island structure to an inhomogeneously dispersed elastomer-enriched structure. We believe that under the action of the DMSA catalyst, EGMA and PLA form an elastomer linked by PLA in situ, which significantly increases its viscosity, inhibits the breakage of the elastomer phase during the blending process, and fixes the structure; at the same time, a small amount of free PLA molecular chains are compatible with the POM matrix. This special structure of inhomogeneously dispersed EGMA enrichment in the SEM image of Example 1 is more conducive to the internal transmission of external stress, and thus helps to improve the toughness of the material.

[0041] like Figure 2 As shown, by performing TEM analysis on Example 1 and Comparative Example 1, we can more clearly see the non-uniformly dispersed elastomer-enriched structure of the sample of Example 1, which is consistent with Figure 1 The SEM image of Example 1 has a good correspondence.

[0042] Example 2: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of POM / EGMA / PLA / DMSA is 80:10:10:0.3.

[0043] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0044] Step S2. EGMA pellets, PLA pellets, and DMSA catalyst were first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0045] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0046] Example 3: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of POM / EGMA / PLA / DMSA is 75:10:15:0.3.

[0047] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0048] Step S2. EGMA pellets, PLA pellets, and DMSA catalyst were first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0049] Step S3. adding the mixture into an internal mixer, and melt-blending at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM;

[0050] Example 4: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of POM / EGMA / PLA / DMSA is 70:10:20:0.3.

[0051] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0052] Step S2. EGMA pellets, PLA pellets, and DMSA catalyst were first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0053] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0054] Example 5: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of POM / EGMA / PLA / DMSA is 65:10:25:0.3.

[0055] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0056] Step S2. EGMA pellets, PLA pellets, and DMSA catalyst were first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0057] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0058] Example 6: Preparation of a polyoxymethylene composite material POM / EGMA-PLA / DMSA, wherein the mass ratio of POM / EGMA / PLA / DMSA is 70:15:20:0.3.

[0059] Step S1. The POM and PLA pellets were vacuum dried at 80 °C for 24 h, and the EGMA pellets were vacuum dried at 50 °C for 24 h;

[0060] Step S2. EGMA pellets, PLA pellets, and DMSA catalyst were first blended at 190° C. and 50 rpm for 10 min to obtain a uniform blend, then cooled to room temperature, and then added to POM pellets, and mixed uniformly at room temperature to obtain a mixture;

[0061] Step S3. The mixture was added into an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain a modified POM.

[0062] Performance test: The modified polyoxymethylene samples prepared in the above comparative examples and embodiments were subjected to notch impact and tensile tests to characterize the mechanical properties of the samples.

[0063] For the impact test, a microinjection molding machine was used to prepare an impact specimen with a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. The depth of the V-notch was 2 mm, and then placed at room temperature for 12 to 24 hours. According to the GB / T 16420-1997 standard, an impact test machine was used to perform an impact test on the specimen, and the pendulum energy used was 2 J.

[0064] For the tensile test, dumbbell-shaped tensile specimens with a length of 20 mm, a width of 4 mm, and a thickness of 2 mm were prepared by microinjection molding and left to stand at room temperature for 12 to 24 h. The specimens were tensile tested by a universal material testing machine at a tensile rate of 10 mm / min.

[0065] Table 1 is a summary of the specific data of the mechanical properties of the above examples and comparative examples:

[0066]

[0067] The present invention is further analyzed below in conjunction with Table 1 and specific embodiments.

[0068] The impact performance of Examples 1 and 4 was analyzed with Comparative Example 1. We can see that the impact strength of Comparative Example 1 is only about 16.6 kJ / m 2 In Examples 1 and 4, the impact strength is significantly improved due to the introduction of PLA and DMSA catalysts. In Example 4, EGMA, PLA, and DMSA catalyst are pre-blended by a two-step method, and the resulting blend is melt-blended with POM. Compared with Example 1, the impact strength of the modified polyoxymethylene can be further improved, thereby obtaining an ultra-tough POM-based composite material.

[0069] The impact properties of Example 4 and Comparative Example 2 were analyzed. We can see that the introduction of a small amount of DMSA catalyst into the sample of Example 4 can significantly improve its impact strength.

[0070] The impact properties of Examples 2 to 5 were analyzed. We can see that the impact strength of the material increases significantly with the increase of PLA content (the decrease of POM content). This is because in this range, with the increase of PLA content, most of the PLA links EGMA, and a small part of the free PLA chains promote the formation of graft copolymer EGMA-g-PLA, which is compatible with the matrix POM, effectively reducing the interfacial tension and improving the interphase adhesion.

[0071] The impact properties of Examples 4 and 6 were compared and analyzed with Comparative Example 1. It can be seen that the impact strength of the material is significantly improved with the increase of EGMA content.

[0072] The tensile properties of Examples 1 and 4 were analyzed with Comparative Example 1. It can be seen that both Examples 1 and 4 have higher Young's modulus and elongation at break, and Example 4 pre-blended EGMA, PLA, and DMSA catalyst by a two-step method, and then melt-blended the obtained blend with POM, which can further improve the Young's modulus and elongation at break of our modified polyoxymethylene. This is mainly due to the introduction of PLA and DMSA catalysts, which effectively improves the compatibility between the elastomer EGMA and the POM / PLA base.

[0073] The tensile properties of Example 4 and Comparative Example 2 were analyzed. We can see that the introduction of a small amount of DMSA catalyst into the sample of Example 4 can improve its Young's modulus and elongation at break.

[0074] The tensile properties of Examples 2 to 5 were analyzed. We can see that the Young's modulus and elongation at break of the material also increase with the increase of PLA content (the decrease of POM content).

[0075] The tensile properties of Examples 4 and 6 and Comparative Example 1 were analyzed. We can see that the elongation at break of the material increases with the increase of EGMA content, but its Young's modulus decreases.

[0076] In summary, when the mass ratio of POM / EGMA / PLA in the polyoxymethylene composite material is 65:10:25, adding a small amount (0.1~1.0 wt%) of N,N-dimethyl n-octadecylamine catalyst, its comprehensive performance reaches the best. At this time, the viscosity of the EGMA elastomer linked by PLA increases, which inhibits the breakage of the elastomer phase during the blending process and fixes the structure; at the same time, the free PLA just plays a compatibilizing role. The synergistic improvement of the comprehensive performance of the incompatible blend components is achieved, and a polyoxymethylene composite material with complementary multi-component advantages and performance is developed. In addition, by changing the addition amount of polyoxymethylene, ethylene methacrylate copolymer and polylactic acid, the mechanical properties of the modified polyoxymethylene composite material can be effectively regulated.

[0077] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a high-strength and high-toughness polyoxymethylene composite material, characterized in that: The following steps are involved: S1. According to the mass ratio of ethylene methacrylate glycidyl copolymer to polylactic acid of 2:1-1:3, 5-20 wt% of ethylene methacrylate glycidyl copolymer pellets or powder, 1-30 wt% of polylactic acid pellets or powder, and 0.1-1.0 wt% of N,N-dimethyl n-octadecylamine catalyst are blended at 170-220° C. through a mixing device to obtain a uniform blend, which is then cooled to room temperature and then added to 60-90 wt% of polyoxymethylene pellets or powder, and mixed uniformly at room temperature to obtain a mixture A; or According to the mass ratio of ethylene methacrylate glycidyl copolymer to polylactic acid being 2:1-1:3, 5-20 wt% of ethylene methacrylate glycidyl copolymer pellets or powder, 1-30 wt% of polylactic acid pellets or powder, and 0.01-1.0 wt% of N,N-dimethyl n-octadecylamine catalyst are added to 60-90 wt% of polyoxymethylene pellets or powder, and mixed uniformly in one step at room temperature to obtain a mixture B; S2. Adding the mixed material A or B into a mixing device for melt blending to obtain modified polyoxymethylene.

2. The method for preparing the high-strength and high-toughness polyoxymethylene composite material according to claim 1, characterized in that: The process also includes a step of drying the raw materials, specifically: Before step S1, the pellets or powders of polyoxymethylene and polylactic acid are vacuum dried at 60-80°C for 24-48 h, and the pellets or powders of ethylene methacrylate copolymer are vacuum dried at 40-50°C for 24-48 h.

3. The method for preparing the high-strength and high-toughness polyoxymethylene composite material according to claim 1, characterized in that: In step S1, the mixing equipment is one of an internal mixer and an extruder, the rotation speed is 20-100 rpm, and the mixing time is 2-20 min.

4. The method for preparing the high-strength and high-toughness polyoxymethylene composite material according to claim 1, characterized in that: In step S2, the mixing equipment is one of an internal mixer and an extruder.

5. The method for preparing the high-strength and high-toughness polyoxymethylene composite material according to claim 4, characterized in that: The temperature range of the internal mixer blending is 170~220 ℃, the speed is 20~100 rpm, and the blending time is 2~20 min.

6. The method for preparing the high-strength and high-toughness polyoxymethylene composite material according to claim 4, characterized in that: The temperature range of the extruder blending is 170-220 °C, and the blending speed is 30-150 rpm.

7. A polyoxymethylene composite material, characterized in that: The method is prepared by any one of claims 1 to 6.

8. Use of the polyoxymethylene composite material according to claim 7 as engineering plastics.