A kind of 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability and preparation method thereof

By optimizing chemical composition and process flow, high surface quality and forming properties of 800MPa hot-dip galvanized composite steel is prepared, which solves the problems of insufficient elongation and surface quality of hot-dip galvanized composite steel in the prior art, and achieves high steel plate Strength, good moldability and low cost production meet the complex parts forming needs of the automobile industry.

CN118639134BActive Publication Date: 2024-12-03ANGANG STEEL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411118570.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The elongation and surface quality of existing hot-dip galvanized composite steel cannot meet the demand for complex parts forming, and lack effective processes for surface quality control, which cannot meet the rapid development requirements of the automotive industry.

Method used

By optimizing the chemical composition design and process flow, a high surface quality and forming 800MPa grade hot-dip galvanized composite steel is prepared, with chemical compositions of C: 0.08% to 0.1%, Si: 0.1% to 0.3%, Mn: 1.8% ~2.1%, Cr: 0.1%~0.4%, Mo: 0.1%~0.4%, P: ≤0.01%, S: ≤0.005%, Ti: 0.02%~0.03%, Nb: 0.02%~0.03%, B: 0.0001%~0.0004%, the structure and surface roughness of the steel plate are controlled by smelting, hot rolling, pickling, cold rolling, continuous degalvanizing and polishing processes.

Benefits of technology

The high tensile strength, yield strength, elongation and pore expansion rate of the steel plate are achieved, the moldability and surface quality of the steel plate are improved, the production cost is reduced, and the high surface quality and high formability requirements of the automobile industry are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639134B_ABST
    Figure CN118639134B_ABST
Patent Text Reader

Abstract

The invention relates to a 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability. The chemical components of the steel are, by mass percentage, C: 0.08%-0.1%, Si: 0.1%-0.3%, Mn: 1.8%-2.1%, Cr: 0.1%-0.4%, Mo: 0.1%-0.4%, P≤0.01%, S≤0.005%, Ti: 0.02%-0.03%, Nb: 0.02%-0.03%, and B: 0.0001%-0.0004%. The preparation method comprises smelting, continuous casting, hot rolling, pickling, cold rolling, continuous galvanizing and skin-finishing processes. The advantages are: industrial mass production can be completed without adding other equipment, welding difficulty is reduced, and there is good process stability; the steel plate produced by the invention adopts the idea of ​​two-phase zone heating combined with slow cooling, controls the content of critical zone ferrite and oriented epitaxial ferrite, improves the yield strength of the steel plate, effectively reduces the hardness difference between the soft and hard phases in the steel, improves the forming performance of the steel plate, and adopts pre-oxidation and reduction process design to achieve high surface quality of the steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of automobile steel manufacturing, and in particular to a 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability and a preparation method thereof. Background Art

[0002] As car companies accelerate the pace of electrification and lightweighting, it is foreseeable that fuel vehicles will be discontinued worldwide. In the manufacturing process of electric vehicles, the status of steel as the main material for automobile bodies is difficult to shake in a short time, especially advanced high-strength steel has gradually become the key research and development direction of automobile steel. Among advanced high-strength steels, dual-phase steel is used in the body in a high proportion. Due to its low flanging performance, dual-phase steel cracks when complex parts are formed, reducing the yield of steel. As a representative of advanced high-strength steel, complex phase steel has a structure of ferrite, bainite, martensite, or contains residual austenite. Because complex phase steel has good flanging performance and strength and plasticity matching, it is suitable for roll forming and is favored by automobile manufacturers, with good market prospects. At present, the elongation of hot-dip galvanized complex phase steel is about 11%. In the face of the rapid development of the automobile industry, it is obviously unable to meet the automobile manufacturers' requirements for complex parts forming, and has strict requirements on the surface of hot-dip galvanized steel sheets. Therefore, improving the formability and surface quality of complex phase steel is an urgent problem to be solved.

[0003] In the prior art, the authorization announcement number is CN113528942B, and the patent name is "A hot-dip galvanized complex phase steel and its production method". Its chemical composition is C: 0.12%~0.17%, Si: 0.2~0.6%, Mn: 1.8%~2.4%, Cr: 0.2%~0.7%, P: ≤0.001%, S: ≤0.006%, and the rest is Fe and unavoidable impurities. The product yield strength is ≥570MPa, the tensile strength is ≥780MPa, the elongation is ≥12%, and the hole expansion rate is greater than 45%; the product hole expansion rate is low, which cannot meet the requirements for complex parts forming, and does not involve surface quality control technology.

[0004] The publication number is CN 114959478A, and the patent name is "A 800MPa-grade complex phase steel with multiple uses and its control method". Its chemical composition is: C: 0.12~0.15%, Si: 0.6~0.8%, Mn: 1.85%~2.15%, Alt: 0.7~0.9%, Cr: 0.2~0.3%, Mo: 0.15~0.3%, B: 0.0015~0.0003%, P: ≤0.005%, S: ≤0.005%, N: ≤0.005%, O: ≤0.005%. In this product, the elongation of hot-dip galvanized 800MPa-grade complex phase steel is greater than 21.5%, and the hole expansion rate is 50%; the product has a low hole expansion rate and cannot meet the requirements for complex parts forming. Excessive carbon content reduces the welding performance of the steel, and the surface quality control process is not involved. Summary of the invention

[0005] The purpose of the present invention is to provide a 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability and a preparation method thereof, which can achieve high surface quality and high formability of steel plates based on the actual production line of existing steel mills without significantly increasing the alloy cost.

[0006] To achieve the above object, the present invention is implemented through the following technical solutions:

[0007] A 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability, wherein the chemical composition of the steel is C: 0.08%-0.1%, Si: 0.1%-0.3%, Mn: 1.8%-2.1%, Cr: 0.1%-0.4%, Mo: 0.1%-0.4%, P: ≤0.01%, S: ≤0.005%, Ti: 0.02%-0.03%, Nb: 0.02%-0.03%, B: 0.0001%-0.0004%, and the balance is Fe and unavoidable impurities; the tensile strength of the finished steel plate is above 800MPa, the yield strength is 640-700MPa, the elongation is ≥15%, and the hole expansion rate is ≥75%. , achieving good strength, plasticity and formability of the steel plate; the finished steel plate structure includes ferrite, bainite, martensite and carbide precipitation; according to the plane area method, the ferrite content is 15% to 30%, ferrite content = critical zone ferrite content + oriented epitaxial ferrite content, among which the critical zone ferrite is 8% to 17%, and the rest is oriented epitaxial ferrite, bainite content is 45% to 65%, and martensite content is 15% to 35%; the ferrite contains 1×10 7 Pieces / mm 2 The hardness ratio of bainite to martensite is greater than 0.6, the hardness ratio of ferrite to bainite is greater than 0.5, and the surface roughness of the steel plate is between 0.8 and 1.7 µm.

[0008] The reasons for adopting the above-mentioned components are as follows:

[0009] C: Carbon is an economical strengthening element in steel. As a solid solution atom in steel, it produces lattice distortion on the solid solution matrix and plays a role in solid solution strengthening. Carbon, as a stable austenitizing element, causes supercooled austenite to partially transform into bainite during isothermal transformation, and retains part of the supercooled austenite to transform into martensite during the subsequent cooling process, thereby ensuring the high strength of the steel. However, excessive addition of carbon will increase the difficulty of welding, and the supercooled austenite is too stable, making it difficult to obtain the desired structure in subsequent processes. Therefore, the C element content in the present invention is controlled at 0.08% to 0.1%.

[0010] Si: Silicon can dissolve in ferrite, increase the strength of ferrite, and significantly increase the yield strength of steel. The addition of silicon in the present invention is to inhibit the precipitation of cementite in the over-aging stage. Too high Si content will reduce the surface quality of the steel plate. Therefore, the Si content in the present invention is controlled at 0.1% to 0.3%.

[0011] Mn: Manganese can be infinitely dissolved in austenite, strengthening the austenite effect. It can expand the austenite phase area, reduce the critical quenching rate of experimental steel, and stabilize austenite. However, excessive manganese content will cause organizational segregation and deteriorate the comprehensive performance of steel.

[0012] Cr: Chromium can improve the hardenability of steel and serve as a supplement to Mn. Appropriate addition of Cr stabilizes austenite. At the same time, the addition of Cr can improve the oxidation resistance of the steel plate to a certain extent and improve the internal oxidation of the steel plate. In the present invention, the Cr content is controlled at 0.1% to 0.4%.

[0013] Mo: Mo is a solid solution strengthening element that strengthens the steel plate. Mo can delay the formation of pearlite in the cooling stage of supercooled austenite, promote the formation of bainite, and ensure the bainite content in the steel. The Mo content of the present invention is controlled to be 0.1% to 0.4%.

[0014] P: Phosphorus is a harmful element in steel, and the lower its content, the better. Considering the cost, the phosphorus content is controlled within P≤0.01% in the present invention.

[0015] S: Sulfur is a harmful element in steel, and the lower its content, the better. Considering the cost, the sulfur content is controlled within S≤0.005% in the present invention.

[0016] Ti: Titanium can fix free N atoms in steel and play a role in fixing N. At the same time, TiN can precipitate during the solidification process and play a role in pinning grain boundaries; Ti(C,N) precipitates during the hot rolling stage and refines the original austenite grains. At the same time, a small amount of Ti precipitates during the continuous annealing process to strengthen ferrite and bainite, but too much Ti carbide precipitation will occupy C in the steel and reduce the stability of supercooled austenite. The Ti content of the present invention is controlled at 0.02% to 0.03%.

[0017] Nb: In the present invention, Nb is appropriately added to induce strain precipitation during the hot rolling recrystallization rolling stage, promote austenite recrystallization, and refine the grains. The Nb content in the present invention is 0.02% to 0.03%.

[0018] B: A trace amount of boron can improve the hardenability of steel and save other relatively precious metals, but too high a boron content will increase the brittleness of the steel plate and reduce the comprehensive mechanical properties of the steel plate; the B content in the present invention is 0.0001% to 0.0004%.

[0019] The preparation method of 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability includes smelting, continuous casting, hot rolling, pickling, cold rolling, continuous annealing and skin-passing. The specific process is as follows:

[0020] 1) Smelting: Smelting is carried out through a converter to obtain an alloy composition within the above range.

[0021] 2) Hot rolling: The billet heating temperature is 1220-1250°C, the starting rolling temperature is 1080-1150°C, the final rolling temperature is 890-920°C, the coiling temperature is between 600-650°C, and the thickness of the hot rolled plate is 3.0-3.2mm.

[0022] The heating temperature is between 1220~1250℃ to ensure the homogenization of alloy elements, the precipitation of Ti (C, N), the pinning of the original austenite grain boundaries, and the refinement of the original austenite grains. The starting rolling temperature is between 1080~1150℃, and the final rolling temperature is above 890℃. Ensure rolling in the recrystallization zone, control the austenite recrystallization behavior, and refine the grains. The final rolling temperature is above 890℃ to prevent the rolling mill from overloading. The coiling temperature is between 600~650℃ to obtain ideal organizational properties. When the coiling temperature is too low, the bainite content in the organization increases, increasing the difficulty of cold rolling; when the coiling temperature is too high, it leads to coil collapse and increases the formation of oxides, such as MnO2, SiO2, and Fe2O3.

[0023] 3) Pickling: The purpose is to remove the iron oxide scale generated on the surface of the hot-rolled plate and improve the surface quality of the cold-rolled plate. The acid temperature is 75-90°C and the pickling speed is 60-180m / min.

[0024] 4) Cold rolling: The overall reduction rate of cold rolling is 50%~60%. Ensuring a reduction rate of more than 50% promotes tissue fiberization and ensures that the strip accumulates a certain amount of deformation energy storage. When the cold rolling reduction rate is too high, the deformation resistance is too large, making it difficult to roll to the target thickness, increasing the mill load, and reducing the life of the roll.

[0025] 5) Continuous galvanizing:

[0026] The cold hard coil obtained by cold rolling is preheated first, and the temperature is raised to 620~680℃ at 8~10℃ / s, and the dew point is 0~20℃, and the pre-oxidation process is carried out. Then it is heated to 760~830℃ at 5~10℃ / s for uniform heating, and the uniform heating time is 100~160s, and the dew point is -50~-30℃, and the reduction process is carried out. Slowly cool to 700~750℃ at 1~5℃ / s; then cool to 300~360℃ at a cooling rate greater than 30℃ / s for overaging, and the heat preservation time is 320~500s; then heat to 450~470℃ at a heating rate of 10℃ / s, which is the adjustment stage before galvanizing, and the adjustment time is 9~17s. The steel sheet then enters the zinc pot, the zinc pot temperature is 455-470℃, the galvanizing time is 1-3s, and then it is cooled to room temperature at a cooling rate greater than 5℃ / s; the weight percentage of Al in the plating solution is: 0.18%-0.23%, and the rest is Zn and unavoidable impurities. The weight of the zinc layer per unit area of ​​the galvanized steel sheet is 90-105g / cm 2 .

[0027] The strip is first preheated to 660℃ with a dew point between 0 and 20℃. The purpose is to have a certain weak oxidizing property of the protective atmosphere. At this time, Fe, Mn and Cr elements on the surface of the steel plate undergo oxidation reaction; then it is heated to 760~830℃ at 5~10℃ / s for even heating, with an even heating time of 100~160s and a dew point of -10~0℃; if the heating rate is lower than 5℃ / s, it cannot meet the production line requirements and will reduce production efficiency; if the heating rate is higher than 10℃ / s, uneven oxidation of easily oxidized elements Mn and Cr will reduce the quality of the coating; the heating temperature is set to 760~830℃, which is the heating temperature in the two-phase region, retaining part of the two-phase region ferrite; the even heating time is 100~160s. Too long an even heating time will result in coarse grains, and too short an even heating time will result in insufficient recrystallization of ferrite, which will reduce the plasticity of the steel plate. At this stage, when the steel strip temperature drops to -50℃~-30℃, the surface Fe oxide will be reduced to sponge iron, and the Mn and Cr oxides will cover the sponge iron, forming the so-called "internal oxidation". The surface sponge Fe has good wettability with the zinc liquid, so that the steel plate has good surface quality. Slowly cool to 690~750℃ at 1~5℃ / ; through the reasonable setting of the slow cooling temperature, the oriented epitaxial ferrite content is controlled to be 7%~18%. The epitaxial ferrite is difficult to diffuse into the austenite in a short time during the slow cooling process due to the difficulty of Mn and other substitution atoms to diffuse into the austenite in the epitaxial ferrite. Reduce the hardness difference between ferrite and bainite and martensite in the organization, improve the coordinated deformation ability of the organization, and thus improve the hole expansion performance of the steel plate. After slow cooling, cool to 300~360℃ at a cooling rate greater than 30℃ / s for over-aging, and the holding time is 320~500s. At this stage, 45%~65% bainite is guaranteed to be formed. The slow cooling rate is greater than 30℃ / s to inhibit the formation of pearlite. Then the temperature is raised to 450~470℃ isothermally at a heating rate of 10℃ / s. This is the adjustment stage before galvanizing: the adjustment time is 9~17s; the purpose is to prevent zinc condensation due to too low temperature, and leakage due to too high temperature, which reduces the surface quality of the steel plate. This process promotes C-rich austenite, and all the supercooled austenite is transformed into martensite during the subsequent cooling process. The martensite content is 15%~35%, which ensures the strength of the steel plate.

[0028] Skin finishing: The steel plate enters the skin finishing machine for plate shape adjustment, and the skin finishing elongation is ≥0.4%. The main purpose is to ensure that the steel plate has a good plate shape. The surface roughness of the steel plate is 0.8-1.7μm. Too large surface roughness makes the steel plate prone to defects such as pits and pits; too small surface roughness affects the subsequent coating process.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The steel plate produced by the present invention is developed based on the existing production line, and industrial mass production can be completed without the addition of other equipment, with low production cost, and the steel plate has a lower carbon equivalent, which reduces the difficulty of welding and has good process stability;

[0031] 2. The steel plate produced by the present invention adopts the idea of ​​two-phase heating combined with slow cooling to control the content of ferrite and oriented epitaxial ferrite in the critical zone, improve the yield strength of the steel plate, effectively reduce the hardness difference between the soft and hard phases in the steel, improve the forming performance of the steel plate, adopt pre-oxidation and reduction process design, give the steel plate a reasonable surface roughness, and achieve high surface quality of the steel plate;

[0032] 3. The steel plate produced by the present invention adopts optimized alloy design and process design to achieve the goals of high surface quality and good formability. The product covers a thickness of 0.8~2.0mm, meeting the automotive industry's requirements for high surface quality and high formability. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a diagram of the organizational structure of an embodiment.

[0034] Figure 2 It is the precipitation diagram of the finished steel plate.

[0035] Figure 3 is the energy spectrum of the precipitate. DETAILED DESCRIPTION

[0036] The present invention is described in detail below in conjunction with the accompanying drawings, but it should be noted that the implementation of the present invention is not limited to the following embodiments.

[0037] The following examples are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples. The methods used in the following examples are conventional methods unless otherwise specified.

[0038] [Example]

[0039] The chemical composition of the steel in Examples 1-6 is shown in Table 1, and the hot rolling process parameters of the steel in Examples 1-6 are shown in Table 2.

[0040] The annealing process parameters of the steel in Examples 1-6 are shown in Table 3, the mechanical properties of the steel in Examples 1-6 are shown in Table 4, and the microstructure of the finished steel plate in Example 1 is shown in Table 5. Figure 1 As shown, the precipitate photo of the finished steel plate of Example 1 is shown in Figure 2 , the precipitate energy spectrum is shown in Figure 3 .

[0041] Table 1 Chemical composition of the example steel (wt%)

[0042] Example C Si Mn Cr Mo P S Ti Nb B 1 0.085 0.15 2.05 0.32 0.24 0.008 0.003 0.029 0.026 0.0003 2 0.092 0.22 1.87 0.19 0.22 0.007 0.002 0.024 0.027 0.0003 3 0.087 0.17 1.92 0.34 0.31 0.009 0.002 0.030 0.029 0.0004 4 0.010 0.23 2.00 0.27 0.18 0.005 0.001 0.020 0.021 0.0002 5 0.089 0.21 1.89 0.33 0.29 0.008 0.002 0.023 0.025 0.0004 6 0.096 0.28 1.94 0.25 0.25 0.007 0.003 0.026 0.022 0.0002

[0043] Table 2 Hot rolling process parameters of example steel

[0044] Example Heating temperature / ℃ Rolling temperature / ℃ Final rolling temperature / ℃ Curling temperature / ℃ Hot rolled plate thickness / mm 1 1224 1089 892 617 3.08 2 1236 1105 901 642 3.17 3 1242 1131 913 633 3.11 4 1250 1138 917 650 3.09 5 1234 1100 899 621 3.14 6 1228 1095 904 609 3.20

[0045] Table 3 Annealing process parameters of example steel

[0046] Example Heating temperature / ℃ Dew point / ℃ Ambient temperature / ℃ Soaking time / s Dew point / ℃ Slow cooling temperature / ℃ Cooling rate / ℃ / s Over-aging temperature / ℃ Insulation time / s Galvanizing temperature / ℃ Finishing elongation / % Surface roughness / μm 1 660 12 790 132 -30 743 32 355 387 460 0.4 1.2 2 660 17 781 154 -45 738 37 324 496 459 0.7 0.8 3 660 15 794 111 -41 722 35 338 446 457 0.6 1.4 4 660 11 822 123 -33 746 43 344 340 460 0.8 1.5 5 660 13 813 102 -36 735 41 332 322 460 0.5 1.0 6 660 14 801 142 -38 709 38 319 355 462 0.7 1.7

[0047] Table 4 Mechanical properties of example steel

[0048] Example Yield strength / MPa Tensile strength / MPa <![CDATA[Elongation (A 50 ) / %]]> Hole expansion rate λ / % Intercritical Ferrite Epitaxial ferrite bainite Martensite Bainite hardness / Martensite hardness Ferrite Hardness / Bainite Hardness The number of precipitates below 30nm in ferrite 1 640 811 15.2 75.0 14 10 55 21 0.7 0.53 <![CDATA[1.3*10 7 ]]> 2 647 805 15.4 75.3 17 12 51 20 0.66 0.58 <![CDATA[1.2*10 7 ]]> 3 661 816 15.1 76.1 15 14 60 11 0.72 0.54 <![CDATA[1.5*10 7 ]]> 4 682 801 15.5 76.3 8 9 65 18 0.65 0.51 <![CDATA[1.6*10 7 ]]> 5 654 812 15.2 75.5 11 13 53 23 0.67 0.57 <![CDATA[1.4*10 7 ]]> 6 677 819 15.1 75.2 12 17 49 22 0.69 0.56 <![CDATA[1.7*10 7 ]]>

[0049] It can be seen from the above embodiments that, based on the traditional production line, by selecting appropriate chemical elements and content ratios, and coordinating with ingenious processes, the tensile strength of the finished steel plate is made to be above 800MPa, the yield strength is 640~700MPa, the elongation is ≥15%, and the hole expansion rate is ≥75%, thereby achieving good strength, plasticity, formability and surface quality of the steel plate.

Claims

1. A 800MPa grade hot-dip galvanized composite steel with high surface quality and formability, characterized in that: The chemical composition of the steel is calculated by mass percentage as follows: C: 0.08% ~ 0.1%, Si: 0.1% ~ 0.3%, Mn: 1.8% ~ 2.1%, Cr: 0.1% ~ 0.4%, Mo: 0.1% ~ 0.4%, P: ≤ 0.01%, S: ≤ 0.005%, Ti: 0.02% ~ 0.03%, Nb: 0.02% ~ 0.03%, B: 0.0001% ~ 0.0004%, the balance is Fe and unavoidable impurities; The preparation method of 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability includes smelting, continuous casting, hot rolling, pickling, cold rolling, continuous annealing and skin-passing. The specific process is as follows: 1) Smelting; 2) Hot rolling: the billet heating temperature is 1220-1250℃, the starting rolling temperature is 1080-1150℃, the final rolling temperature is 890-920℃, and the coiling temperature is between 600-650℃; 3) Pickling: the acid temperature is 75-90°C, and the pickling speed is 60-180m / min; 4) Cold rolling: The cold rolling reduction rate is 50% to 60%; 5) Continuous galvanizing: ① Raise the temperature to 620~680℃ at 8~10℃ / s, with a dew point of 0~20℃, and carry out the pre-oxidation process; ② Then heat to 760-830℃ at 5-10℃ / s for equalization, the equalization time is 100-160s, the dew point is -50--30℃, and the reduction process is carried out; ③ Slowly cool to 700-750℃ at 1-5℃ / s; then cool to 300-360℃ at a cooling rate greater than 30℃ / s for overaging, with a holding time of 320-500s; then heat to 450-470℃ at a heating rate of 10℃ / s as an isothermal adjustment stage before galvanizing, with an adjustment time of 9-17s; ④ The steel plate enters the zinc pot, the zinc pot temperature is 455-470℃, the galvanizing time is 1-3s, and then it is cooled to room temperature at a cooling rate greater than 5℃ / s; the weight percentage content of Al in the plating solution is: 0.18%-0.23%, and the rest is Zn and unavoidable impurities. The surface quality grade of the steel plate is FC grade; ⑤ Skin finishing: The steel plate enters the skin finishing machine for plate shape adjustment, and the skin finishing elongation is ≥0.4%.

2. The 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability according to claim 1, characterized in that: The tensile strength of the finished steel plate is above 800MPa, the yield strength is 640~700MPa, the elongation is ≥15%, and the hole expansion rate is ≥75%.

3. The 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability according to claim 1, characterized in that: The microstructure of the finished steel plate includes ferrite, bainite, martensite and carbide precipitation; according to the plane area method, the ferrite content is 15% to 30%, of which the critical zone ferrite is 8% to 17%, and the rest is oriented epitaxial ferrite; the bainite content is 45% to 65%, and the martensite content is 15% to 35%.

4. The 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability according to claim 3, characterized in that: The ferrite contains 1×10 7 Pieces / mm 2 The precipitates are larger than 30 nm in size.

5. The 800MPa grade hot-dip galvanized complex phase steel with high surface quality and formability according to claim 3, characterized in that: The ratio of the hardness of bainite to the hardness of martensite is greater than 0.60, the ratio of the hardness of ferrite to the hardness of bainite is greater than 0.50, and the surface roughness of the steel plate is between 0.8 and 1.7 µm.

Citation Information

Patent Citations

  • A hot-dip galvanized multiphase steel and its production method

    CN113528942B

  • 800 MPa-grade complex-phase steel with one steel for multiple purposes and regulation and control method of 800 MPa-grade complex-phase steel

    CN114959478A

  • Cold-rolled hot galvanizing dual-phase steel and preparation method thereof

    CN109023106A