A tin spraying solution, its preparation method and its application in spraying process
By using nitrogen-containing five-membered heterocyclic compounds and poly compounds as stabilizers and levelers in tin spraying solution, combined with specific spraying process conditions, the problems of uniformity and density of tin plating layer in electroplating process are solved. , realizes efficient and stable tin coating deposition, and improves the quality and process efficiency of semiconductor devices.
Patent Information
- Application Number
- CN202411087347.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing electroplating process is difficult to achieve rapid deposition of high uniformity and dense tin plating on semiconductor devices and wafer chip materials, especially on plating parts with complex shapes, and it is difficult to maintain consistency of the fluid flow field, resulting in plating. Evenness and circuit spacing issues.
Using nitrogen-containing five-membered heterocyclic compounds and specific poly compounds as stabilizers and levelers, the stability and deposition performance of the tin plating solution are improved by forming stable and huge molecules in the tin spraying solution, and combined with specific spraying Plating process conditions, such as current density and temperature control, achieve efficient tin plating deposition.
It realizes the density of the tin plating, no pinholes and joints, and has a smooth surface, which improves the stability and reliability of electronic products of semiconductor devices, meets the demand for high-end precision tin materials in the high-tech field, and simplifies the electroplating process and shortens the The electroplating time broadens the selection range of process conditions.
Smart Images

Figure CN118639282B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrolytic or electrophoretic production process and electroforming of coatings, and particularly relates to a tin spraying solution, a preparation method thereof and an application thereof in a spraying process. Background Art
[0002] Electroplating is a special processing technology that forms nano- or micron-scale metal-plated devices in an electrolytic cell based on the principle of electrochemical cathode deposition. Electroplating can be used to manufacture precision-structured semiconductor devices or wafer chip materials. In order to make semiconductor devices and wafer chip materials have reliable and excellent electronic communication performance, it is necessary to develop high-speed electrolytic processing technology for plated parts of various complex shapes, and the tin plating layer formed needs to have high thickness, high uniformity and excellent density.
[0003] When using electroplating to manufacture precision nano- or micron-level semiconductor devices and wafer chip materials, as the thickness of the coating on the circuit surface increases, the cross-sectional area of the chip material circuit will gradually decrease. This is because metal cations have the characteristic of preferential discharge deposition at the edge of the plated circuit; as the thickness of the coating on the circuit surface increases, the distance between adjacent circuits decreases and tends to close short circuits; at the same time, the uniformity of the coating on the circuit surface decreases, resulting in a decrease in the precision of the wafer chip circuit, and even failing to meet product specification requirements.
[0004] Existing electroplating processes show that by adding appropriate leveling agents to the electroplating solution, during the electrolysis process of semiconductor devices and wafer chip materials, the metal ions are preferentially discharged in the concave parts of the circuit surface to suppress the decrease in the uniformity of the coating, so as to achieve the thickening of the surface coating of the semiconductor devices and wafer chip material circuits while suppressing the trend of reducing the circuit spacing. However, the regulatory effect of this type of electroplating leveling agent on the deposition behavior of metal cations is greatly affected by the fluid flow field, flow rate, flow direction, etc. of the electroplating solution. Specifically, the existing tin plating process usually immerses semiconductor devices and wafer chip materials in a circulating electroplating solution. It is extremely difficult for the electroplating solution to form a rapid flow exchange-electrolysis precipitation effect on the surface of the semiconductor devices and wafer chip material circuits, and it is difficult to ensure that the fluid flow field state at various locations on the surface of the semiconductor devices and wafer chip material circuits remains consistent, resulting in the difficulty in achieving uniform deposition rates at various locations on the surface of the semiconductor devices and wafer chip material circuits.
[0005] For the electroplating process of high-end precision electronic materials such as semiconductor devices and wafer chips with complex shapes, it is an important technical indicator for the production and manufacturing of high-end electroplating processes to deposit tin coatings quickly and obtain tin coatings with high uniformity and density. However, the existing electroplating tin solutions and electroplating processes are difficult to achieve the electroplating effect of the above technical indicators; the main reason is that it is difficult to simultaneously achieve the effect of high-speed and uniform flow to flush the plated surface of semiconductor devices and wafer chip materials without interfering with the electric field distribution. Summary of the invention
[0006] [Technical issues]
[0007] Provided is a tin spraying solution for semiconductor devices, which can be suitable for the electroplating process of semiconductor devices and has the advantages of rapid deposition of tin plating layers, obtaining tin plating layers with high uniformity and density, and the obtained tin-plated semiconductor device products are of high quality.
[0008] [Technical solution]
[0009] In one aspect, a tinning solution is provided, comprising components in the following concentrations:
[0010]
[0011] Wherein, the stabilizer includes at least one of the following:
[0012] Polyacrylic acid, sodium polyacrylate, ammonium polyacrylate, hydroxypropyl acrylate polymer with an average molecular weight of less than 2000, acrylic acid-maleic acid copolymer with a molecular weight of 800-1200, polymaleic acid or polyethylene glycol with a molecular weight of 200-400 and their derivatives;
[0013] The leveler includes nitrogen-containing five-membered heterocyclic compounds.
[0014] In some embodiments, polyethylene glycol and its derivatives include at least one of heptapolyethylene glycol, octapolyethylene glycol, decapolyethylene glycol, aminopolyethylene glycol hydroxyl with a molecular weight of 300-500, M-tetrapolyethylene glycol-sulfonic acid, polyethylene glycol diacrylate with a molecular weight of 800-1200, polyethylene glycol dicarboxylic acid with a molecular weight of 500-700, mercaptotetrapolyethylene glycol, polyethylene glycol dicarboxylic acid with a molecular weight of 800-1200, amino-heptapolyethylene glycol-carboxylic acid, and amino-nonapolyethylene glycol-carboxylic acid.
[0015] Preferably, the stabilizer includes: polyacrylic acid with an average molecular weight of less than 2000, sodium polyacrylate, ammonium polyacrylate, hydroxypropyl acrylate polymer, acrylic acid maleic acid copolymer with a molecular weight of 1000, polymaleic acid with a molecular weight of 300, heptapolyethylene glycol, octapolyethylene glycol, decapolyethylene glycol, aminopolyethylene glycol hydroxyl with a molecular weight of 400, M-tetrapolyethylene glycol-sulfonic acid, polyethylene glycol diacrylate with a molecular weight of 1000, polyethylene glycol dicarboxylic acid with a molecular weight of 600, mercaptotetrapolyethylene glycol, polyethylene glycol dicarboxylic acid with a molecular weight of 1000, amino-heptapolyethylene glycol-carboxylic acid, amino-nonapolyethylene glycol-carboxylic acid, at least one of the group.
[0016] In some embodiments, the leveler includes at least one of azoles, imidazoles, oxazoles, or thiazoles.
[0017] In some embodiments, the pyrroles include at least one of 2-acetylpyrrole, 4-pyrrolidin-1-pyridine-2-carboxylic acid hydrochloride, pyrrole-3-carboxylic acid, 2-nitro-1H-pyrrole, 2-methylpyrrole-3-carboxylic acid ethyl ester, 3-nitropyrrole, 1-ethylpyrrolidin-3-ol, 1-(2-hydroxyethyl)pyrrole, or 4-(pyrrolidin-3-yl)pyridine hydrochloride.
[0018] In some embodiments, the imidazoles include at least one of 4-nitroimidazole, 2-nitroimidazole, imidazolidinyl urea, imidazole-5-acetic acid, 2,4-dinitroimidazole, 2-(1-imidazolyl)acetic acid, 5-methyl-4-nitroimidazole, imidazole-4-amine dihydrochloride or L-histidine.
[0019] In some embodiments, the oxazoles include at least one of oxazole-5-acetic acid, 2-amino-1,3-oxazole-4-carboxylic acid, 5-(1-methyl-2-pyrrolyl)isoxazole-3-carboxylic acid, 3-methyl-4-nitroisoxazole-5-carboxylic acid methyl ester, or 5-(propan-2-yl)-1,3-oxazole-4-carboxylic acid.
[0020] In some embodiments, the thiazoles include at least one of thiazole-5-carboxylic acid, thiazole-2-sulfonic acid, 4-nitroisothiazole, thiazole-2(3H)-thione, D-4-thiazolealanine, 2-bromo-5-nitrothiazole, 1-(thiazol-2-yl)ethanol, 2-amino-5-nitrothiazole, and (Z)-2-(2-aminothiazol-4-yl)-2-((2-methoxy-2-oxoethoxy)imino)acetic acid.
[0021] In some embodiments, the wetting agent includes at least one of octylphenol polyoxyethylene ether with a polymerization degree of 7<≤20, sodium salt of diisooctyl sulfosuccinate, or 1,2-propylene glycol polyoxypropylene polyoxyethylene.
[0022] In some embodiments, the tin salt includes at least one of tin sulfate, 2-hydroxyethyl-1-tin sulfonate, tin methane sulfonate, tin nitrate, tin ethyl sulfonate, tin propyl sulfonate, tin hydroxymethane sulfonate, or 2-hydroxybutyl-1-tin sulfonate.
[0023] In some embodiments, the organic acid comprises at least one of sulfuric acid, methanesulfonic acid, ethylsulfonic acid, propylsulfonic acid, 2-hydroxyethyl-1-sulfonic acid, hydroxymethanesulfonic acid, or 2-hydroxybutyl-1-sulfonic acid.
[0024] On the other hand, a method for preparing the aforementioned tin plating solution is provided, comprising the following steps:
[0025] (1) Add a certain amount of deionized water to a container, heat it, and under stirring conditions, add tin salts, organic acids, wetting agents, stabilizers and leveling agents in small amounts and multiple times according to the required volume of the tin-plating solution and the final concentrations of the components in the aforementioned tin-plating solution, and continue to add deionized water to 70-90% of the required volume of the tin-plating solution to obtain solution A; titrate and analyze the total acid content with a standard sodium hydroxide solution to control the total acid content in solution A to be 230-250 mL / L;
[0026] (2) Deionized water is added to solution A until the required volume of the tin-plating solution is reached to obtain solution G, that is, a tin-plating solution is obtained.
[0027] In another aspect, a use of the aforementioned tin plating solution in a spray plating process is provided.
[0028] In another aspect, a method for preparing a tin coating by spraying on the surface of a semiconductor device is provided, wherein the tin plating solution is used as the tin spraying solution; the method comprises the following steps:
[0029] S1. Degreasing and acid activation treatment of the semiconductor device to be processed;
[0030] S2, according to the electroplating area and the form of the plated part, select the corresponding tin spraying conditions, configure the corresponding anode mask, install the anode mask and the semiconductor device to be processed in the electroplating device; the current density of the tin spraying solution during electroplating is 11 to 50 A / dm 2 , the temperature of the tin spraying solution is 40-50°C;
[0031] S3, selecting a corresponding electrolytic power source according to the plated part to perform electroplating;
[0032] S4, regularly testing the tin concentration and total acid content in the tin spraying solution, judging whether the change value of the tin concentration and the total acid content exceeds the limit value, and automatically adding the corresponding components;
[0033] S5, completing the spray electroplating process on the plated parts.
[0034] In some embodiments, the electrolysis power supply includes one of a forward and reverse pulse power supply or a single pulse power supply.
[0035] [Beneficial Effects]
[0036] (1) The present invention adopts specific polymer compounds (polyacrylic acid with an average molecular weight of less than 2000, sodium polyacrylate, ammonium polyacrylate, hydroxypropyl acrylate polymer, acrylic acid-maleic acid copolymer with a molecular weight of 800-1200, polymaleic acid or polyethylene glycol and its derivatives with a molecular weight of 200-400) as a stabilizer and nitrogen-containing five-membered heterocyclic compounds as a leveling agent; the interaction between the nitrogen-containing five-membered heterocyclic compounds and the specific polymer compounds is utilized to improve the stability of the tin plating solution during the spraying operation. Among them, utilizing the interaction between nitrogen-containing five-membered heterocyclic compounds and specific polymer compounds specifically refers to that in the strong acidic system of the tin-plating solution of the present invention, the nitrogen atoms of the nitrogen-containing five-membered heterocyclic compounds easily form a core of positive charge distribution, and attract each other with the oxygen negative charge distribution core in the specific polymer compound to form a more stable and large molecule; the tin-plating solution exhibits excellent stability during high-speed electroplating, and the tin plating layer deposited in the plating area of the semiconductor device is dense, pinhole-free, crack-free, and has a smooth surface. It can effectively prevent defects such as unstable signal transmission, high resistance, and excessive power loss caused by defects such as pinholes or cracks, further improve the stability and reliability of semiconductor device electronic products, and better meet the demand for the development trend of high-end precision tin materials in the field of high-tech, high-quality, and high-precision electronic electroplating products.
[0037] (2) The present invention has found through a large number of experimental studies that, based on the specific stabilizer and specific leveler of the present invention, the tin-plating solution with a stabilizer concentration of 0.5-1.7 mmol / L, a leveler concentration of 0.6-1.8 mmol / L, a tin salt concentration of 900-2100 mmol / L, and an organic acid concentration of 1300-1900 mmol / L, combined with the spraying process of the present invention, can simply and efficiently manufacture high-end precision semiconductor electronic devices with high uniformity, excellent compactness, and strong corrosion resistance in various harsh environments. The tin-plated high-end precision semiconductor electronic devices are of high quality and can be widely used in the fields of electroplating of high-end electronic products such as wafer chip manufacturing, three-dimensional integration and device packaging, sensors, micro-nano device manufacturing, micro-electromechanical systems, components, etc. The present invention has also found that too high or too low a stabilizer dosage in the tin spraying solution of the present invention may lead to a decrease in tin plating performance.
[0038] (3) The present invention also found that, based on the preferred embodiment 17, after only replacing the leveler with non-nitrogen-containing five-membered heterocyclic 2,5-dimethylfuran, or replacing the stabilizer with non-carboxylic acid polymer S10 polyoxyethylene stearate, not only the required electroplating time increased, but also the tin plating performance decreased significantly. It is confirmed that the combined action of nitrogen-containing five-membered heterocyclic compounds and polymer compounds is one of the key technical features for solving the technical problems of the present invention.
[0039] (4) The tin spraying solution and high-speed spraying process of the present invention can not only shorten the electroplating time, but also have a wider range of electroplating conditions, are easy to operate, and are more conducive to practical application, overcoming the technical difficulties of spraying electroplating high-end precision electronic plated parts to produce high-quality tin-plated products. The electroplating method of the present invention can simply and efficiently electroplate and manufacture high-end precision electronic devices with complex shapes that have high film thickness, high uniformity, and excellent compactness. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A schematic flow chart of the steps of the electroplating method of the tin spraying solution according to an embodiment of the present invention;
[0041] Figure 2 A semiconductor device structure to be processed;
[0042] Figure 3 The semiconductor device structure to be processed.
[0043] 10-semiconductor device; 11-electroplating area. DETAILED DESCRIPTION
[0044] Test method:
[0045] Tin coating thickness test: Tested using FISCHERSCOPE X-RAY XDV-SDD detector manufactured by Fischer Figure 3The coordinates of the tin plating film thickness at the central black dot ● of each electroplating area 11 of the semiconductor device plated parts I to VII are: 4 (3.24 mm, 15.62 mm), 8 (3.24, 12), 12 (3.24, 8.32), 16 (3.24, 4.64) in column I; 3 (5.55, 16.54), 7 (5.55, 12.86), 13 (5.55, 7.43), 17 (5.55, 3.80) in column II; 2 (7.86 mm, 17.46 mm), 6 (7.86, 18.38), 10 (7.86, 10.16), 14 (7.86, 6.52), 18 (7.86, 2.89) in column III; 1 (10.16 mm, 18.35 mm), 1 mm), 5 (10.16, 14.71), 9 (10.16, 11.07), 11 (10.16, 9.25), 15 (10.16, 5.61), 19 (10.16, 1.97); 4 in column V (12.47 mm, 15.62 mm), 8 (12.47, 12), 12 (12.47, 8.36), 16 (12.47, 4.72); 3 in column VI (14.78 mm, 16.54 mm), 7 (14.78, 12.90), 13 (12.47, 7.44), 17 (12.47, 3.80); 6 in column VII (14.78 mm, 18.38 mm), 10 (17.09, 10.16), 14 (17.09, 6.52). Analyze the maximum value (Max), minimum value (Min), average value (Ave), and maximum-minimum value (Max-Min) of the tin plating film thickness data.
[0046] The calculation formula of tin film thickness error is:
[0047] .
[0048] Appearance inspection of tin-plated semiconductor device products: Appearance inspection, using 40x optical microscope and 5000x electron microscope for observation, the results are judged according to the following standards;
[0049] Excellent: The tin plating layer should be uniform, smooth, without bubbles, pits, scratches, missing plating, penetration and other defects, which is evaluated as excellent.
[0050] Good: The tin plating layer is uniform, smooth, free of bubbles, pits, scratches, missing plating, and penetration plating. The defect area is less than 3% of the overall test area, which is evaluated as good.
[0051] Medium: The tin plating layer is uniform, smooth, free of bubbles, pits, scratches, missing plating, and penetration plating. The defect area is greater than 3% of the overall test area, and the defect area is less than 5% of the overall test area. It is evaluated as medium.
[0052] Unqualified: The uniformity, smoothness, no bubbles, no pits, no scratches, no missing plating, no seepage plating, etc. of the tin plating layer, the defect area is greater than 5% of the overall test area, and it is evaluated as unqualified.
[0053] Solderability test of tin-plated semiconductor device products: The test was conducted according to the national standard GB / T2423.28-2005 soldering test method, and the soldering performance was judged according to the following standards. Five data were tested for each example sample, and the average defect area of the soldering test was calculated. Among them, the defect area is expressed as a percentage relative to the total test area; the larger the defect area percentage, the larger the defect area of the soldering test, indicating that the soldering performance of the tin coating is worse; conversely, the smaller the defect area percentage, the better the soldering performance of the tin coating.
[0054] Tinning: The solder forms a uniform, smooth, and completely adhered tin layer on the metal surface; that is, the area of defects such as non-tinning is zero, and the area of tinning is 100%, which is evaluated as excellent.
[0055] Tin shrinkage: When tinning, the molten solder covers the entire surface to be tested. After the sample product leaves the tin melting furnace, an irregular tin layer is formed on the surface to be tested, and the base metal is not exposed. If the area of defects such as non-sticking is less than 5% of the overall test area, it is evaluated as good.
[0056] Pinhole: After the sample product leaves the tin melting furnace, there are small hole-like defects penetrating the tin layer on the tested surface; if the area of defects such as non-sticking tin is greater than 5% of the overall test area, it is evaluated as unqualified.
[0057] Non-stick tin: After the sample product leaves the tin melting furnace, there is no change on the tested surface and no tin layer is formed; it is evaluated as completely unqualified.
[0058] Tin-plated semiconductor device product tin plating surface roughness test: The surface roughness was tested according to the national standard GB3505-83 using the 3D profile measuring instrument VR-6000 manufactured by Keyence.
[0059] like Figure 1 As shown, the electroplating method based on the tin spraying solution of the present invention comprises the following steps:
[0060] S1. Perform alkali degreasing and acid activation treatment on the semiconductor device to be processed;
[0061] S2. Select corresponding tin spraying conditions according to the electroplating area and the form of the plated part, configure the corresponding anode mask, and install the anode mask and the semiconductor device (plated part) to be processed in the electroplating device;
[0062] S3, selecting a corresponding electrolytic power source according to the plated part to perform electroplating;
[0063] S4, regularly testing the tin concentration and total acid content in the tin spraying solution, judging whether the change value of the tin concentration and the total acid content of the solution exceeds the limit value, and automatically adding the corresponding components;
[0064] S5, completing the spray electroplating process on the plated parts.
[0065] Example 1
[0066] 1. A tin spraying solution comprising the following components in concentration:
[0067]
[0068] 2. The preparation method of the above-mentioned tin spraying solution comprises the following steps:
[0069] (1) Add a certain amount of deionized water to a container and heat it to 50 °C. Under the condition of circulating pump operation and stirring, add tin methanesulfonate, methanesulfonic acid, wetting agent, stabilizer and leveling agent in small amounts and multiple times according to the required volume of tin plating solution and the above-mentioned final concentration ratio. Continue to add deionized water to 80% of the required volume of tin plating solution to obtain solution A; accurately measure 2.0 mL of solution A, and titrate and analyze the total acid content with sodium hydroxide standard solution to control the total acid content in solution A to 240 mL / L;
[0070] (2) Add a certain amount of deionized water to solution A until the required volume of the tin spraying solution is reached to obtain solution G, that is, a finished tin spraying solution is obtained.
[0071] 3. The use of the above tin spraying solution in preparing a tin coating by spraying on the surface of a semiconductor device comprises the following steps:
[0072] (1) The structure of the semiconductor device 10 to be processed is as follows Figure 2 As shown. A copper disc with a diameter of 8 inches (20.32 mm) and a thickness of 0.35 mm is used as the raw material; a dry film is applied to one side of the disc and the other side is protected with a 3M electroplating tape; the following operations are performed on the side where the dry film is applied: 1) mask exposure, 2) development, 3) film stripping, 4) neutralization, 5) cleaning, and 6) drying to obtain a single-sided experimental sheet with 58 electroplating areas 11. The dry film is still protected outside the electroplating area. During electroplating, only the 58 electroplating areas 11 are in contact with the electroplating solution, and the area of each plating area is 6×13=78 mm 2 , the total surface area of the plating area of the semiconductor device 10 is 58×78 mm 2 =4524 mm 2 The bottom nickel is plated in the electroplating area of the semiconductor device 10 with a thickness ranging from 780 to 830 nm, thereby obtaining the semiconductor device 10 to be processed.
[0073] (2) The semiconductor device 10 to be processed is installed in a spraying mold (commercially available), and the above-mentioned tin spraying solution is used for electroplating. A forward and reverse pulse electroplating power source is used to perform spraying under the electroplating conditions shown in Table 1 to obtain a tin-plated semiconductor device product.
[0074] Table 1 Electroplating conditions
[0075]
[0076] The tin plating film thickness results of Example 1 are shown in Table 2.
[0077] Table 2 Tin plating film thickness results of Example 1 (nm)
[0078]
[0079] As can be seen from Table 2, the tin plating solution of Example 1 is applied to a plating mold for high-speed and high-current density plating processing, and the thickness of the tin plating layer on the surface of the obtained semiconductor device ranges from 3019 to 3223 nm; the difference between the maximum film thickness and the minimum film thickness of Max-Min is 204 nm; the error of its maximum value compared with the target setting value of 3000 nm is (3223-3000) / 3000=7.43%, indicating that the tin plating solution of Example 1 achieves good uniformity of film thickness distribution.
[0080] Example 2 to Example 11 Optimization of the dosage ratio of stabilizer, leveler and tin salt
[0081] 1. A tin spraying solution, referring to Example 1, except that the concentrations of the stabilizer and the leveler are adjusted according to Table 3.
[0082] Table 3 Amounts of stabilizers and levelers used in the tin spraying solutions of Examples 1 to 11 (mmol / L)
[0083]
[0084] 2. The preparation method of the above tin spraying solution is as described in Example 1.
[0085] 3. The application of the above tin spraying solution in preparing a tin coating by spraying on the surface of a semiconductor device is described in Example 1.
[0086] Test Example 1:
[0087] The tin-plated semiconductor device products obtained in Examples 1 to 11 were subjected to appearance inspection, and the results are shown in Table 4.
[0088] Table 4 Appearance inspection results of the tin-plated semiconductor device products obtained from Examples 1 to 11
[0089]
[0090] The tin-plated semiconductor device products obtained in Examples 1 to 11 were tested for tin plating film thickness, and the results are shown in Table 5.
[0091] Table 5 Tin plating film thickness results of tin-plated semiconductor device products obtained from Examples 1 to 11 (nm)
[0092]
[0093] The soldering performance test was performed on the tin-plated semiconductor device products obtained in Examples 1 to 11. The results are shown in Table 6.
[0094] Table 6 Results of solder test defect area inspection of tin-plated semiconductor device products obtained in Examples 1 to 11 (%)
[0095]
[0096] Any flaws in the appearance of the tin plating of semiconductor devices or poor uniformity in film thickness will lead to a decrease in the soldering performance of the tin plating, or even the occurrence of no tin sticking on the soldering surface, and ultimately lead to the scrapping of the semiconductor device electroplating products.
[0097] As can be seen from Table 4, the tin spraying solutions of Examples 3 to 9 are rated as excellent according to the appearance inspection under an electron microscope at 5000 times magnification.
[0098] As can be seen from Table 5, there is no significant difference in the test results of the tin plating film thickness of Examples 1 to 11; the film thickness range is Min3016~Max3233 nm, the difference Max-Min is 212 nm, and the error between the maximum value Max and the film thickness standard value 3000 nm is (3233-3000) / 3000 = 0.0776 = 7.76%; that is, the film thickness error value is only 7.76%, which confirms that the film thickness distribution of the tin plating layer of Examples 1 to 11 has excellent uniformity.
[0099] As can be seen from Table 6, the average defect area of the solder test of Examples 3 to 9 is 0.0%, which confirms that the soldering performance of the corresponding tin plating layer is in the optimal range.
[0100] In summary, the tin spraying solutions of Examples 3 to 9 are applied to the spraying mold for high-speed and high-current density spraying processing, and the semiconductor devices obtained simultaneously achieve excellent appearance, excellent uniformity of tin plating film thickness distribution and excellent soldering performance (the average value of the defect area of the soldering test is 0.0%). Therefore, the amount of stabilizer in the tin spraying solution of the present invention is preferably 0.5-1.7 mmol / L, and the amount of leveler is preferably in the range of 0.6-1.8 mmol / L. When the amount of stabilizer is less than 0.5 mmol / L and the amount of leveler is less than 0.6 mmol / L, the appearance color or surface smoothness of the tin plating obtained under the same conditions is evaluated to be good and medium, and the soldering surface has pinholes and tin shrinkage to varying degrees; when the amount of stabilizer is higher than 1.7 mmol / L and the amount of leveler is higher than 1.8 mmol / L, the precipitated tin particles are rough, and the density of the tin plating is poor, resulting in tin shrinkage and irregular soldering surface.
[0101] In Examples 1 to 11, the amount of tin used is 1200 mmol / L. Combined with the aforementioned preferred range of the total amount of stabilizers and levelers being 1.1 to 3.5 mmol / L, the preferred range of the molar ratio of (total amount of stabilizers and levelers) to the amount of tin used is determined to be (0.91 to 2.91): 1000. Based on the result that the preferred range of the molar ratio of (total amount of stabilizers and levelers) to the amount of tin used is (0.91 to 2.91): 1000, the tin salt use range of 500 to 2500 mmol / L is divided into 11 equal parts, and the total amount of stabilizers and levelers in the molar ratio (0.91 to 2.91): 1000 is also divided into 11 equal parts, and Examples 12 to 22 are designed.
[0102] Embodiment 12 to Embodiment 22
[0103] 1.1 The tin spraying solution of Example 12 comprises components with the following concentrations:
[0104]
[0105] Among them, in Example 12, the amount of tin salt is 500 mmol / L, and the molar ratio of (the total amount of stabilizer and leveler) to the amount of tin metal is 0.91:1000. Therefore: (the total amount of stabilizer and leveler) can be calculated as follows;
[0106] (Total amount of stabilizer and leveler): Tin salt amount = molar ratio: 1000
[0107] Total amount of stabilizer and leveler = molar ratio × tin salt amount ÷ 1000
[0108] =0.91×500÷1000
[0109] =0.455 mmol / L
[0110] Total amount of stabilizer and leveler = stabilizer amount + leveler amount
[0111] It can be seen from Table 3 that the amount of leveling agent is 0.1 mmol / L more than that of stabilizer. Therefore, the amount of stabilizer and leveling agent can be calculated respectively according to the following formula.
[0112] Total amount of stabilizer and leveler = stabilizer amount + (stabilizer amount + 0.1 mmol / L)
[0113] Stabilizer dosage = (total dosage of stabilizer and leveler - 0.1mmol / L) / 2
[0114] = (0.455-0.1) / 2
[0115] =0.18 mmol / L
[0116] Leveling agent dosage = total dosage of stabilizer and leveling agent - stabilizer dosage
[0117] =0.455-0.1775
[0118] =0.28 mmol / L
[0119] That is, the amount of stabilizer used in Example 12 is 0.18 mmol / L, and the amount of leveler used is 0.28 mmol / L. In the same way, the amount of stabilizer and the amount of leveler used in Examples 13 to 22 are calculated, and the results are shown in Table 7. It should be noted that the raw material components of Examples 13 to 22 are the same as those of Example 12.
[0120] Table 7 Stabilizer dosage and leveler dosage in Examples 13 to 22 mmol / L
[0121]
[0122] 1.2 The tin spraying solution of Example 13 comprises components with the following concentrations:
[0123]
[0124] 1.3 The tin spraying solution of Example 14 comprises components with the following concentrations:
[0125]
[0126] 1.4 The tin spraying solution of Example 15 comprises components with the following concentrations:
[0127]
[0128] 1.5 The tin spraying solution of Example 16 comprises components with the following concentrations:
[0129]
[0130] 1.6 The tin spraying solution of Example 17 comprises components with the following concentrations:
[0131]
[0132] 1.7 The tin spraying solution of Example 18 comprises components with the following concentrations:
[0133]
[0134] 1.8 The tin spraying solution of Example 19 comprises components with the following concentrations:
[0135]
[0136] 1.9 The tin spraying solution of Example 20 comprises components with the following concentrations:
[0137]
[0138] 1.91 The tin spraying solution of Example 21 comprises components in the following concentrations:
[0139]
[0140] 1.92 The tin spraying solution of Example 22 comprises components in the following concentrations:
[0141]
[0142] 2. The preparation methods of the tin spraying solutions in Examples 12 to 22 refer to those in Example 1.
[0143] 3. The use of the tin spraying solution in Example 12 to Example 22 for preparing a tin plating layer by spraying on the surface of a semiconductor device is similar to Example 1, except that Examples 12 to Example 22 are implemented according to the electroplating conditions in Table 8.
[0144] Table 8 Electroplating conditions of Examples 12 to 22
[0145]
[0146] Test Example 2:
[0147] The tin-plated semiconductor device products obtained in Examples 12 to 22 were subjected to appearance inspection, tin plating film thickness inspection, and soldering performance test, respectively. The results are shown in Tables 9 to 11.
[0148] Table 9 Appearance test results of Examples 12 to 22
[0149]
[0150] Table 10 Tin plating film thickness results of Example 12 to Example 22 (nm)
[0151]
[0152] Table 11 Results of solder test defect area inspection for Examples 12 to 22 (%)
[0153]
[0154] It can be seen from Table 10 that there is no significant difference in the test results of the tin plating film thickness of Examples 12 to 22; the film thickness range is Min3018~Max3236 nm, the difference Max-Min is 216 nm, and the error between the maximum value Max and the film thickness standard value 3000 nm is (3236-3000) / 3000 = 0.0786 = 7.86%; that is, the film thickness error value is only 7.86%, which confirms that the film thickness distribution of the tin plating layer of Examples 12 to 22 has excellent uniformity.
[0155] Combining Tables 9 to 11, it can be seen that the tin spraying solutions of Examples 14 to 20 are applied to the spraying mold for high-speed and high-current density spraying processing, and the obtained semiconductor devices simultaneously achieve excellent appearance, excellent uniformity of tin plating film thickness distribution and excellent soldering performance (the average value of the defect area in the soldering test is 0.0%). Therefore, the preferred range of the amount of tin salt in the tin spraying solution of the present invention is 900 to 2100 mmol / L, and the preferred range of the amount of organic acid is 1300 to 1900 mmol / L.
[0156] Comparative Example 1
[0157] 1. Tin plating solution and its preparation method refer to the non-patent literature [Modern Electroplating Handbook] Volume 1 Chapter 7 Tin plating solution, which includes the following concentrations of components:
[0158]
[0159] The additives HS2001, HS2001 Make-Up and antioxidant 1 were purchased from Deli Company, USA.
[0160] 2. The above tin plating solution is used in preparing a tin plating layer by spraying on the surface of a semiconductor device. Referring to Example 17, the specific electroplating conditions are shown in Table 12.
[0161] Table 12 Electroplating conditions of comparative example 1
[0162]
[0163] Comparative Example 2
[0164] 1. A tin plating solution and its preparation method Referring to the non-patent literature [Modern Electroplating Handbook] Volume 1, Chapter 7 Tin Plating Solution, wherein the concentrations of tin salt and organic acid are the same as those in Example 17, and the additive adopts the formula of Comparative Example 1, specifically including the following components in the following concentrations:
[0165]
[0166] 2. The above tin spraying solution is used for preparing a tin coating by spraying on the surface of a semiconductor device. Referring to Example 17, the specific electroplating conditions are shown in Table 12.
[0167] Comparative Example 3
[0168] 1. A tin spraying solution, which is the same as that of Example 17, except that the amount of stabilizer is adjusted to 0.1 or 3.6 mmol / L, and specifically comprises components of the following concentrations:
[0169] 2. The preparation method of the above tin spraying solution is as described in Example 1.
[0170] 3. The above tin spraying solution is used for preparing a tin coating by spraying on the surface of a semiconductor device. Referring to Example 17, the specific electroplating conditions are shown in Table 12.
[0171] Comparative Example 4
[0172] 1. A tin spraying solution, referring to Example 17, except that a non-five-membered nitrogen-containing heterocyclic compound (such as 2,5-dimethylfuran) is used as a leveling agent, and the amount of the leveling agent remains unchanged.
[0173] 2. The preparation method of the above tin spraying solution is as described in Example 1.
[0174] 3. The above tin spraying solution is used for preparing a tin coating by spraying on the surface of a semiconductor device. Referring to Example 17, the specific electroplating conditions are shown in Table 12.
[0175] Comparative Example 5
[0176] 1. A tin spraying solution, referring to Example 17, except that S10 polyoxyethylene stearate is used as a stabilizer, and the amount of the stabilizer remains unchanged.
[0177] 2. The preparation method of the above tin spraying solution is as described in Example 1.
[0178] 3. The above tin spraying solution is used for preparing a tin coating by spraying on the surface of a semiconductor device. Referring to Example 17, the specific electroplating conditions are shown in Table 12.
[0179] Test Example 3:
[0180] The electroplating time required for Comparative Examples 1 to 5 to achieve a tin-plated film thickness of ≥3000 nm was tested, and the results are shown in Table 13.
[0181] Table 13 Plating time required for Comparative Examples 1 to 5
[0182]
[0183] Among them: 3a*: the amount of stabilizer is 0.1 mmol / L, 3b*: the amount of stabilizer is 3.6 mmol / L.
[0184] The appearance inspection results of the tin-plated semiconductor device products obtained in Comparative Examples 1 to 5 using a 40x optical microscope are shown in Table 14.
[0185] Table 14 Appearance test results of Comparative Examples 1 to 5
[0186]
[0187] The tin plating film thickness results of Comparative Examples 1 to 5 are shown in Table 15.
[0188] Table 15 Tin plating film thickness results of Comparative Examples 1 to 5 (nm)
[0189]
[0190] The soldering performance test results of Comparative Examples 1 to 5 are shown in Table 16.
[0191] Table 16 Results of solder test defect area inspection of tin-plated semiconductor device products obtained in Comparative Examples 1 to 5 (%)
[0192]
[0193] Combining Tables 13 to 16, it can be seen that Comparative Example 1 uses the existing tin plating solution as the tin spraying solution, the concentration of tin salt and organic acid in Comparative Example 2 is the same as that in Example 17, and the additive adopts the formula of Comparative Example 1. Comparative Examples 1 and 2 use the same spray electroplating equipment as in Example 1, and the same electroplating conditions. To meet the tin film thickness ≥ 3000 nm, the required electroplating time is increased to 109 sec and 93 sec respectively compared with 18 sec in Example 17; the appearance of the prepared semiconductor device tin-plated sample is uneven and not smooth, and it is judged to be unqualified; the tin plating layer is detected, the film thickness distribution is uneven, and the film thickness difference Max-Min is 534 nm and 527 nm respectively; the solder test defect area inspection results are 25.9% and 26.2% respectively, the soldering performance is very poor, and the comprehensive evaluation is at an unqualified level. It can be seen that the existing tin plating solution based on Comparative Examples 1 and 2 cannot solve the technical problem of the present invention at all.
[0194] Compared with Example 17, the amount of stabilizer in Comparative Example 3a* is reduced to 0.1 mmol / L, and the amount of stabilizer in Comparative Example 3b* is increased to 3.6 mmol / L; the electroplating time required for Comparative Example 3a* and Comparative Example 3b* is not much different from 18 sec in Example 17, which are 23 sec and 19 sec respectively; the appearance inspection of the tin-plated samples of semiconductor devices is the same as that of Example 17 in terms of no bubbles, no pits, no scratches, no leakage plating, and no penetration plating, but the film thickness uniformity and surface smoothness are slightly poor, so the appearance is judged to be good; the tin-plated film thickness detection results are not much different from the results of Example 17; the solder test defect area inspection results are 0.5% and 0.6%, respectively, which are lower than that of Example 17, but still at a good level; from the above results, it can be seen that too high or too low an amount of stabilizer in the tin spraying solution of the present invention may lead to a decrease in tin plating performance.
[0195] In Comparative Example 4, except that the leveler is replaced by non-nitrogen-containing five-membered heterocyclic 2,5-dimethylfuran instead of the nitrogen-containing five-membered heterocyclic 5-(propan-2-yl)-1,3-oxazole-4-carboxylic acid in Example 17, the other components remain unchanged; in Comparative Example 5, except that the 50wt% sodium polyacrylate aqueous solution in Example 17 is replaced by non-carboxylic acid polymer S10 polyoxyethylene stearate, the other components remain unchanged; Comparative Examples 4 and 5 use the same jet electroplating equipment as in Example 1, and the electroplating conditions are basically the same as in Example 17. In order to meet the tin film thickness of ≥3000 nm, the required electroplating time is increased to 65 sec and 87 sec compared with 18 sec in Example 17. The prepared semiconductor device tin-plated samples are uneven and not smooth in appearance inspection and are judged to be unqualified; the tin plating layer is detected, and the film thickness distribution is uneven, and the film thickness difference Max-Min is 351 and 362 respectively. nm; the solder test defect area inspection results are 13.6% and 13.9% respectively, the solder performance is very poor, and the comprehensive evaluation is at an unqualified level. It can be seen that the joint action of the five-membered nitrogen-containing heterocyclic compound and the polymer compound is one of the key technical features for solving the technical problem of the present invention.
[0196] Comparative Example 6
[0197] 1. The composition and preparation method of the tin plating solution are the same as those of Comparative Example 1;
[0198] 2. The application of the above tin plating solution in preparing a tin plating layer by electroplating a semiconductor device is different from Example 17 in that the semiconductor device is immersed in the tin plating solution for electroplating; a pulse electroplating power supply is used; and the electroplating conditions are shown in Table 17.
[0199] Comparative Example 7 to Comparative Example 16
[0200] 1. The composition and preparation method of the tin plating solution are the same as those of Comparative Example 1;
[0201] 2. The application of the above tin plating solution in preparing a tin plating layer by electroplating of a semiconductor device is different from that of Comparative Example 6 in terms of the electroplating conditions, as shown in Table 17.
[0202] Table 17 Immersion tin plating conditions for Comparative Examples 6 to 16
[0203]
[0204] Test Example 4:
[0205] The tin-plated semiconductor device products obtained in Comparative Examples 6 to 16 were subjected to appearance inspection, tin plating film thickness inspection, and soldering performance test, respectively. The results are shown in Tables 18 to 20.
[0206] Table 18 Appearance test results of Comparative Examples 6 to 16
[0207]
[0208] Table 19 Tin plating film thickness results of Comparative Examples 6 to 16 (nm)
[0209]
[0210] Table 20 Results of solder test defect area inspection for Comparative Examples 6 to 16 (%)
[0211]
[0212] Table 21 Comparison of film thickness errors of Examples 12 to 22 and Comparative Examples 6 to 16
[0213]
[0214] Table 22 Surface roughness (Ra) test results (nm) of Examples 12 to 22 and Comparative Examples 6 to 16
[0215]
[0216] By comparing Table 8 and Table 17, it can be seen that based on the tin spraying solution and the spraying process of the present invention, the preferred scheme is Example 14 to Example 20, and the corresponding required electroplating time is 9 to 38 seconds; and based on the existing tin plating solution of Comparative Example 6 and the immersion plating processes of Comparative Example 6 to Comparative Example 16, the preferred scheme is Comparative Example 10 to Comparative Example 13, and the corresponding required electroplating time is 32 to 51 seconds; it can be seen that the tin spraying solution and the spraying process based on the present invention can shorten the electroplating time and is more conducive to practical application.
[0217] Comparing Table 9 and Table 18, it can be seen that according to the optimization results of the electron microscope 5000 times, based on the tin spraying solution and the spraying process of the present invention, the preferred schemes are Examples 14 to 20, and the corresponding current density is preferably in the range of 11 to 50 A / dm 2 Based on the existing tin plating solution of Comparative Example 6 and the immersion plating process of Comparative Examples 6 to 16, the preferred scheme is Comparative Examples 10 to 13, and the corresponding current density is preferably in the range of 10 to 19 A / dm 2 It can be seen that the tin spraying solution and the spraying process based on the present invention have a wider selection range of electroplating conditions and are more conducive to practical applications.
[0218] According to Table 21, the film thickness error of Examples 11 to 22 is no more than 7.9%, while the film thickness error of Comparative Examples 6 to 16 is as high as more than 18%. It can be seen that the tin spraying solution and spraying process based on the present invention are significantly reduced in film thickness error and have better film thickness distribution uniformity compared to the existing tin plating solution based on Comparative Example 6 and the immersion plating process of Comparative Examples 6 to 16, thereby improving the electroplating quality of semiconductor device tin-plated products. The larger the film thickness error, on the one hand, is not conducive to the uniformity of film thickness distribution; on the other hand, it will also increase the loss of tin metal in the plating solution and increase the electroplating processing cost.
[0219] According to Table 22, the surface roughness of Examples 11 to 22 is no higher than 82 nm, while the surface roughness of Comparative Examples 6 to 16 is as high as 351 nm or more; thus, it can be seen that the tin spraying solution and the spraying process based on the present invention greatly reduce the surface roughness of the plated parts compared with the existing tin plating solution based on Comparative Example 6 and the immersion plating processes of Comparative Examples 6 to 16, thereby improving the electroplating quality of tin-plated products of semiconductor devices.
[0220] In summary, the tin spraying solution and spraying process of the present invention, compared with the existing tin-plating electroplating solution based on Comparative Example 6 and the immersion plating processes of Comparative Examples 6 to 16, can improve the appearance of the coating, enhance the uniformity of film thickness distribution, reduce film thickness error, reduce the solder test defect area, and reduce surface roughness. While improving the electroplating quality of tin-plated products of semiconductor devices, it is beneficial to shorten the electroplating time, broaden the current density selection range, and is more conducive to practical applications.
[0221] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A tinning solution, characterized in that The components are included in the following concentrations: Wherein, the tin salt includes at least one of 2-hydroxyethyl-1-tin sulfonate, tin methane sulfonate, tin ethyl sulfonate, tin propyl sulfonate, tin hydroxymethane sulfonate or 2-hydroxybutyl-1-tin sulfonate; The stabilizer includes at least one of the following: Polyacrylic acid, sodium polyacrylate, ammonium polyacrylate, hydroxypropyl acrylate polymer with an average molecular weight of less than 2000, acrylic acid-maleic acid copolymer with a molecular weight of 800-1200, polymaleic acid or polyethylene glycol with a molecular weight of 200-400 and their derivatives; The leveler includes nitrogen-containing five-membered heterocyclic compounds.
2. The tin plating solution according to claim 1, characterized in that The leveler includes at least one of azoles, imidazoles, oxazoles or thiazoles.
3. The tin plating solution according to claim 2, characterized in that: The pyrroles include at least one of 2-acetylpyrrole, 4-pyrrolidin-1-pyridine-2-carboxylic acid hydrochloride, pyrrole-3-carboxylic acid, 2-nitro-1H-pyrrole, 2-methylpyrrole-3-carboxylic acid ethyl ester, 3-nitropyrrole, 1-ethylpyrrolidin-3-ol, 1-(2-hydroxyethyl)pyrrole or 4-(pyrrolidin-3-yl)pyridine hydrochloride; The imidazoles include at least one of 4-nitroimidazole, 2-nitroimidazole, imidazolidinyl urea, imidazole-5-acetic acid, 2,4-dinitroimidazole, 2-(1-imidazolyl)acetic acid, 5-methyl-4-nitroimidazole, imidazole-4-amine dihydrochloride or L-histidine; The oxazoles include at least one of oxazole-5-acetic acid, 2-amino-1, 3-oxazole-4-carboxylic acid, 5-(1-methyl-2-pyrrolyl)isoxazole-3-carboxylic acid, 3-methyl-4-nitroisoxazole-5-carboxylic acid methyl ester or 5-(isopropyl)-1,3-oxazole-4-carboxylic acid; The thiazoles include at least one of thiazole-5-carboxylic acid, thiazole-2-sulfonic acid, 4-nitroisothiazole, thiazole-2(3H)-thione, D-4-thiazolealanine, 2-bromo-5-nitrothiazole, 1-(thiazol-2-yl)ethanol, 2-amino-5-nitrothiazole, and (Z)-2-(2-aminothiazol-4-yl)-2-methoxycarbonylmethoxyiminoacetic acid.
4. The tin plating solution according to claim 1, characterized in that The wetting agent includes at least one of octylphenol polyoxyethylene ether with a polymerization degree of 7<≤20, sodium salt of diisooctyl sulfosuccinate, or 1,2-propylene glycol polyoxypropylene polyoxyethylene.
5. The tin plating solution according to claim 1, characterized in that: The organic acid includes at least one of methanesulfonic acid, ethylsulfonic acid, propylsulfonic acid, 2-hydroxyethyl-1-sulfonic acid, hydroxymethanesulfonic acid or 2-hydroxybutyl-1-sulfonic acid.
6. The tin plating solution according to claim 1, characterized in that The stabilizer comprises at least one of heptapolyethylene glycol, octapolyethylene glycol, decapolyethylene glycol, aminopolyethylene glycol hydroxyl with a molecular weight of 300-500, M-tetrapolyethylene glycol-sulfonic acid, polyethylene glycol diacrylate with a molecular weight of 800-1200, polyethylene glycol dicarboxylic acid with a molecular weight of 500-700, mercaptotetrapolyethylene glycol, polyethylene glycol dicarboxylic acid with a molecular weight of 800-1200, amino-heptapolyethylene glycol-carboxylic acid, and amino-nonapolyethylene glycol-carboxylic acid.
7. Use of the tin plating solution according to any one of claims 1 to 6 in a spraying process.
8. A method for preparing the tin plating solution according to any one of claims 1 to 6, characterized in that: The steps include: (1) Add a certain amount of deionized water to a container, heat it, and under stirring conditions, add tin salt, organic acid, wetting agent, stabilizer and leveling agent in small amounts and multiple times according to the required volume of the tin-plating solution and the final concentration of each component in the tin-plating solution, and continue to add deionized water to 70-90% of the required volume of the tin-plating solution to obtain solution A; titrate and analyze the total acid content with a standard sodium hydroxide solution to control the total acid content in solution A to be 230-250 mL / L; (2) Add deionized water to solution A until the required volume of the tin-plating solution is reached to obtain solution G, that is, a tin-plating solution is obtained.
9. A method for preparing a tin coating by spraying on the surface of a semiconductor device, characterized in that: The tin plating solution according to any one of claims 1 to 6 is used as a tin spraying solution; the method comprises the following steps: S1. Degreasing and acid activation treatment of the semiconductor device to be processed; S2, according to the electroplating area and the form of the plated part, select the corresponding tin spraying conditions, configure the corresponding anode mask, install the anode mask and the semiconductor device to be processed in the electroplating device; the current density of the tin spraying solution during electroplating is 11 to 50 A / dm 2 , the temperature of the tin spraying solution is 40-50°C; S3, selecting a corresponding electrolytic power source according to the plated part to carry out electroplating; S4, regularly testing the tin concentration and total acid content in the tin spraying solution, judging whether the change value of the tin concentration and the total acid content exceeds the limit value, and automatically adding the corresponding components; S5, completing the spray electroplating process on the plated parts.
10. The method according to claim 9, characterized in that The electrolysis power supply includes a forward and reverse pulse power supply or a single pulse power supply.