A preparation method of leak-proof pulp layer paper and its application in batteries

By using leak-proof pulp layer paper prepared from materials such as modified diatomite and dopamine hydrochloride coating layers in carbonic zinc-manganese dioxide dry batteries, the problems of zinc electrode corrosion and leakage are solved, the battery cost is reduced, and the battery cost is improved. Improve the flame retardant performance and tensile strength of the battery.

CN118639473BActive Publication Date: 2024-10-29LIAOYUAN JINYU JOURNEY DIAPHRAGM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411124044.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-29
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

During the use, storage or intermittent discharge of existing carbonic zinc-manganese dioxide dry batteries, the zinc electrode comes into contact with the acidic substances in the electrolyte, causing corrosion, resulting in reduced battery capacity, swelling and leakage, and a significant increase in the weight of the zinc cylinder. the battery cost.

Method used

The leak-proof pulp layer paper is prepared using modified diatomite and dopamine hydrochloride coating layer, phosphorus-silicon synergistic flame retardant and amino starch, and is coated on the inner wall of the zinc cylinder to form a protective layer to inhibit zinc electrode corrosion and Improve flame retardant properties and ionic conductivity.

Benefits of technology

Effectively prevent zinc electrode corrosion, reduce battery leakage, reduce the weight of the zinc cylinder, reduce production costs, and improve the flame retardant performance and tensile strength of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for preparing a leak-proof pulp layer paper and its application in a battery, and relates to the technical field of battery materials. When preparing the leak-proof pulp layer paper, the invention loads 8-hydroxyquinoline into diatomite, and then polymerizes and deposits dopamine hydrochloride on the surface of diatomite to obtain polydopamine-coated modified diatomite; starch is sequentially reacted with 3-aminopropyltriethoxysilane and phosphorus silicon synergistic flame retardant to obtain modified amino starch; polyvinyl alcohol is reacted with vinyl pyridinium salt to obtain modified polyvinyl alcohol; modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomite, and bismuth oxide are prepared into a mixed slurry and coated on a base paper to obtain leak-proof pulp layer paper. When the leak-proof pulp layer paper prepared by the invention is applied to a carbon battery, the leakage resistance of the battery during discharge can be improved, so that the battery can achieve an excellent leakage resistance effect, and the performance and service life of the battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery materials, and in particular to a method for preparing leakage-proof pulp layer paper and application thereof in batteries. Background Art

[0002] Carbon battery is the full name of neutral zinc-manganese dioxide dry battery. Due to different structures, it can be divided into paste battery and paperboard battery. The one with pulp paper as the isolation layer is called paperboard battery. Due to its low price and safe and reliable use, it is widely used in electronic and electrical products.

[0003] The electrolyte of carbon battery is zinc chloride / ammonium chloride / water solution; the positive electrode is electrolytic manganese dioxide, acetylene black, etc., and a conductive fluid carbon rod is inserted in the middle; zinc has a low hydrogen evolution overpotential and is used as the negative electrode of the battery and also as the shell. The positive and negative electrodes are separated by a pulp paper diaphragm to ensure that there is no short circuit and the conductive ions in the electrolyte can pass smoothly. The disadvantage of carbon battery is that during use, storage or intermittent discharge, the zinc electrode contacts with the acidic substances in the electrolyte and corrodes, causing the battery capacity to decrease and swell. The thinning of the zinc cylinder will cause leakage and corrode electrical equipment. The disposable carbon battery currently used has strict requirements on the weight of the zinc cylinder. This is mainly because the zinc cylinder needs to have a sufficient wall thickness to ensure that the zinc cylinder wall will not be perforated during the discharge or long-term storage of the battery, thereby preventing the occurrence of leakage. The heavy weight of the zinc cylinder has caused great pressure on the battery cost. In view of this, according to the actual situation of the battery during storage and discharge, in-depth research and improvement of the pulp layer paper close to the inner wall of the zinc cylinder inside the battery is carried out. It is of great significance to reduce the weight of the zinc cylinder and reduce production costs while ensuring battery performance. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing leakage-proof pulp layer paper and its application in batteries, so as to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing leak-proof pulp layer paper, the method comprising polymerizing and depositing dopamine hydrochloride on the surface of modified diatomite to obtain polydopamine-coated modified diatomite; reacting starch with 3-aminopropyltriethoxysilane to obtain amino starch; reacting amino starch with a phosphorus-silicon synergistic flame retardant to obtain modified amino starch; reacting polyvinyl alcohol with vinyl pyridinium salt to obtain modified polyvinyl alcohol; preparing a mixed slurry of modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomite and bismuth oxide, coating the mixed slurry on base paper, drying, slitting and rewinding the paper;

[0007] The modified diatomaceous earth is prepared by loading 8-hydroxyquinoline into diatomaceous earth;

[0008] The phosphorus-silicon synergistic flame retardant is prepared by reacting 2,4,6,8-tetramethylcyclotetrasiloxane with allyl phosphoric acid;

[0009] The vinyl pyridinium salt is prepared by reacting 4-vinyl pyridine with 1,6-dichlorohexane;

[0010] The base paper is Xueshan brand battery base paper with a thickness of 80 microns.

[0011] As an optimization, the method for preparing the leakage-proof pulp layer paper includes the following preparation steps:

[0012] (1) Modified diatomaceous earth, dopamine hydrochloride and deionized water are mixed uniformly in a mass ratio of 1:(2-3):(50-60), stirred at 10-30°C and 300-500 r / min for 10-20 min, tris(hydroxymethyl)aminomethane (0.04-0.06 times the mass of dopamine hydrochloride) is added, stirred at 30-40°C and 300-500 r / min for 18-20 h, centrifuged, washed with deionized water for 3-5 times, and dried at 50-60°C under vacuum conditions for 8-10 h to obtain polydopamine-coated modified diatomaceous earth;

[0013] (2) Mix starch, 3-aminopropyltriethoxysilane, and 10-20% ethanol aqueous solution in a mass ratio of 1:(0.3-0.5):(10-12), adjust the pH to 4 with acetic acid, stir and react at 55-65°C, 300-500 r / min for 3-4 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain amino starch; mix amino starch, phosphorus silicon synergistic flame retardant, and 4-6% acetic acid aqueous solution in a mass ratio of 1:(1.5-1.7):(10-12), add dicyclohexylcarbodiimide (0.03-0.05 times the mass of amino starch), stir and react at 70-80°C, 300-500 r / min for 2-3 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain modified amino starch;

[0014] (3) Mix ammonium cerium nitrate and deionized water in a mass ratio of 1:(6-8) to prepare an ammonium cerium nitrate solution; mix polyvinyl alcohol, vinyl pyridinium salt and deionized water in a mass ratio of 1:(1.5-1.7):(10-12) to prepare an ammonium cerium nitrate solution; adjust the pH to 5.8-6.0 with a 1 mol / L nitric acid aqueous solution, uniformly add 3-4 times the mass of polyvinyl alcohol to the mixture dropwise within 20 minutes, stir at 40-42°C and 300-500 r / min for 4-6 hours, and dry at 40-50°C under vacuum for 8-10 hours to obtain modified polyvinyl alcohol;

[0015] (4) Mix the modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water in a mass ratio of 1:(0.1-0.12):(0.01-0.02):(0.03-0.05):(0.0002-0.0003):(2-3) and adjust the viscosity to 180-200 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 28~30g / m 2 The drying temperature is 100~120℃; the drying speed is 25~30m / min for winding; slitting and rewinding to obtain leakage-proof pulp layer paper.

[0016] As an optimization, the preparation method of the modified diatomite in step (1) is as follows: 8-hydroxyquinoline and anhydrous ethanol are mixed evenly in a mass ratio of 1:(9-11) to prepare an 8-hydroxyquinoline solution; diatomite with a particle size of 10-20 μm and the 8-hydroxyquinoline solution are mixed evenly in a mass ratio of 1:(8-10), ultrasonically dispersed for 2-3 hours, and dried at 50-60° C. for 10-12 hours under vacuum conditions to obtain modified diatomite.

[0017] As an optimization, the preparation method of the phosphorus-silicon synergistic flame retardant in step (2) is: add 2,4,6,8-tetramethylcyclotetrasiloxane and allyl phosphoric acid in a molar ratio of 1:4 to toluene with a mass of 12 to 14 times that of 2,4,6,8-tetramethylcyclotetrasiloxane, then add chloroplatinic acid with a mass of 0.03 to 0.05 times that of 2,4,6,8-tetramethylcyclotetrasiloxane, stir and react at 70 to 80°C and 300 to 500 r / min for 2 to 3 hours, and dry at 50 to 60°C under vacuum conditions for 8 to 10 hours to obtain the phosphorus-silicon synergistic flame retardant.

[0018] As an optimization, the deacetylation degree of the amino starch in step (2) is 95%, and the weight average molecular weight is 180-200 kDa.

[0019] As an optimization, the preparation method of the vinyl pyridinium salt in step (3) is as follows: under a nitrogen atmosphere, 4-vinyl pyridine and 1,6-dichlorohexane are added in a molar ratio of 1:1 to dichloromethane which is 10 to 12 times the mass of 4-vinyl pyridine, and the mixture is stirred at 30 to 40° C. and 300 to 500 r / min for 6 to 8 hours, and then dried at 50 to 60° C. under vacuum conditions for 8 to 10 hours to obtain the vinyl pyridinium salt.

[0020] As an optimization, the number average molecular weight of the polyvinyl alcohol in step (3) is 80,000 to 100,000.

[0021] As an optimization, the degree of polymerization of the polyacrylamide in step (4) is 3000-4000.

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0023] When preparing the leakage-proof pulp layer paper, the present invention loads 8-hydroxyquinoline into diatomite to obtain modified diatomite; polymerizes and deposits dopamine hydrochloride on the surface of the modified diatomite to obtain polydopamine-coated modified diatomite; reacts 2,4,6,8-tetramethylcyclotetrasiloxane with allyl phosphoric acid to obtain a phosphorus-silicon synergistic flame retardant; reacts starch with 3-aminopropyltriethoxysilane to obtain amino starch; reacts amino starch with the phosphorus-silicon synergistic flame retardant to obtain modified amino starch; reacts 4-vinylpyridine with 1,6-dichlorohexane to obtain vinyl pyridinium salt; reacts polyvinyl alcohol with vinyl pyridinium salt to obtain modified polyvinyl alcohol; and prepares a mixed slurry of modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomite and bismuth oxide, and applies the mixed slurry on base paper, and performs drying, slitting and rewinding to obtain the leakage-proof pulp layer paper.

[0024] First, 8-hydroxyquinoline is loaded into diatomaceous earth to obtain modified diatomaceous earth; dopamine hydrochloride is polymerized and deposited on the surface of the modified diatomaceous earth to obtain polydopamine-coated modified diatomaceous earth; during the use, storage or intermittent discharge of the zinc-manganese battery, the zinc cylinder as the negative electrode comes into contact with the acidic substances in the electrolyte and is corroded, causing the battery capacity to decrease and swell, and the zinc cylinder becomes thinner and leaks, thereby corroding electrical equipment; diatomaceous earth is an inorganic porous material with a rich pore structure and is heat-resistant and corrosion-resistant. 8-hydroxyquinoline is a metal corrosion inhibitor , which can complex with metal ions and be adsorbed on the metal surface to form a protective layer to inhibit corrosion of the metal surface; 8-hydroxyquinoline is loaded into the pores of diatomaceous earth to obtain modified diatomaceous earth, and then dopamine hydrochloride is polymerized and coated on the surface of the modified diatomaceous earth to obtain polydopamine-coated modified diatomaceous earth. The polydopamine on the polydopamine-coated modified diatomaceous earth will be gradually decomposed in an acidic electrolyte to release the corrosion inhibitor 8-hydroxyquinoline, thereby achieving the purpose of long-term corrosion inhibition of the negative electrode of the zinc-manganese battery and preventing the negative electrode of the battery from being corroded and causing electrolyte leakage.

[0025] Secondly, the Si-H bond on 2,4,6,8-tetramethylcyclotetrasiloxane and the carbon-carbon double bond on allyl phosphoric acid are subjected to a silylation reaction to obtain a phosphorus-silicon synergistic flame retardant; starch is reacted with 3-aminopropyltriethoxysilane to obtain amino starch; amino starch is reacted with an excess of phosphorus-silicon synergistic flame retardant to obtain modified amino starch, and the amino group on the amino starch reacts with the phosphoric acid group on the phosphorus-silicon synergistic flame retardant to form a phosphoramide bond, and at the same time, siloxane, phosphorus and phosphoric acid groups are introduced into the modified amino starch, and the phosphorus element can It captures free radicals and promotes the formation of carbon layer to isolate heat and oxygen, giving the leak-proof pulp layer paper excellent flame retardant properties; the layered SiO2 formed by the degradation of siloxane during combustion migrates to the surface of the carbon layer, making the carbon layer denser, inhibiting the oxidation of the carbon layer, enhancing the stability of the carbon layer at high temperatures, and further improving the flame retardant properties of the leak-proof pulp layer paper; amino starch contains a large number of hydrophilic groups, has a high affinity with the electrolyte, and has good wettability to the electrolyte. The good wettability between the leak-proof pulp layer paper and the electrolyte helps to improve the ionic conductivity.

[0026] Finally, 4-vinylpyridine is reacted with 1,6-dichlorohexane to obtain vinyl pyridinium salt; polyvinyl alcohol is reacted with vinyl pyridinium salt to obtain modified polyvinyl alcohol, and pyridinium salt and chlorine atoms are introduced into the side chain of polyvinyl alcohol. The introduction of pyridinium salt can further improve the ionic conductivity of the anti-leakage slurry paper; the chloride ions introduced into the side chain of polyvinyl alcohol can react with the amino groups on the polydopamine-coated modified diatomaceous earth to form a cross-linked network, inhibit the relative slip of the molecular chains, and give the anti-leakage slurry paper excellent tensile strength; the pyridinium salt introduced into the side chain of polyvinyl alcohol can also combine with the phosphate groups on the modified amino starch through positive and negative charges to form a cross-linked network, inhibit the relative slip of the molecular chains, and further improve the tensile strength of the anti-leakage slurry paper. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] Embodiment 1: A method for preparing leakage-proof pulp layer paper, the method for preparing leakage-proof pulp layer paper comprising the following preparation steps:

[0029] (1) 8-hydroxyquinoline and anhydrous ethanol were mixed in a mass ratio of 1:9 to prepare an 8-hydroxyquinoline solution; diatomaceous earth with a particle size of 10 μm and the 8-hydroxyquinoline solution were mixed in a mass ratio of 1:8, ultrasonically dispersed for 2 hours, and dried at 50°C for 12 hours under vacuum conditions to obtain modified diatomaceous earth; modified diatomaceous earth, dopamine hydrochloride, and deionized water were mixed in a mass ratio of 1:2:50, stirred at 10°C and 300 r / min for 20 minutes, tris(hydroxymethyl)aminomethane (0.04 times the mass of dopamine hydrochloride) was added, stirred at 30°C and 300 r / min for 20 hours, centrifuged, washed with deionized water three times, and dried at 50°C for 10 hours under vacuum conditions to obtain polydopamine-coated modified diatomaceous earth;

[0030] (2) 2,4,6,8-tetramethylcyclotetrasiloxane and allyl phosphoric acid were added in a molar ratio of 1:4 to toluene (12 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane), and then chloroplatinic acid (0.03 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane) was added, and the mixture was stirred at 70°C and 300 r / min for 3 h. The mixture was dried at 50°C for 10 h under vacuum conditions to obtain a phosphorus-silicon synergistic flame retardant. Starch, 3-aminopropyltriethoxysilane, and 10% ethanol aqueous solution were added in a mass ratio of 1:4. :0.3:10, mix evenly, adjust the pH to 4 with acetic acid, react at 55°C, 300r / min with stirring for 4h, dry at 50°C for 10h under vacuum conditions to obtain amino starch; amino starch, phosphorus silicon synergistic flame retardant, and 4% acetic acid aqueous solution are mixed evenly at a mass ratio of 1:1.5:10, add dicyclohexylcarbodiimide (0.03 times the mass of amino starch), react at 70°C, 300r / min with stirring for 3h, dry at 50°C for 10h under vacuum conditions to obtain modified amino starch;

[0031] (3) Under nitrogen atmosphere, 4-vinylpyridine and 1,6-dichlorohexane were added to dichloromethane (10 times the mass of 4-vinylpyridine) in a molar ratio of 1:1, and the mixture was stirred at 30°C and 300 r / min for 8 hours, and dried at 50°C for 10 hours under vacuum conditions to obtain vinyl pyridine salt; ammonium cerium nitrate and deionized water were mixed at a mass ratio of 1:6 to prepare ammonium cerium nitrate solution; polyvinyl alcohol, vinyl pyridine salt and deionized water were mixed at a mass ratio of 1:1.5:10, and the pH was adjusted to 5.8 with a nitric acid aqueous solution with a molar concentration of 1 mol / L, and the ammonium cerium nitrate solution (3 times the mass of polyvinyl alcohol) was uniformly added dropwise within 20 minutes, and the mixture was stirred at 40°C and 300 r / min for 6 hours, and dried at 40°C for 10 hours under vacuum conditions to obtain modified polyvinyl alcohol;

[0032] (4) Modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water were mixed evenly in a mass ratio of 1:0.1:0.01:0.03:0.0002:2, and the viscosity was adjusted to 180 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 28g / m 2 , the drying temperature is 100℃; the drying speed is 25m / min for winding; slitting and rewinding are carried out to obtain the leakage-proof pulp layer paper.

[0033] Embodiment 2: A method for preparing leakage-proof pulp layer paper, the method for preparing leakage-proof pulp layer paper comprising the following preparation steps:

[0034] (1) 8-hydroxyquinoline and anhydrous ethanol were mixed in a mass ratio of 1:10 to prepare an 8-hydroxyquinoline solution; diatomaceous earth with a particle size of 15 μm and the 8-hydroxyquinoline solution were mixed in a mass ratio of 1:9, ultrasonically dispersed for 2.5 hours, and dried at 55°C for 11 hours under vacuum conditions to obtain modified diatomaceous earth; modified diatomaceous earth, dopamine hydrochloride, and deionized water were mixed in a mass ratio of 1:2.5:55, stirred at 20°C and 400 r / min for 15 minutes, tris(hydroxymethyl)aminomethane (0.05 times the mass of dopamine hydrochloride) was added, stirred at 35°C and 400 r / min for 19 hours, centrifuged, washed with deionized water 4 times, and dried at 55°C for 9 hours under vacuum conditions to obtain polydopamine-coated modified diatomaceous earth;

[0035] (2) 2,4,6,8-tetramethylcyclotetrasiloxane and allyl phosphoric acid were added in a molar ratio of 1:4 to toluene (13 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane), and then chloroplatinic acid (0.04 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane) was added, and the mixture was stirred at 75°C and 400 r / min for 2.5 h. The mixture was dried at 55°C under vacuum for 9 h to obtain a phosphorus-silicon synergistic flame retardant. Starch, 3-aminopropyltriethoxysilane, and 15% ethanol aqueous solution were mixed in a mass ratio of 1: 0.4:11 was mixed evenly, the pH was adjusted to 4 with acetic acid, the mixture was stirred at 60°C and 400r / min for 3.5h, and dried at 55°C for 9h under vacuum conditions to obtain amino starch; amino starch, phosphorus silicon synergistic flame retardant, and 5% acetic acid aqueous solution were mixed evenly at a mass ratio of 1:1.6:11, dicyclohexylcarbodiimide (0.04 times the mass of amino starch) was added, the mixture was stirred at 75°C and 400r / min for 2.5h, and dried at 55°C for 9h under vacuum conditions to obtain modified amino starch;

[0036] (3) Under nitrogen atmosphere, 4-vinylpyridine and 1,6-dichlorohexane were added to dichloromethane (11 times the mass of 4-vinylpyridine) in a molar ratio of 1:1, and the mixture was stirred at 35°C and 400 r / min for 7 hours, and dried at 55°C for 9 hours under vacuum conditions to obtain vinyl pyridine salt; ammonium cerium nitrate and deionized water were mixed at a mass ratio of 1:7 to prepare ammonium cerium nitrate solution; polyvinyl alcohol, vinyl pyridine salt and deionized water were mixed at a mass ratio of 1:1.6:11, and the pH was adjusted to 5.9 with a nitric acid aqueous solution with a molar concentration of 1 mol / L, and ammonium cerium nitrate solution (3.5 times the mass of polyvinyl alcohol) was added dropwise at a uniform rate within 20 minutes, and the mixture was stirred at 41°C and 400 r / min for 5 hours, and dried at 45°C for 9 hours under vacuum conditions to obtain modified polyvinyl alcohol;

[0037] (4) Modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water were mixed evenly in a mass ratio of 1:0.11:0.015:0.04:0.00025:2.5, and the viscosity was adjusted to 190 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 29g / m 2 The drying temperature is 110°C; the drying speed is 27.5m / min for winding; slitting and rewinding are carried out to obtain leakage-proof pulp layer paper.

[0038] Embodiment 3: A method for preparing leakage-proof pulp layer paper, the method for preparing leakage-proof pulp layer paper comprising the following preparation steps:

[0039] (1) 8-hydroxyquinoline and anhydrous ethanol were mixed in a mass ratio of 1:11 to prepare an 8-hydroxyquinoline solution; diatomaceous earth with a particle size of 20 μm and the 8-hydroxyquinoline solution were mixed in a mass ratio of 1:10, ultrasonically dispersed for 3 hours, and dried at 60°C for 10 hours under vacuum conditions to obtain modified diatomaceous earth; modified diatomaceous earth, dopamine hydrochloride, and deionized water were mixed in a mass ratio of 1:3:60, stirred at 30°C and 500 r / min for 10 minutes, tris(hydroxymethyl)aminomethane (0.06 times the mass of dopamine hydrochloride) was added, stirred at 40°C and 500 r / min for 18 hours, centrifuged, washed with deionized water 5 times, and dried at 60°C for 8 hours under vacuum conditions to obtain polydopamine-coated modified diatomaceous earth;

[0040] (2) 2,4,6,8-tetramethylcyclotetrasiloxane and allyl phosphoric acid were added in a molar ratio of 1:4 to toluene (14 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane), and then chloroplatinic acid (0.05 times the mass of 2,4,6,8-tetramethylcyclotetrasiloxane) was added, and the mixture was stirred at 80°C and 500 r / min for 2 h. The mixture was dried at 60°C under vacuum for 8 h to obtain a phosphorus-silicon synergistic flame retardant. Starch, 3-aminopropyltriethoxysilane, and 20% ethanol aqueous solution were added in a molar ratio of 1:4 to obtain a phosphorus-silicon synergistic flame retardant. :0.5:12, adjust the pH to 4 with acetic acid, stir and react at 65°C, 500r / min for 3h, and dry at 60°C for 8h under vacuum to obtain amino starch; amino starch, phosphorus silicon synergistic flame retardant, and 6% acetic acid aqueous solution are mixed at a mass ratio of 1:1.7:12, add dicyclohexylcarbodiimide (0.05 times the mass of amino starch), stir and react at 80°C, 500r / min for 2h, and dry at 60°C for 8h under vacuum to obtain modified amino starch;

[0041] (3) Under nitrogen atmosphere, 4-vinylpyridine and 1,6-dichlorohexane were added to dichloromethane (12 times the mass of 4-vinylpyridine) in a molar ratio of 1:1, and the mixture was stirred at 40°C and 500 r / min for 6 hours, and dried at 60°C for 8 hours under vacuum conditions to obtain vinyl pyridine salt; ammonium cerium nitrate and deionized water were mixed at a mass ratio of 1:8 to prepare ammonium cerium nitrate solution; polyvinyl alcohol, vinyl pyridine salt and deionized water were mixed at a mass ratio of 1:1.7:12, and the pH was adjusted to 6.0 with a nitric acid aqueous solution with a molar concentration of 1 mol / L, and ammonium cerium nitrate solution (4 times the mass of polyvinyl alcohol) was uniformly added dropwise within 20 minutes, and the mixture was stirred at 42°C and 500 r / min for 4 hours, and dried at 50°C for 8 hours under vacuum conditions to obtain modified polyvinyl alcohol;

[0042] (4) Modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water were mixed evenly in a mass ratio of 1:0.12:0.02:0.05:0.0003:3, and the viscosity was adjusted to 200 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 30g / m 2 , the drying temperature is 120℃; the drying speed is 30m / min for winding; slitting and rewinding are carried out to obtain the leakage-proof pulp layer paper.

[0043] Comparative Example 1

[0044] The difference between the preparation method of the leakproof pulp layer paper of Comparative Example 1 and Example 2 is that step (1) is not performed, and step (4) is modified as follows: modified amino starch, modified polyvinyl alcohol, polyacrylamide, bismuth oxide, and deionized water are mixed uniformly in a mass ratio of 1:0.11:0.015:0.00025:2.5 to prepare a mixed slurry; the mixed slurry is uniformly coated on the battery base paper, and the coating amount is 29g / m 2 , the drying temperature is 110°C; the drying speed is 27.5 m / min; the paper is rolled up; the paper is cut and rewound to obtain the leak-proof pulp layer paper. The remaining steps are the same as those in Example 2.

[0045] Comparative Example 2

[0046] The difference between the preparation method of the leakproof pulp layer paper of Comparative Example 2 and Example 2 lies in the difference in step (2), where step (2) is modified as follows: starch, 3-aminopropyltriethoxysilane, and 15% ethanol aqueous solution are uniformly mixed in a mass ratio of 1:0.4:11, the pH value is adjusted to 4 with acetic acid, the mixture is stirred at 60°C and 400 r / min for 3.5 h, and dried at 55°C under vacuum for 9 h to obtain modified amino starch. The remaining steps are the same as those of Example 2.

[0047] Comparative Example 3

[0048] The preparation method of the leak-proof pulp layer paper of Comparative Example 3 is different from that of Example 2 only in that step (3) is not performed, and step (4) is modified as follows: modified amino starch, polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water are mixed uniformly in a mass ratio of 1:0.11:0.015:0.04:0.00025:2.5, and the viscosity is adjusted to 190 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 29g / m 2 , the drying temperature is 110°C; the drying speed is 27.5 m / min; the paper is rolled up; the paper is cut and rewound to obtain the leak-proof pulp layer paper. The remaining steps are the same as those in Example 2.

[0049] Test Example 1

[0050] Flame retardant performance test

[0051] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 1.

[0052] Table 1

[0053]

[0054] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the leakage-proof pulp layer paper prepared by the present invention has good flame retardant properties.

[0055] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that the Si-H bond on 2,4,6,8-tetramethylcyclotetrasiloxane and the carbon-carbon double bond on allyl phosphoric acid undergo a silylation reaction to prepare a phosphorus-silicon synergistic flame retardant; amino starch is reacted with an excess of the phosphorus-silicon synergistic flame retardant to prepare a modified amino starch, and the amino group on the amino starch reacts with the phosphate group on the phosphorus-silicon synergistic flame retardant to form a phosphoramide bond, and at the same time, siloxane and phosphorus are introduced into the modified amino starch, and the phosphorus element can capture free radicals and promote the formation of a carbon layer to isolate heat and oxygen, thereby giving the leak-proof pulp layer paper excellent flame retardant properties; the layered SiO2 formed by the degradation of siloxane during combustion migrates to the surface of the carbon layer, making the carbon layer denser, inhibiting the oxidation of the carbon layer, enhancing the stability of the carbon layer at high temperatures, and further improving the flame retardant properties of the leak-proof pulp layer paper.

[0056] Test Example 2

[0057] Ionic conductivity test

[0058] Test method: The ionic conductivity of the embodiments and comparative examples was tested by AC impedance method. The pulp paper was cut into circular samples with a diameter of 18 mm. The positive and negative pole pieces were replaced with stainless steel to assemble into a blocked type battery (stainless steel sheet / pulp paper / stainless steel sheet). The bulk impedance at 40°C was tested by an electrochemical workstation. The ionic conductivity was calculated according to the formula: ionic conductivity = pulp paper thickness / (bulk resistance × effective contact area) ×%. The results are shown in Table 2.

[0059] Table 2

[0060]

[0061] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the leakage-proof pulp layer paper prepared by the present invention has good ion conductivity.

[0062] By comparison, the ionic conductivity of Examples 1 to 3 is greater than that of Comparative Example 3, indicating that 4-vinylpyridine is reacted with 1,6-dichlorohexane to obtain vinyl pyridinium salt; polyvinyl alcohol is reacted with vinyl pyridinium salt to obtain modified polyvinyl alcohol, and pyridinium salt is introduced into the side chain of polyvinyl alcohol. The introduction of pyridinium salt can further improve the ionic conductivity of the anti-leakage pulp layer paper.

[0063] Test Example 3

[0064] Leakage resistance test

[0065] Test method: Using the examples and comparative examples as pulp paper for carbon batteries, zinc-manganese batteries were assembled according to GB8897-2008-T, and the leakage resistance of the batteries was tested. The results are shown in Table 3.

[0066] Table 3

[0067]

[0068] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 3, it can be found that the leakage-proof pulp layer paper prepared by the present invention has good liquid leakage resistance.

[0069] By comparison, there is no leakage in Examples 1 to 3, while only in Comparative Example 1 there is leakage, which indicates that 8-hydroxyquinoline is loaded into diatomite to obtain modified diatomite; dopamine hydrochloride is polymerized and deposited on the surface of modified diatomite to obtain polydopamine-coated modified diatomite; during the use, storage or intermittent discharge of the carbon battery, the zinc cylinder as the negative electrode comes into contact with the acidic substance in the electrolyte and is corroded, causing the battery capacity to decrease and swell, and the zinc cylinder becomes thinner, resulting in leakage, thereby corroding the electrical equipment; diatomite is an inorganic porous material with rich pore structure, heat resistance and corrosion resistance. 8-Hydroxyquinoline is a metal corrosion inhibitor that can complex with metal ions and be adsorbed on the metal surface to form a protective layer to inhibit corrosion of the metal surface; 8-Hydroxyquinoline is loaded into the pores of diatomaceous earth to obtain modified diatomaceous earth, and then dopamine hydrochloride is polymerized and coated on the surface of the modified diatomaceous earth to obtain polydopamine-coated modified diatomaceous earth. The polydopamine on the polydopamine-coated modified diatomaceous earth will be gradually decomposed in an acidic electrolyte to release the corrosion inhibitor 8-hydroxyquinoline, thereby achieving the purpose of long-term corrosion inhibition of the negative electrode of the zinc-manganese battery and preventing the negative electrode of the battery from being corroded and causing electrolyte leakage.

[0070] Test Example 4

[0071] Tensile strength test

[0072] Test method: The examples and comparative examples were cut into dumbbell-shaped specimens with a length of 6 mm and a width of 4 mm, and stretched using an electronic universal testing machine at 30°C and a stretching rate of 5 mm / min to test the tensile strength of the specimens. The results are shown in Table 4.

[0073] Table 4

[0074]

[0075] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 4, it can be found that the leakage-proof pulp layer paper prepared by the present invention has good tensile strength.

[0076] By comparison, the tensile strengths of Examples 1 to 3 are greater than those of Comparative Examples 1 and 3, indicating that 8-hydroxyquinoline is loaded into diatomite to obtain modified diatomite; dopamine hydrochloride is polymerized and deposited on the surface of the modified diatomite to obtain polydopamine-coated modified diatomite, and amino groups are introduced into the polydopamine-coated modified diatomite; 4-vinylpyridine is reacted with 1,6-dichlorohexane to obtain vinylpyridinium salt; polyvinyl alcohol is reacted with vinylpyridinium salt to obtain modified polyvinyl alcohol, and chlorine atoms are introduced into the side chains of polyvinyl alcohol. The chloride ions introduced into the side chains of polyvinyl alcohol can react with the amino groups on the polydopamine-coated modified diatomite to form a cross-linked network, thereby inhibiting the relative slippage of the molecular chains and giving the leakage-proof pulp layer paper excellent tensile strength.

[0077] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Examples 2 to 3, indicating that the Si-H bond on 2,4,6,8-tetramethylcyclotetrasiloxane and the carbon-carbon double bond on allyl phosphoric acid are subjected to a silylation reaction to obtain a phosphorus-silicon synergistic flame retardant; amino starch is reacted with an excess of the phosphorus-silicon synergistic flame retardant to obtain modified amino starch, and the amino group on the amino starch reacts with the phosphate group on the phosphorus-silicon synergistic flame retardant to form a phosphoramide bond, and at the same time, a phosphate group is introduced into the modified amino starch; 4-vinylpyridine is reacted with 1,6-dichlorohexane to obtain vinyl pyridinium salt; polyvinyl alcohol is reacted with vinyl pyridinium salt to obtain modified polyvinyl alcohol, and pyridinium salt is introduced into the side chain of polyvinyl alcohol, and the pyridinium salt can be combined with the phosphate group on the modified amino starch through positive and negative charges to form a cross-linked network, thereby inhibiting the relative slip of the molecular chain and further improving the tensile strength of the leakage-proof pulp layer paper.

[0078] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing leak-proof pulp layer paper, characterized in that: The preparation method of the leakage-proof pulp layer paper comprises the following steps: polymerizing and depositing dopamine hydrochloride on the surface of modified diatomaceous earth to obtain polydopamine-coated modified diatomaceous earth; reacting starch with 3-aminopropyltriethoxysilane to obtain amino starch; reacting amino starch with a phosphorus-silicon synergistic flame retardant to obtain modified amino starch; preparing a mixed slurry with modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide and deionized water, coating the mixed slurry on a base paper, drying, slitting and rewinding the paper to obtain the leakage-proof pulp layer paper; The modified diatomaceous earth is prepared by loading 8-hydroxyquinoline into diatomaceous earth; The phosphorus-silicon synergistic flame retardant is prepared by reacting 2,4,6,8-tetramethylcyclotetrasiloxane with allyl phosphoric acid; The preparation method of the modified polyvinyl alcohol comprises the following steps: uniformly mixing ammonium cerium nitrate and deionized water at a mass ratio of 1:(6-8) to prepare an ammonium cerium nitrate solution; uniformly mixing polyvinyl alcohol, vinyl pyridinium salt and deionized water at a mass ratio of 1:(1.5-1.7):(10-12), adjusting the pH value to 5.8-6.0 with a nitric acid aqueous solution with a molar concentration of 1 mol / L, uniformly dropping the ammonium cerium nitrate solution with a mass of 3-4 times that of the polyvinyl alcohol within 20 minutes, stirring and reacting at 40-42° C. and 300-500 r / min for 4-6 hours, and drying at 40-50° C. under vacuum conditions for 8-10 hours to obtain the modified polyvinyl alcohol; The preparation method of the vinyl pyridine salt is as follows: under a nitrogen atmosphere, 4-vinyl pyridine and 1,6-dichlorohexane are added to dichloromethane with a molar ratio of 1:1, the mixture is stirred at 30-40° C. and 300-500 r / min for 6-8 hours, and the mixture is dried at 50-60° C. for 8-10 hours under vacuum conditions to obtain the vinyl pyridine salt; In the mixed slurry, the mass ratio of modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water is 1:(0.1-0.12):(0.01-0.02):(0.03-0.05):(0.0002-0.0003):(2-3); The base paper is Xueshan brand battery base paper with a thickness of 80 microns.

2. The method for preparing leakage-proof pulp layer paper according to claim 1, characterized in that: The number average molecular weight of the polyvinyl alcohol is 80,000 to 100,000.

3. The method for preparing leakage-proof pulp layer paper according to claim 1, characterized in that: The method comprises the following preparation steps: (1) Modified diatomaceous earth, dopamine hydrochloride and deionized water are mixed uniformly in a mass ratio of 1:(2-3):(50-60), stirred at 10-30°C and 300-500 r / min for 10-20 min, tris(hydroxymethyl)aminomethane (0.04-0.06 times the mass of dopamine hydrochloride) is added, stirred at 30-40°C and 300-500 r / min for 18-20 h, centrifuged, washed with deionized water for 3-5 times, and dried at 50-60°C under vacuum conditions for 8-10 h to obtain polydopamine-coated modified diatomaceous earth; (2) Mix starch, 3-aminopropyltriethoxysilane, and 10-20% ethanol aqueous solution in a mass ratio of 1:(0.3-0.5):(10-12), adjust the pH to 4 with acetic acid, stir and react at 55-65°C, 300-500 r / min for 3-4 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain amino starch; mix amino starch, phosphorus silicon synergistic flame retardant, and 4-6% acetic acid aqueous solution in a mass ratio of 1:(1.5-1.7):(10-12), add dicyclohexylcarbodiimide (0.03-0.05 times the mass of amino starch), stir and react at 70-80°C, 300-500 r / min for 2-3 hours, and dry at 50-60°C for 8-10 hours under vacuum conditions to obtain modified amino starch; (3) Mix the modified amino starch, modified polyvinyl alcohol, polyacrylamide, polydopamine-coated modified diatomaceous earth, bismuth oxide, and deionized water evenly, and adjust the viscosity to 180-200 mm with deionized water. 2 / s to obtain a mixed slurry; the mixed slurry is evenly coated on the battery base paper, and the coating amount is 28~30g / m 2 The drying temperature is 100~120℃; the drying speed is 25~30m / min for winding; slitting and rewinding to obtain leakage-proof pulp layer paper.

4. The method for preparing leakage-proof pulp layer paper according to claim 3, characterized in that: The preparation method of the modified diatomite in step (1) is as follows: 8-hydroxyquinoline and anhydrous ethanol are mixed evenly at a mass ratio of 1:(9-11) to prepare an 8-hydroxyquinoline solution; diatomite with a particle size of 10-20 μm and the 8-hydroxyquinoline solution are mixed evenly at a mass ratio of 1:(8-10), ultrasonically dispersed for 2-3 hours, and dried at 50-60° C. for 10-12 hours under vacuum conditions to obtain the modified diatomite.

5. The method for preparing leakage-proof pulp layer paper according to claim 3, characterized in that: The preparation method of the phosphorus-silicon synergistic flame retardant in step (2) is as follows: 2,4,6,8-tetramethylcyclotetrasiloxane and allyl phosphoric acid are added in a molar ratio of 1:4 to toluene with a mass of 12 to 14 times that of 2,4,6,8-tetramethylcyclotetrasiloxane, and then chloroplatinic acid with a mass of 0.03 to 0.05 times that of 2,4,6,8-tetramethylcyclotetrasiloxane is added, and the mixture is stirred at 70 to 80° C. and 300 to 500 r / min for 2 to 3 hours, and dried at 50 to 60° C. under vacuum conditions for 8 to 10 hours to obtain the phosphorus-silicon synergistic flame retardant.

6. The method for preparing leakage-proof pulp layer paper according to claim 3, characterized in that: The amino starch in step (2) has a deacetylation degree of 95% and a weight average molecular weight of 180-200 kDa.

7. The method for preparing leakage-proof pulp layer paper according to claim 3, characterized in that: The degree of polymerization of the polyacrylamide in step (3) is 3000-4000.

8. Use of the leak-proof pulp layer paper prepared by the method for preparing leak-proof pulp layer paper according to any one of claims 1 to 7 in batteries.

Citation Information

Patent Citations

  • Water-based flame-retardant fluorosilicon oil and preparation method thereof

    CN107602861A