An ion-type flexible pressure sensor with wide environmental humidity adaptability
The design of the sensor in low temperature and high humidity environments is solved by using polyvinyl alcohol, LiCl and acetone glycerol dielectric layer, bonding layer of SEBS and PANI in flexible pressure sensors The water loss and freezing problems improve mechanical properties and sensitivity, and achieve high ambient humidity adaptability and stability.
Patent Information
- Application Number
- CN202411115159.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing flexible pressure sensors are prone to water loss, freeze or swelling in low temperature and high humidity environments, resulting in limited applicability and service life. The mechanical properties and sensitivity of the sensor are insufficient, and it is difficult for the packaging layer to effectively diffuse and absorb moisture, affecting the environmental humidity. Adaptability and stability.
An ionized flexible pressure sensor with a sandwich-like structure is used. The dielectric layer is composed of polyvinyl alcohol, LiCl, dispersant and acetone glycerol. A micron-scale raised structure is introduced on the surface of the dielectric layer. The adhesive layer is composed of SEBS and PANI. The electrode layer is a circular annular structure, and the encapsulation layer is a bilayer structure, including hydroxypropyl methyl cellulose and polytetrafluoroethylene film.
It improves the environmental humidity adaptability and stability of the sensor, enhances mechanical flexibility and sensitivity, extends service life, and achieves high biocompatibility and environmental friendliness.
Smart Images

Figure CN118641068B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sensors, and in particular to an ion-type flexible pressure sensor adaptable to a wide range of environmental humidity. Background Art
[0002] In the fields of wearables, human-computer interaction, etc., flexible pressure sensors have attracted much attention due to their advantages such as being thin, soft, bendable, highly stretchable, and able to accurately feedback pressure signals. Conductive ion gel has good mechanical properties, excellent biocompatibility and strong self-healing ability, and is an important material for the preparation of flexible pressure sensors. However, since ion gel contains a large amount of water, it is very easy to become brittle and dry in the natural environment, or freeze or swell in low temperature and high humidity environments, which greatly limits the applicability and working life of such sensors.
[0003] Patent application CN117510901A proposes a method for preparing an antifreeze and moisturizing double network organic hydrogel. Polyvinyl alcohol, lipoic acid, sodium phytate, conductive filler and alcohol organic solvent are mixed, and after freeze-thawing treatment, an organic hydrogel with an antifreeze and moisturizing double network is obtained. While solving the antifreeze problem, the conductivity and mechanical properties are also improved.
[0004] Patent application CN116948096A blends methacrylamide, 2-acrylamido-2-methylpropanesulfonic acid and hydroxyethyl methacrylate, and introduces glycerol as a humectant to prepare a double-network conductive hydrogel with strong moisturizing properties, high tensile properties, fast self-healing speed and high conductivity.
[0005] Patent application CN117229530A mixes the deep eutectic solvent prepared by hydrogen bond acceptors and hydrogen bond donors with an alkaline solution, uses nanocellulose as a toughening material and polydopamine as an adhesive component, and obtains a multifunctional conductive hydrogel with self-adhesive, antifreeze and moisturizing properties through a polymerization reaction. It has the advantages of simple operation and low cost.
[0006] Patent application CN116731459A introduces a starch / 1-allyl-3-methylimidazolium chloride / polyvinyl alcohol composite gel system, and through a mixed low eutectic solvent system of ethylene glycol and water, a hydrogel with high electromechanical properties and high moisturizing and antifreeze additional properties is prepared by freeze-thaw cycle.
[0007] Patent application CN117586465A proposes a method for preparing a conductive hydrogel, which mainly polymerizes N-(2-amino-2-oxyethyl) acrylamide, acrylic acid, N,N'-methylenebisacrylamide and sodium chorionate by ultraviolet light curing, and improves the conductivity of the hydrogel by encapsulating silver nanoparticles; further, by introducing glycerol, the hydrogel is endowed with moisturizing properties, and the problem of repeated adhesion and easy detachment faced by hydrogel-based sensors is solved.
[0008] In the academic paper "Ionic conductive hydrogels with long-lasting antifreezing, water retention and self-regeneration abilities" published in the Chemical Engineering Journal, Sui's team used LiCl as an antifreeze agent and poly (sulfobetaine-co-acrylic acid) hydrogel as an electrolyte to prepare a hydrogel with strong hygroscopicity that can still maintain its initial water content after being exposed to ambient temperature for one week.
[0009] In the academic paper "Physically cross-linked silk fibroin-based tough hydrogel electrolyte with exceptional water retention and freezing tolerance" published in the journal ACS Applied Materials & Interfaces, Wang's team designed a flexible fibrous supercapacitor based on SF / EMImAc / H2O / KCl composite electrolyte that can maintain excellent performance after being stored in a low-temperature environment of -50°C for 28 days, solving the problem of short service life of conductive hydrogel due to water loss.
[0010] In the academic paper "A super-toughionic conductive hydrogel with anti-freezing, water retention, and self-regenerated properties for self-powered flexible sensor" published in the journal Applied Materials Today, Tang's team designed a super-tough agarose / P(HEAA-co-AA) / Ca 2+ DN hydrogel and its application in making flexible sensors, Ca 2+The introduction of makes the hydrogel have good antifreeze, water retention and self-regeneration properties.
[0011] In the academic paper "Fabrication of wearable hydrogel sensors with simple ionic-digital conversion and inherent water retention" published in the journal IEEE Sensors Journal, Chen's team used polyacrylamide (PAM) as the matrix and highly absorbent polymer SAP as the water-retaining agent to prepare a hydrogel with excellent water-retention properties, which was then used to prepare flexible sensors.
[0012] In the academic paper "Anti-Freezing and non-drying sensors of ionic hydrogels with double-layer structure for highly sensitive motion monitoring" published in the journal ACS Applied Materials & Interfaces, Zhang's team was inspired by the structure of mussels. In order to solve the problem that traditional hydrogels are difficult to withstand freezing and dehydration environments, they designed a flexible strain-type double-layer hydrogel sensor using sodium p-styrene sulfonate (SSS) and [BMIM]Cl ionic liquids. + The strong interaction between them makes the sensor have a wide temperature range and good antifreeze and moisturizing effects.
[0013] Although some progress has been made in the research of antifreeze and moisture retention of flexible pressure sensors based on ion gel, there are still the following shortcomings:
[0014] 1. Ion gels usually use organic polymer materials that are not easily degradable. The degradation process requires high-temperature treatment or the introduction of chemical reagents such as strong acids and alkalis, and is prone to produce harmful substances that affect the natural environment.
[0015] 2. Alcohol organic solvents, mainly glycerol, are often introduced to improve the moisturizing effect of ion gels. However, polyol solvents, such as glycerol, can only slow down the volatilization rate of water molecules and cannot absorb water from the outside to maintain the stability of the mass of water molecules inside the gel. The introduction of ionic salts with strong hygroscopicity can also effectively improve the moisturizing properties of the gel. However, in order to ensure excellent moisture absorption, the concentration of ionic salts is often increased, resulting in deterioration of the mechanical properties of the sensor. At present, there is a small amount of work that combines moisturizing solvents with strongly hygroscopic ionic salts, so that ion gels have both high moisturizing effects and strong moisture absorption capacity, thereby making such sensors have better durability.
[0016] 3. The capacitive flexible pressure sensor based on ion gel has low sensitivity. Generally, a single microstructure including cylinder, cone and pyramid is introduced on the surface of the dielectric layer. Although the sensitivity is improved, it is difficult to be compatible with high sensitivity and wide linear working range.
[0017] 4. Flexible pressure sensors based on capacitive sensing mechanisms often use electrodes with consistent geometric dimensions. However, during the sensor preparation process, high alignment requirements affect the consistency and stability of the sensor. At the same time, during long-term use, there may be structural slippage between the sensor electrodes, changing the zero-point characteristics of the sensor and its input-output relationship. In addition, the lack of an effective adhesive between the electrode and the dielectric material makes it easy for the sensor electrode and the dielectric layer to loosen or fall off, resulting in limited reliability and durability of the sensor.
[0018] 5. The packaging layer of the flexible pressure sensor generally uses a polymer film that isolates water vapor, and a dense polymer adhesive is introduced between the packaging layer and the electrode. This will make it difficult for the ion gel to effectively diffuse and adsorb water molecules, thereby reducing its moisturizing and moisture absorption effects, and affecting the environmental humidity adaptability and stability of the sensor. Summary of the invention
[0019] In view of the shortcomings of the prior art, the present invention proposes an ion-type flexible pressure sensor with wide environmental humidity adaptability, aiming to effectively improve the environmental humidity adaptability and the stability of static and dynamic performance of such flexible pressure sensor.
[0020] To achieve the purpose, the present invention adopts the following technical solution:
[0021] The present invention first discloses an ion-type flexible pressure sensor that can adapt to a wide range of environmental humidity. The ion-type flexible pressure sensor is a sandwich-like structure as a whole, with an ion gel dielectric layer as the central layer, and an adhesive layer, a flexible electrode layer, an inner flexible packaging layer and an outer flexible packaging layer are symmetrically arranged on the upper and lower surfaces of the ion gel dielectric layer.
[0022] Furthermore, the ion gel dielectric layer is obtained by dissolving polyvinyl alcohol (PVA), LiCl, a dispersant and acetone glycerol in deionized water and then solidifying. The dispersant is one of sodium carboxymethyl cellulose, sodium dodecyl sulfate and octylphenol polyoxyethylene ether. Furthermore, in the ion gel dielectric layer, polyvinyl alcohol, LiCl, a dispersant and acetone glycerol are composed of LiCl 15% to 30%, acetone glycerol 5% to 15%, a dispersant 0.8% to 1.2%, and the remainder is PVA. Acetone glycerol is a diketone compound, which contains only a single hydroxyl group (—OH) in the molecule. Compared with traditional moisturizing solvents such as glycerol, it has fewer binding sites for hydrogen ions in water supply molecules. Based on density functional theory, the calculation and analysis of the binding energy change curves of acetone glycerol-water composite system and glycerol-water composite system effectively explained the reason why acetone glycerol can absorb less water from the outside under low temperature and high humidity environment and retain more water inside the mixed solution under high temperature and low humidity environment. Therefore, the internal mass of the gel can always be kept constant for different external environments, slowing down the water loss rate of the gel and improving the moisture retention of the gel to a certain extent. By introducing LiCl, the number of positive and negative ions that can move freely in the composite material increases, and the ion mobility in the composite system increases. Based on the double-layer capacitance theory, the sensitivity of the sensor is effectively improved; in addition, LiCl ionizes in aqueous solution to produce Li + Compared with the monovalent positive ions produced by ionization of the same main group elements, they have the highest ionic potential. They produce the strongest hydrogen bonding effect by combining with the PVA chain, and change the arrangement of water molecules in the internal system of the gel, further enhancing the water exchange with the air, so that the gel has both strong water locking and high hygroscopicity, maintaining the mass of water molecules in the ion gel in dynamic balance, and improving the stability and service life of the sensor.
[0023] Furthermore, the ion gel dielectric layer is formed on the upper surface of a planar layer with multiple micron-scale protrusion structures arranged in an array, each protrusion structure is composed of multiple elliptical protrusions, one end of the long axis of the multiple elliptical protrusions converges to a point to form a base point, and the other end is diffusely distributed, and adjacent elliptical protrusions overlap in a section near the base point. Further: in the multiple micron-scale protrusion structures arranged in an array, the spacing between adjacent protrusion structures does not exceed 7μm; the long axis chord length of each elliptical protrusion in the same protrusion structure does not exceed 12μm, and the short axis chord length does not exceed 8μm. In the multiple micron-scale protrusion structures arranged in an array, the protrusion heights of the protrusion structures in the same row are the same, and the protrusion heights of the protrusion structures in different rows show a trend of decreasing from the middle row to the two side rows with a height difference of 1~3μm, and the highest height does not exceed the long axis chord length of each elliptical protrusion. The number of elliptical protrusions that make up a protrusion structure is 3 to 6. By introducing a surface structure composed of multiple elliptical protrusions, the surface morphology of the dielectric layer can be changed compared to the traditional flat surface, and the effective surface area of the dielectric layer can be increased, thereby improving the sensitivity of the sensor. Compared with the single structure, the gradient difference structure has a higher pressure sensing range, a larger normalized contact area and capacitance change, and reduces the non-uniformity and cross-interference of the electric field inside the dielectric layer, making the sensor have both high sensitivity and high linearity.
[0024] Furthermore, the total thickness of the ion gel dielectric layer is 150-300 μm, the tensile strength is 10-30 MPa, the elongation at break is not less than 60%, and the ionic conductivity is not more than 2×10 -2 S / cm.
[0025] Furthermore, the bonding layer is formed by printing a conductive ink composed of an organic high molecular weight elastomeric polymer, a conductive polymer, a plasticizer and an initiator on the upper and lower surfaces of the ion gel dielectric layer. In the bonding layer, the organic high molecular weight elastomeric polymer, the conductive polymer, the plasticizer and the initiator are composed of 14% to 18% conductive polymer, 0.8% to 1.3% plasticizer, 0.3% to 0.5% initiator, and the balance is an organic high molecular weight elastomeric polymer. Furthermore, the organic high molecular weight elastomeric polymer is a styrene-butadiene block copolymer (SEBS), the conductive polymer is polyaniline (PANI), the plasticizer is sodium octanoate, and the initiator is ammonium persulfate. The SEBS is dissolved using 1,2-dichloroethane, the polyaniline is dissolved using N,N-dimethylformamide (DMF), and the sodium octanoate and ammonium persulfate are dissolved using deionized water. The difference in flexibility between the polystyrene and ethylene-butylene blocks in the SEBS molecule makes SEBS highly elastic as a whole and able to withstand a wide range of stretching; in addition, SEBS has a strong oxidation induction period, and the internal saturated carbon-carbon bond structure increases the time for the oxidation reaction to occur, making SEBS have certain heat resistance and aging resistance, which improves the service life of the sensor; the internal structure of SEBS contains different polymer blocks, which makes the dielectric layer and the electrode have good adhesion, effectively improving the interface bonding ability between the two. The unique molecular structure of PANI makes it easy to undergo conformational changes under the action of an electric field, and to transform between different oxidation states, which is beneficial to the transmission of electrons on the molecular chain, so that the adhesive layer also has a certain high conductivity, further promoting ion transmission.
[0026] Furthermore, the thickness of the bonding layer is 40 μm to 60 μm, the elongation at break is not less than 50%, the shear strength is 2 to 6.6 MPa, and the electrical conductivity is 2500 S / cm to 7500 S / cm.
[0027] Furthermore, the flexible electrode layer is in a circular ring structure, and a plurality of circular holes extending vertically through the ring are provided in the ring. The flexible electrode layer may be made of copper foil or the like. The two circular ring-shaped flexible electrode layers located on the upper and lower sides of the ion gel dielectric layer have different sizes. The outer ring diameter of the large circular ring structure matches the sensor size, and the ring width is 5 to 40 mm. The outer ring radius of the small circular ring structure is 0.5 to 1.5 mm smaller than that of the large circular ring structure, and the ring width is 0.5 to 1.5 mm smaller; the number of circular holes in the two circular ring structures is not less than 100 / cm 2 The use of an annular electrode with inconsistent upper and lower areas and an asymmetric structure can effectively reduce the impact of structural slip on the stability of the output signal during use based on the area difference between the two. The large number of micropores on the surface of the annular ring effectively block liquid water and allow water vapor to pass through, promoting the exchange of water between the dielectric layer and the air, making the sensor have an excellent long-term moisturizing effect.
[0028] Furthermore, the material of the inner flexible packaging layer is hydroxypropyl methylcellulose, and the outer flexible packaging layer is a polytetrafluoroethylene film. The inner flexible packaging layer in contact with the electrode and the outer flexible packaging layer in contact with the air environment constitute a double-layer flexible packaging layer. Furthermore: the thickness of the inner flexible packaging layer is 30-45 μm, the particle size of the hydroxypropyl methylcellulose raw material is 300-400 mesh, and the viscosity is not less than 80000 mPa / s; the thickness of the polytetrafluoroethylene film used in the outer flexible packaging layer is 100-120 μm, and the number of micropores is not less than 8000 / cm 2 , the pore size is 80~140nm. The surface of the polytetrafluoroethylene film has a large number of microporous structures, which has good air permeability and can allow air to pass through while effectively blocking the liquid, avoiding damage to the sensor caused by direct contact between water vapor in the air and the electrode. In addition, the excellent heat resistance and stability of the polytetrafluoroethylene film itself can also effectively insulate and prevent the sensor from being affected by the external environment. The filamentous structure inside the hydroxypropyl methylcellulose has strong spatial cross-linking. The hydrogen bonding formed by a large number of hydroxyl groups (—OH) and methoxy groups (—OCH3) makes cellulose have good adhesion, thickening and anti-permeability, and can form an excellent adhesion effect with the outer packaging layer and the electrode, and can improve the high temperature resistance to a certain extent; cellulose can form a uniform and flexible film. As a natural biomatrix material, it has excellent environmental sustainability.
[0029] The present invention further provides a method for preparing the ion-type flexible pressure sensor with wide environmental humidity adaptability, comprising the following steps:
[0030] Step 1: Preparation of ion gel dielectric layer
[0031] First, polyvinyl alcohol is dissolved in deionized water, and then LiCl, a dispersant and glycerol acetone are added and heated and stirred until the whole is in a uniformly mixed viscous state to obtain a flexible ion gel material; then the flexible ion gel material is cast into a mold, cured, and demolded to form an ion gel dielectric layer.
[0032] Step 2: Prepare the bonding layer
[0033] An organic high molecular weight elastomeric polymer, a conductive polymer, a plasticizer and an initiator are stirred and mixed uniformly in a solvent to obtain a bonding layer material; the bonding layer material is pre-cured into a viscous state to obtain a conductive ink; and then the conductive ink is printed on the upper and lower surfaces of the ion gel dielectric layer respectively through a screen printing process to form a bonding layer.
[0034] Furthermore, an adhesive layer is introduced into the ion gel dielectric layer and the electrode, and a screen printing process is used for uniform coating. After the adhesive layer material is processed into an ink-like state, the number of times of application with a scraper is no more than 8 times, and the thickness of the ink applied to the screen printing plate in a single time is 5-7.5μm. By adjusting the printing parameters, the thickness of the ink passing through the mesh to the ion gel dielectric layer can be precisely controlled, which improves the consistency and repeatability of the sensor.
[0035] Step 3: Prepare flexible electrode layer
[0036] The metal is cut into two required annular structures, and then the two annular structures are respectively adhered to the adhesive layers on the upper and lower surfaces of the ion gel dielectric layer to form two flexible electrode layers.
[0037] Furthermore, the metal is cut by laser cutting. The structural characteristic parameters of the two circular ring structures and the characteristic parameters of the aperture are set, the parameters are imported into the laser cutting machine, and the cutting power, cutting speed, focal length and other parameters of the laser cutting machine are adjusted. After the laser cutting is completed, the copper foil surface is cleaned with anhydrous ethanol.
[0038] Step 4: Prepare flexible packaging layer
[0039] After dissolving the hydroxymethylpropyl cellulose powder, it is evenly coated on the surfaces of the two flexible electrode layers to form two inner flexible packaging layers. Then, polytetrafluoroethylene films are adhered to the two inner flexible packaging layers and pressure-sealed to complete the production of the ion-type flexible pressure sensor.
[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0041] 1. The organic polymer materials used in the flexible pressure sensor of the present invention, such as PVA, SEBS, polytetrafluoroethylene, hydroxypropyl methylcellulose, etc., can be naturally degraded or simply green-degraded. The inorganic ion salt LiCl used is non-toxic and harmless to the human body. The solvents used, such as acetone glycerol, 1,2-dichloroethane, and DMF, can naturally volatilize in a high temperature environment above 100°C, and will not cause gas pollution to the environment. They are non-toxic and harmless to the human body and have good biocompatibility and environmental friendliness. The mechanical flexibility of the ion gel is improved through the strong hydrogen bonding between the PVA chain and the lithium ion.
[0042] 2. The present invention introduces acetone acetal and LiCl salt into the ion gel dielectric layer. Based on the slow water loss rate and excellent moisture retention of acetone acetal, the face-centered cubic regular stacking mode inside the LiCl molecular crystal and the large number of binding sites for the adsorption of water molecules in the air form a strong water absorption and water locking effect. Based on the excellent strong water locking and high hygroscopicity of LiCl molecules, the dynamic balance of the water molecule content in the ion gel is effectively maintained, so that the sensor has high environmental humidity adaptability and stability.
[0043] 3. The present invention adopts a casting process and a mold forming method to introduce a micron-sized protrusion structure with different heights on the surface of the ion gel dielectric layer, thereby increasing the effective surface area of the dielectric layer. Compared with a single structure, it has a higher pressure sensing range, a larger normalized contact area and capacitance change, and reduces the non-uniformity of the electric field inside the dielectric layer, so that the sensor has both high sensitivity and a wide linear working range.
[0044] 4. The present invention sets a bonding layer based on SEBS molecules between the ion gel dielectric layer and the electrode. The multi-segment copolymer structure of olefin blocks and styrene blocks alternately arranged inside SEBS and the difference in hydrophilicity make it have a strong interface adsorption effect. Therefore, the ion gel dielectric layer and the electrode have good interface adhesion, which improves the consistency and stability of the sensor.
[0045] 5. The present invention uses an annular electrode with different upper and lower geometric dimensions as a signal electrode. Based on the size difference between the upper and lower annular rings, the influence of structural alignment or slip on the sensor output signal is weakened, so that the sensor has both high consistency and stability, and has good anti-shielding ability. A circular hole structure is designed in the middle part of the annular electrode to enhance the water exchange capacity between the ion gel dielectric layer and the air.
[0046] 6. The encapsulation layer of the present invention is a double-layer structure, the outer encapsulation layer in contact with the air environment is a polytetrafluoroethylene film, and the inner encapsulation layer in contact with the electrode is made of hydroxypropyl methylcellulose. The large number of micropores on the surface of the polytetrafluoroethylene film allows the outer encapsulation layer to have good air permeability while effectively isolating the liquid in the external environment. The spatial network structure inside the hydroxypropyl methylcellulose can promote the permeation of water vapor through the mesh, and enhance the surface adhesion through the strong hydrogen bonding between the hydroxyl groups and methoxy groups inside the cellulose molecules and the electrodes, so that the inner encapsulation layer has excellent adhesion to the outer encapsulation layer and the electrodes, thereby improving the high environmental humidity adaptability and stability of the sensor.
[0047] 7. The ion-type flexible pressure sensor prepared by the present invention has good adaptability to environmental humidity, and has the characteristics of high sensitivity, high linearity, and excellent biocompatibility and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is an overall structural diagram of an ion-type flexible pressure sensor with wide environmental humidity adaptability provided by the present invention.
[0049] Figure 2 This is a top view of a flexible electrode layer manufactured in an embodiment of the present invention, which illustrates different sizes of a flexible upper electrode and a flexible lower electrode.
[0050] Figure 3 Schematic diagram of the chemical reaction synthesis of acetone glycerol acetal.
[0051] Figure 4 This is the binding energy change curve of glycerol acetone acetal-water and glycerol-water composite systems.
[0052] Figure 5 Schematic diagram of the interaction between PVA and LiCl.
[0053] Figure 6 Schematic diagram of the unit cell structure of LiCl.
[0054] Figure 7 The effect of LiCl concentration on the hygroscopic properties of ion gel.
[0055] Figure 8 Schematic diagram of the sunflower structure inspired by the imitation chicken feet of reed catkins and the schematic diagram of the mold for making the ion gel dielectric layer obtained thereby.
[0056] Fig. 9 Stress-strain curves of SEBS / PANI at different PANI concentrations.
[0057] Fig.10 The current-voltage relationship curve of SEBS / PANI at different PANI concentrations.
[0058] Fig.11 The weight change rate curve of the ion-type flexible pressure sensor manufactured in an embodiment of the present invention under different humidity environments.
[0059] Fig.12 The stress-capacitance change rate curve of the ion-type flexible pressure sensor manufactured in the embodiment of the present invention under the stress range of 200KPa.
[0060] Fig.13 The frequency characteristic curves of the ion-type flexible pressure sensor manufactured in the embodiment of the present invention at different frequencies.
[0061] Fig.14 This is a repetitive characteristic curve of the ion-type flexible pressure sensor manufactured in an embodiment of the present invention. DETAILED DESCRIPTION
[0062] The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0063] The PVA used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (1797 type, alcoholysis degree 98.0-99.0 mol%, Mw-195000).
[0064] The LiCl used in the following examples was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (AR, 99%).
[0065] The glycerol acetone acetal used in the following examples was purchased from Guangzhou Xuxiang Chemical Co., Ltd. (AR, 99%).
[0066] The sodium dodecyl sulfate used in the following examples was purchased from China National Pharmaceutical Group Chemical Reagent Co., Ltd. (chemically pure, CP).
[0067] The SEBS used in the following examples was purchased from Shanghai Juyi Plastic Material Technology Co., Ltd. (G1650 powder).
[0068] The PANI used in the following examples was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (AR, 98%).
[0069] Sodium octanoate used in the following examples was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd. (AR, 99%).
[0070] The ammonium persulfate used in the following examples was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (AR, 98%).
[0071] The 1,2-dichloroethane used in the following examples was purchased from China National Pharmaceutical Group Chemical Reagent Co., Ltd. (AR, 99.5%).
[0072] The DMF used in the following examples was purchased from China National Pharmaceutical Group Chemical Reagent Co., Ltd. (AR, 99.5%).
[0073] The anhydrous ethanol used in the following examples was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. (AR, 99.5%).
[0074] The polytetrafluoroethylene films used in the following examples were purchased from Shenzhen Changlongxin Plastic Materials Co., Ltd. (100 μm thickness).
[0075] The hydroxypropyl methylcellulose used in the following examples was purchased from Hebei Zhicheng Cellulose Co., Ltd. (viscosity 100000 mPa / s).
[0076] Example 1
[0077] like Figure 1 As shown, the ion gel flexible pressure sensor with wide environmental humidity adaptability provided in this embodiment is a sandwich-like structure as a whole, with an ion gel dielectric layer 1 as the central layer, and an adhesive layer 2, a flexible electrode layer 3, an inner flexible packaging layer 4 and an outer flexible packaging layer 5 are symmetrically arranged on the upper and lower surfaces of the ion gel dielectric layer.
[0078] The ion-type flexible pressure sensor with wide environmental humidity adaptability of this embodiment is manufactured according to the following steps:
[0079] Step 1: Preparation of ion gel dielectric layer
[0080] 2 g of PVA was added to a beaker, and 40 mL of deionized water was dripped into it to dissolve it. The solution was magnetically stirred for 3 hours at a high temperature of 150° C. to make the solution clear and transparent, and there were no obvious particles at the bottom of the beaker. 0.46 g of LiCl, 0.22 g of acetone glycerol and 0.03 g of sodium dodecyl sulfate were further added to the solution. The solution was magnetically stirred for 1 hour at 80° C. until the solution was evenly mixed and the whole solution was light white and viscous, thereby obtaining a flexible ion gel material.
[0081] The production mold of the ion gel dielectric layer is drawn using modeling software. The ion gel dielectric layer is formed on the upper surface of a planar layer with multiple micron-sized protrusion structures arranged in an array. The specific shape of the micron-sized protrusion structure is an incomplete sunflower shape inspired by the reed chicken feet. In this embodiment, the protrusion structure is arranged in an array of 5 rows and 4 columns, and each protrusion structure is composed of 4 elliptical protrusions. One end of the long axis of the 4 elliptical protrusions converges to a point to form a base point, and the other end is diffusely distributed, and adjacent elliptical protrusions overlap in a section near the base point. The spacing between adjacent protrusion structures is 6μm; the long axis chord length of each elliptical protrusion in the same protrusion structure is 10μm and the short axis chord length is 6μm. The angle between the long axes of two adjacent elliptical protrusions is 8.5°. Among the multiple raised structures arranged in an array, the raised heights of the raised structures in the same row are the same, and the raised heights of the raised structures in different rows show a trend of decreasing from the middle row to the side rows with a height difference of 2μm. The specific heights of each row are 4μm, 6μm, 8μm, 6μm, and 4μm, respectively. The above mold is printed by photocuring, and the flexible ion gel material is cast into the mold. It is dried and cured in a constant temperature oven at 70°C for 4 hours, and demolded to form an ion gel dielectric layer with a total thickness of 220μm. After testing, the tensile strength of the ion gel dielectric layer obtained in this embodiment is 22.8MPa, the elongation at break is 71.6%, and the ionic conductivity at room temperature is 1.2×10 -2 S / cm.
[0082] Step 2: Prepare the bonding layer
[0083] 4.3 g of SEBS particles were added to a beaker, 30 mL of 1,2-dichloroethane was added to dissolve, and magnetic stirring was performed at 120°C until there were no obvious particles at the bottom of the beaker and the solution was clear and transparent as a whole; 0.94 g of PANI, 0.05 g of sodium octanoate and 0.024 g of ammonium persulfate were added to the solution, 15 mL of DMF was used to dissolve, and 5 mL of deionized water was dropped to promote dissolution, and magnetic stirring was performed at 60°C for 1 hour to obtain a bonding layer material.
[0084] Place the bonding layer material in a 150°C oven and dry it for 1 hour. When the solution is in a non-fluid viscous state, take it out to obtain the required conductive ink. Use the screen printing process to apply the ink to the position above the mesh of the screen printing plate, and place the ion gel dielectric layer obtained in step 1 below the mesh area of the screen printing plate. The thickness of the ink applied to the screen printing plate at a single time is 6μm. Use a scraper to scrape 6 times. After the ink is printed on the surface of the ion gel dielectric layer, dry it at 90°C for 30 minutes. Repeat the above operation on the reverse side of the ion gel dielectric layer to successfully achieve the coating of the bonding layer on the ion gel dielectric layer. The thickness of the bonding layer obtained in this embodiment is 47μm. After testing, the bonding layer has an elongation at break of 72.2%, a shear strength of 5.3MPa, and a conductivity of 4336S / cm.
[0085] Step 3: Prepare flexible electrode layer
[0086] Take a piece of 6cm×6cm×0.1mm copper foil, set the outer ring radius of the upper electrode ring structure to 2.8cm and the inner ring radius to 1.4cm in the laser cutting machine, set the laser cutting machine to perform the first step of cutting the copper foil at a cutting power of 80W, a cutting speed of 20mm / s and a focal length of 125mm; after the cutting is completed, further set the circular hole radius to 0.4μm and the number of cuts to 160 / cm in the laser cutting machine 2 , and the second step of cutting is performed on the surface of the obtained copper foil to obtain a flexible upper electrode with a through circular hole structure. Take another piece of copper foil of the same size, set the outer ring radius of the lower electrode ring structure to 2.75cm and the inner ring radius to 1.3cm in the laser cutting machine, set the laser cutting machine to perform the first step of cutting with the same parameters, and repeat the above second step of cutting process to obtain a flexible lower electrode with a through circular hole structure. After cutting, drip 5mL of anhydrous ethanol on the surface of the two electrode layers to clean the surface, and the electrode can be obtained after drying.
[0087] Step 4: Prepare flexible packaging layer
[0088] Take 8g of hydroxymethyl propyl cellulose powder with a particle size of 350 mesh and a viscosity of 100000mPa / s, dissolve it in 25mL of deionized water, and stir it at 80℃ for 1 hour until the solution is uniform to obtain a hydroxymethyl propyl cellulose solution; take a 100μm thick, surface micropore number of 9200 / cm 2 5 mL of anhydrous ethanol is dropped onto the surface of the polytetrafluoroethylene film with a single pore size of 105 nm to clean the surface, and a pure polytetrafluoroethylene film can be obtained after drying.
[0089] Step 42: Sensor assembly
[0090] Use a coating rod to evenly coat a layer of hydroxymethylpropyl cellulose solution on the surface of the upper flexible electrode layer. After the solution dries, lightly press a layer of polytetrafluoroethylene film on the surface of the hydroxymethylpropyl cellulose for pre-adhesion. Use a press to apply pressure to the two packaging layers until they are fully in contact and bonded to achieve packaging of the upper packaging layer. Repeat the above operation for the lower packaging layer to complete the production of an ion-type flexible pressure sensor that can adapt to a wide range of environmental humidity.
[0091] Figure 2 This is a top view of the flexible electrode layer. The upper and lower electrodes are distributed in a circular ring shape, with a large number of micrometer-level micropores penetrating the electrode layer on the surface. The larger upper flexible electrode has an outer ring radius of 2.8 cm and an inner ring radius of 1.4 cm; the smaller lower flexible electrode has an outer ring radius of 2.75 cm and an inner ring radius of 1.3 cm.
[0092] Figure 3 The figure is a schematic diagram of the chemical reaction synthesis of acetone glycerol acetal. From the perspective of chemical reaction, the reasons why acetone glycerol acetal has stronger moisturizing effect and slow water loss rate compared with the traditional moisturizing solvent glycerol are analyzed. The glycerol molecule contains three hydroxyl groups (-OH) that can form hydrogen bonds. After the acetone glycerol acetal is formed by condensation reaction with acetone, some hydroxyl groups are replaced, so that there is only one hydroxyl group in the acetone glycerol acetal molecule, resulting in a decrease in the number of hydroxyl groups available for hydrogen bonds and a weakening of the strength of hydrogen bonds. Due to the decrease in the binding force of intermolecular interactions and the fact that acetone glycerol acetal has fewer reaction sites available for hydrogen ion binding compared with glycerol molecules, the water loss rate is significantly slowed down. Therefore, acetone glycerol acetal has stronger moisturizing and water evaporation slowing capabilities.
[0093] Figure 4 The binding energy change curves of acetone glycerol acetal-water and glycerol-water composite systems. Based on density functional theory, the change process of the binding energy of the two solvent systems was analyzed by conducting binding energy verification experiments. Under low humidity environment (the number of water molecules that can be bound is less than 2), the binding energy required for the acetone glycerol acetal-water composite system is lower than that of the glycerol-water composite system. Under the same conditions, acetone glycerol acetal needs to absorb more energy to lose internal water molecules, and has a stronger moisturizing effect in low humidity environment; under high temperature environment (the number of water molecules that can be bound is greater than 4), the binding energy required for the glycerol-water composite system is lower than that of the acetone glycerol acetal-water composite system. At this time, glycerol is very easy to bind a large number of water molecules and cause gel swelling. In contrast, acetone glycerol acetal can show different moisturizing effects for different humidity environments to ensure that the gel always has stable characteristics, proving that acetone glycerol acetal has better adaptability to wide humidity environments as a moisturizing solvent.
[0094] Figure 5 and Figure 6 The principle of LiCl's strong hygroscopicity and water-locking properties is explained. Figure 5Schematic diagram of the interaction between PVA and LiCl. In aqueous solution, PVA chains are dispersed. When lithium salt is introduced, a large number of ions generated by ionization move freely and quickly combine with PVA chains. + It forms strong hydrogen bonds with the hydroxyl groups of the PVA chain, absorbs a large number of water molecules at the cross-linking site to form hydrated lithium ions, and while preventing the PVA chain from crystallizing, it quickly converts free water into bonded water with a directional cluster arrangement, effectively reducing the evaporation of water. Figure 6 The schematic diagram of the unit cell structure of LiCl. LiCl is face-centered cubic. + With Cl - Through the regular arrangement of dense packing, there are a large number of pores and adsorption sites inside the crystal for adsorption of H in water molecules. + With OH - , which results in LiCl being able to effectively absorb moisture from the external environment.
[0095] Figure 7 The effect of different concentrations of LiCl on the hygroscopic properties of ion gel was investigated. When preparing the ion gel dielectric layer according to the method in step 1 above, the mass of sodium dodecyl sulfate, glycerol acetone and deionized water was kept unchanged, and the amount of PVA was adjusted to 2.46g, 2.325g, 2.054g, 2.168g, 1.647g and 1.476g respectively, and the total amount of PVA and LiCl was kept at 2.46g to form gel dielectric layers with LiCl mass fractions of 0%, 5%, 15%, 20%, 30% and 40% respectively. The results show that within a certain mass fraction range (≤30%), as the LiCl concentration increases, a large amount of Li + It is fully dispersed in the solution system and can interact with water molecules, and the weight change rate increases accordingly; when the mass fraction of LiCl increases further, the solution concentration becomes higher, and the water molecules interact with Li due to the increased osmotic pressure. + The interaction between them weakens and the weight change rate begins to decrease. Therefore, in order to ensure the optimal moisture absorption effect, the LiCl concentration is selected to be in the range of 15% to 30%.
[0096] Figure 8 The schematic diagram of the incomplete sunflower-shaped structure inspired by the imitation chicken feet and the schematic diagram of the mold for making the ion gel dielectric layer further formed. Inspired by the incomplete sunflower-shaped structure naturally formed by chicken feet, the effective surface area of the dielectric layer is increased by introducing irregular protrusions at the micro-nano level, thereby improving the sensitivity and response ability of the sensor.
[0097] Fig. 9 and Fig.10The mechanical properties and electrical properties of the sensor obtained when the bonding layer contains different concentrations of PANI. When preparing the bonding layer according to the method of step 2 above, keep the mass of sodium octanoate, ammonium persulfate, 1,2-dichloroethane and DMF solvent unchanged, and adjust the amount of SEBS to 5.24g, 4.974g, 4.516g and 4.251g respectively, and keep the total mass of SEBS and PANI to 5.24g, so as to form bonding layers with PANI mass fractions of 0%, 5%, 15% and 20% respectively. After the sensor is assembled, the sensor is subjected to mechanical tensile testing by the tensile press ZQ990B, and the sensor is electrically tested by connecting the LCR resistor through a wire, and the obtained mechanical properties and electrical properties are plotted respectively.
[0098] Fig. 9 The stress-strain curves of the sensors obtained when the bonding layer contains different concentrations of PANI are shown. Pure SEBS shows typical strong tensile properties. After combining with PANI, the tensile strength is slightly reduced, but the elongation at break can still be maintained at about 800%. Due to the crystallization of the soft segment and the plastic deformation of the hard segment inside SEBS, the rising point of the self-enhancement effect can be clearly distinguished in the stress-strain curve.
[0099] Fig.10 The current-voltage curves of the sensors obtained when the bonding layer contains different concentrations of PANI are shown. As the PANI concentration increases, the slope of the IV curve increases and the resistance of the composite material decreases due to the increase in the number of conductive paths formed in the SEBS matrix. When the PANI concentration reaches 20%, the composite material is disconnected under a voltage of about 80V due to the generation of a large amount of Joule heat.
[0100] Fig.11 The weight change rate curve of the ion-type flexible pressure sensor provided in this embodiment under different humidity environments. The sensor was placed in a high humidity environment of 80% humidity, a normal environment of 50% humidity, and a low humidity environment of 20% humidity for 72 hours each. The weight of the sensor before and after placement was weighed and the weight change rate was calculated. It can be seen from the curve that the sensor can maintain excellent moisture retention performance in different humidity environments, can quickly adapt to the humidity changes in the external environment, and has excellent adaptability to a wide range of humidity environments.
[0101] Fig.12 The stress-capacitance change rate curve of the ion-type flexible pressure sensor provided in this embodiment under the stress range of 200KPa. The obtained sensor is fixed on the measurement platform, and the stress of 0~200KPa is applied to the sensor by the tension press ZQ990B. The results show that under the wide stress range of 200KPa, the sensor can still have a 0.38KPa -1 High sensitivity and high linearity of 0.996.
[0102] Fig.13 The frequency characteristic curve of the ion-type flexible pressure sensor provided in this embodiment at different frequencies. It can be seen from the curve that the sensor can withstand different loading frequencies and can still maintain a stable capacitance change at a loading frequency of 8 Hz, which is of great significance for monitoring loading signals under medium and low frequency pressure.
[0103] Fig.14 This is the repetitive characteristic curve of the ion-type flexible pressure sensor provided in this embodiment. The prepared sensor was stretched 5000 times and the capacitance change was recorded. It can be seen from the curve that the sensor still has good repeatability even after multiple stretching.
[0104] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An ion-type flexible pressure sensor with wide environmental humidity adaptability, characterized in that: The ion-type flexible pressure sensor has a sandwich-like structure as a whole, with an ion gel dielectric layer as the central layer, and an adhesive layer, a flexible electrode layer, an inner flexible packaging layer and an outer flexible packaging layer are symmetrically arranged on the upper and lower surfaces of the ion gel dielectric layer in sequence; The ion gel dielectric layer is obtained by dissolving polyvinyl alcohol, LiCl, a dispersant and glycerol acetone in deionized water and then solidifying; The bonding layer is formed by printing conductive ink composed of organic high molecular weight elastic polymer, conductive polymer, plasticizer and initiator on the upper and lower surfaces of the ion gel dielectric layer; The flexible electrode layer is in a circular ring structure, and a plurality of circular holes penetrating vertically are arranged in the ring; The material of the inner flexible packaging layer is hydroxypropyl methylcellulose, and the material of the outer flexible packaging layer is polytetrafluoroethylene film; The ion gel dielectric layer is formed on the upper surface of a planar layer with multiple micron-scale protrusion structures arranged in an array, each protrusion structure is composed of multiple elliptical protrusions, one end of the long axis of the multiple elliptical protrusions converges to a point to form a base point, and the other end is diffusely distributed, and adjacent elliptical protrusions overlap in a section close to the base point.
2. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: In the ion gel dielectric layer, polyvinyl alcohol, LiCl, dispersant and glycerol acetone acetal are composed of: LiCl 15%-30%, glycerol acetone acetal 5%-15%, dispersant 0.8%-1.2%, and the balance is PVA.
3. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: In the plurality of micrometer-scale protrusion structures arranged in an array, the spacing between adjacent protrusion structures does not exceed 7 μm; in the same protrusion structure, the major axis chord length of each elliptical protrusion does not exceed 12 μm, and the minor axis chord length does not exceed 8 μm.
4. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: Among the multiple micron-scale protrusion structures arranged in an array, the protrusion structures located in the same row have the same protrusion height, and the protrusion heights of the protrusion structures located in different rows show a trend of decreasing from the middle row to the side rows with a height difference of 1 to 3 μm, and the maximum height does not exceed the long axis chord length of each elliptical protrusion.
5. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1 or 2, characterized in that: The total thickness of the ion gel dielectric layer is 150-300 μm, the tensile strength is 10-30 MPa, the elongation at break is not less than 60%, and the ionic conductivity is not more than 2×10 -2 S / cm.
6. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: In the adhesive layer, the organic high molecular weight elastomeric polymer, the conductive polymer, the plasticizer and the initiator are composed of 14% to 18% conductive polymer, 0.8% to 1.3% plasticizer, 0.3% to 0.5% initiator, and the balance is the organic high molecular weight elastomeric polymer.
7. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1 or 6, characterized in that: The organic high molecular weight elastic polymer is a styrene-butadiene block copolymer, the conductive polymer is polyaniline, the plasticizer is sodium octanoate, and the initiator is ammonium persulfate.
8. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1 or 6, characterized in that: The thickness of the bonding layer is 40 μm to 60 μm, the elongation at break is not less than 50%, the shear strength is 2 to 6.6 MPa, and the electrical conductivity is 2500 S / cm to 7500 S / cm.
9. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: The two circular ring-shaped flexible electrode layers located on the upper and lower sides of the ion gel dielectric layer have different sizes. The outer ring diameter of the large circular ring structure matches the sensor size and the ring width is 5~40mm. The outer ring radius of the small circular ring structure is 0.5~1.5mm smaller than that of the large circular ring structure, and the ring width is 0.5~1.5mm smaller; the number of circular holes in the two circular ring structures is not less than 100 / cm 2 .
10. The ion-type flexible pressure sensor with wide environmental humidity adaptability according to claim 1, characterized in that: The thickness of the inner flexible packaging layer is 30-45 μm, the particle size of the hydroxypropyl methylcellulose raw material is 300-400 mesh, and the viscosity is not less than 80000 mPa / s; the thickness of the polytetrafluoroethylene film used in the outer flexible packaging layer is 100-120 μm, and the number of micropores is not less than 8000 / cm 2 , the pore size is 80~140nm.
11. A method for preparing an ion-type flexible pressure sensor with wide environmental humidity adaptability, used for preparing the ion-type flexible pressure sensor according to any one of claims 1 to 10, characterized in that: The steps include: Step 1: Preparation of ion gel dielectric layer First, polyvinyl alcohol is dissolved in deionized water, and then LiCl, a dispersant and acetone glycerol are added and heated and stirred until the whole is in a uniformly mixed viscous state to obtain a flexible ion gel material; Then, the flexible ion gel material is cast into the mold, cured, and demoulded to form an ion gel dielectric layer; Step 2: Prepare the bonding layer The organic high molecular weight elastic polymer, the conductive polymer, the plasticizer and the initiator are stirred and mixed uniformly in a solvent to obtain a bonding layer material; Pre-curing the bonding layer material into a viscous state to obtain a conductive ink; then printing the conductive ink on the upper and lower surfaces of the ion gel dielectric layer respectively by a screen printing process to form a bonding layer; Step 3: Prepare flexible electrode layer Cutting the metal into two required circular ring structures, and then adhering the two circular ring structures to the adhesive layers on the upper and lower surfaces of the ion gel dielectric layer, respectively, to form two flexible electrode layers; Step 4: Prepare flexible packaging layer After dissolving the hydroxymethylpropyl cellulose powder, it is evenly coated on the surfaces of the two flexible electrode layers to form two inner flexible packaging layers. Then, polytetrafluoroethylene films are adhered to the two inner flexible packaging layers and pressure-sealed to complete the production of the ion-type flexible pressure sensor.
Citation Information
Patent Citations
Starch / ionic liquid / polyvinyl alcohol high-performance composite hydrogel as well as preparation method and application thereof
CN116731459A
Copolymerized dual-network conductive hydrogel as well as preparation method and application thereof
CN116948096A
Self-adhesion anti-freezing moisturizing multifunctional conductive hydrogel as well as preparation method and application thereof
CN117229530A
Anti-freezing moisturizing dual-network organic hydrogel as well as preparation method and application thereof