A radioactive iodine-loaded manganese-based metal organic framework degradable embolic microsphere and its preparation method

By combining radioactive iodine-131 in a manganese-based metal-organic framework and solidifying it into polyurethane microspheres, the problem of poor stability of collagen-polyvinyl alcohol microspheres is solved, achieving more stable radioactive iodine loading and safer thyroid protection, improving It improves the liver magnetic resonance imaging effect and is suitable for non-permanent radioactive embolization treatment.

CN118649277BActive Publication Date: 2024-10-29WEST CHINA HOSPITAL SICHUAN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411154410.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-10-29
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing collagen-polyvinyl alcohol embolization microspheres loaded with iodine 131 have poor stability. After treatment, free iodine-131 is easily produced to damage the thyroid gland, and the magnetic resonance imaging effect is poor.

Method used

A hollow porous manganese-based metal organic framework is used to combine radioactive iodine-131 and solidify it into polyurethane microspheres to form radioactive iodine-loaded manganese-based metal organic framework degradable embolic microspheres, which are polymerized through solvothermal method and self-emulsification. Preparation method, using polydopamine coating method to improve the stability and imaging performance of microspheres.

Benefits of technology

It achieves a more stable loading of radioactive iodine, avoids radiation damage to the thyroid gland caused by radioactive iodine loss, improves the contrast of liver magnetic resonance imaging, is suitable for non-permanent radioactive embolization treatment, and monitors the treatment effect through SPECT imaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118649277B_ABST
    Figure CN118649277B_ABST
Patent Text Reader

Abstract

The present invention discloses a radioactive iodine-loaded manganese-based metal organic framework degradable embolic microsphere and a preparation method thereof, which relates to the technical field of clinical medical embolic therapy. A hollow porous manganese-based metal framework is combined with radioactive iodine-131 to obtain 131 I‑Mn‑MOF, and then 131 I‑Mn‑MOF is solidified onto polyurethane microspheres to obtain embolic microspheres. Not only can it complete tumor treatment and liver nuclear medicine SPECT phenomena, but it can also effectively avoid radiation damage to normal tissues such as the thyroid gland caused by radioactive iodine shedding, making it more suitable for non-permanent radioembolization therapy. It can also effectively improve the contrast of liver magnetic resonance, which helps to use magnetic resonance imaging to detect the effect of liver treatment after embolization therapy, and can also avoid the need for patients to inject gadolinium Gd(III) contrast agents for enhanced magnetic resonance imaging, which may cause the potential risk of nephrogenic systemic fibrosis and gadolinium ion brain deposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of clinical medical embolization therapy, and in particular to a radioactive iodine-loaded manganese-based metal organic framework degradable embolization microsphere and a preparation method thereof. Background Art

[0002] Transarterial radioembolization (TARE) with yttrium-90 has achieved good results in the clinical treatment of liver cancer. However, yttrium-90 microspheres are pure beta rays, which make it difficult to monitor patients in vivo after surgery. Detection can only rely on enhanced magnetic resonance imaging. The glass or resin used as the main material of the microspheres is difficult to degrade in the body and does not support secondary intervening treatment.

[0003] Patent CN202010042088.9 discloses a collagen-polyvinyl alcohol embolic microsphere loaded with iodine 131 and a preparation method thereof. First, collagen-polyvinyl alcohol embolic microspheres are prepared by cross-linking polyvinyl alcohol and type I collagen, and then the collagen-polyvinyl alcohol embolic microspheres are labeled with radioactive iodine 131 to obtain iodine 131-collagen-polyvinyl alcohol embolic microspheres. The prepared embolic microspheres can not only slow down the growth rate of tumors and increase the maximum survival time of patients, but also have the advantages of low specific gravity, easy perfusion, long half-life, and the ability to release gamma rays for imaging monitoring. Expensive activation equipment is not required, which is conducive to reducing costs.

[0004] However, the above patent uses tyrosine on the surface of collagen to label iodine-131. The stability of the radionuclide loaded by this method is poor. Free iodine-131 is easily generated after embolization therapy, causing damage to the thyroid gland. The microspheres as a whole do not improve magnetic resonance imaging. Summary of the invention

[0005] Based on the problem that the currently prepared collagen-polyvinyl alcohol embolic microspheres loaded with iodine-131 have poor stability and are prone to generate free iodine-131 after embolization therapy, which causes damage to the thyroid gland, the object of the present invention is to provide a manganese-based metal organic framework-containing degradable embolic microsphere loaded with radioactive iodine and a preparation method thereof. The microspheres can load radioactive iodine more stably, can not only complete tumor treatment and liver nuclear medicine SPECT imaging, but also can effectively avoid radiation damage to normal tissues such as the thyroid gland caused by the shedding of radioactive iodine, and are more suitable for non-permanent radioembolization therapy.

[0006] The present invention is achieved through the following technical solutions:

[0007] In the first aspect, the present invention provides a method for preparing a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere, which uses a hollow porous manganese-based metal framework combined with radioactive iodine-131 to obtain 131I-Mn-MOF, and then 131 I-Mn-MOF was solidified onto polyurethane microspheres to obtain manganese-based metal-organic framework-degradable embolic microspheres loaded with radioactive iodine.

[0008] The radioactive iodine-loaded manganese-based metal organic framework degradable embolic microspheres prepared by the preparation method of the present invention can load radioactive iodine more stably, not only can complete tumor treatment and liver nuclear medicine SPECT phenomenon, but also can effectively avoid radiation damage to normal tissues such as the thyroid gland caused by the shedding of radioactive iodine, and are more suitable for non-permanent radioembolic treatment. In addition, the manganese-based Mn (II) contained in the prepared microspheres can effectively improve the contrast of liver magnetic resonance, which is helpful for using magnetic resonance imaging to detect the liver treatment effect after embolization treatment, and can also avoid the need for patients to inject gadolinium Gd (III) contrast agents for enhanced magnetic resonance imaging, which may cause the potential risk of nephrogenic systemic fibrosis and gadolinium ion brain deposition.

[0009] Furthermore, the preparation method of the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres comprises the following steps:

[0010] Solid manganese-based metal organic frameworks were first synthesized by solvothermal method using MnCl2•4H2O, polyvinyl pyrrolidone, dimethylimidazole and 1,3,5-trimethylbenzene carboxylic acid, and then hollow porous manganese-based metal frameworks were obtained by heat treatment;

[0011] The polyurethane microspheres were prepared by self-emulsifying dispersion polymerization.

[0012] First, a hollow porous manganese-based metal framework is used to stably bind radioactive iodine-131, and then the polydopamine encapsulation method is used to encapsulate the radioactive iodine-131. 131 I-Mn-MOF was solidified onto polyurethane microspheres to obtain manganese-based metal-organic framework-degradable embolic microspheres loaded with radioactive iodine.

[0013] Furthermore, the method for preparing the hollow porous manganese-based metal framework comprises the following steps:

[0014] S1-1, dissolve MnCl2•4H2O, polyvinyl pyrrolidone and dimethylimidazole in deionized water to obtain solution A; dissolve 1,3,5-trimethylbenzene carboxylic acid in ethanol to obtain solution B;

[0015] S1-2, mixing solution A and solution B to form a mixture, then transferring the mixture to a reactor for heat preservation and reaction, washing and drying the powder obtained by the reaction to obtain Mn-sMOF;

[0016] S1-3, heat-treating the Mn-sMOF, first heating it up, then keeping it warm, and then cooling it down to obtain a sample;

[0017] S1-4. The sample is added to a deionized water solution of dimethylimidazole for ultrasonic treatment, and then centrifuged to remove non-nanoscale large agglomerates to obtain a hollow porous manganese-based metal framework Mn-HMS-MOF.

[0018] Furthermore, the mass ratio of MnCl2•4H2O, polyvinyl pyrrolidone, dimethylimidazole, and 1,3,5-trimethylbenzene carboxylic acid is 20~50:10~20:5~10:5~10.

[0019] Furthermore, the preparation method of the polyurethane microspheres comprises the following steps:

[0020] S2-1, dissolving isocyanate, polylactic acid and polypropylene glycol in acetonitrile, heating the reaction system to 65°C to 70°C after complete reaction, stirring and reacting to obtain a polyurethane prepolymer;

[0021] S2-2, lowering the temperature of the reaction system to 37-50°C and adding a chain extender;

[0022] S2-3, adding triethylamine solution as a neutralizing agent to carry out a neutralization reaction;

[0023] S2-4, after the reaction is completed, add distilled water and stir to emulsify;

[0024] S2-5. After centrifugal filtration, monodisperse modified polyurethane microspheres are obtained.

[0025] Among them, the isocyanate includes toluene diisocyanate (TDI) or isocyanate diisocyanate (IPDI).

[0026] Wherein, the polylactic acid is polylactic acid (PLA) with a molecular weight of 2000-4000.

[0027] The polypropylene glycol has a molecular weight of 2500.

[0028] Wherein, the neutralizing agent is 1-2% (wt%) triethylamine (TEA) solution.

[0029] Furthermore, in step S1 of preparing polyurethane microspheres, the content of isocyanate accounts for 40% to 55% of the reaction system, the content of polylactic acid accounts for 8% to 10% of the reaction system, and the content of polypropylene glycol accounts for 3% to 5% of the reaction system.

[0030] Furthermore, the ratio of -NCO to -OH in the chain extender monomer added in step S2 of preparing polyurethane microspheres is 1.5-2.5:1.

[0031] Furthermore, hollow porous manganese-based metal framework and polyurethane microspheres were used to prepare 131 The method of I-Mn-MOF@PU microspheres comprises the following steps:

[0032] S3-1, dispersing and suspending Mn-HMS-MOF in tromethamine solution;

[0033] S3-2, adding dopamine hydrochloride and polyurethane microspheres;

[0034] S3-3. Join 131 I-NaI solution reaction;

[0035] S3-4. After the reaction is completed, the reaction product is collected, centrifuged and the supernatant is discarded;

[0036] S3-5, the precipitated product is washed to obtain 131 I-Mn-MOF@PU microspheres.

[0037] Furthermore, the mass ratio of Mn-HMS-MOF, dopamine hydrochloride, and polyurethane microspheres is 10~100:5~10:100.

[0038] In a second aspect, the present invention provides a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere prepared by any one of the above-mentioned preparation methods.

[0039] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0040] (1) The radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres prepared by the preparation method of the present invention can load radioactive iodine more stably, not only can complete tumor treatment and liver nuclear medicine SPECT phenomenon, but also can effectively avoid radiation damage to normal tissues such as the thyroid gland caused by the shedding of radioactive iodine, and are more suitable for non-permanent radioembolization treatment;

[0041] (2) The manganese-based Mn(II) contained in the radioiodine-loaded manganese-based metal-organic framework-degradable embolic microspheres prepared by the preparation method of the present invention can effectively improve the contrast of liver magnetic resonance imaging, which is helpful for detecting the liver treatment effect using magnetic resonance imaging after embolization therapy, and can also avoid the need for patients to inject gadolinium Gd(III) contrast agent for enhanced magnetic resonance imaging, which may induce the potential risk of nephrogenic systemic fibrosis and gadolinium ion brain deposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0043] Figure 1 The present invention is a flow chart of the preparation process and verification process of a radioactive iodine-loaded manganese-based metal organic framework degradable embolic microsphere;

[0044] Figure 2 The effect verification diagram of the manganese-based metal organic framework prepared in Example 1 of the present invention, wherein A is an energy dispersion spectrum diagram; B is an X-ray photoelectron spectrum diagram; C is a scanning electron microscope display diagram;

[0045] Figure 3 This is a graph showing the hemolysis test results of the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres prepared in Example 1 of the present invention;

[0046] Figure 4 This is a graph showing the coagulation test results of the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres prepared in Example 1 of the present invention;

[0047] Figure 5 This is a diagram showing the cytotoxicity test results of the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres prepared in Example 1 of the present invention;

[0048] Figure 6 This is a graph showing the results of the detection of the nuclide loading rate of the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres prepared in Example 1 of the present invention;

[0049] Figure 7 This is a graph showing the results of the radionuclide loading rate test of the embolic microspheres prepared in Comparative Example 1 (CN202010042088.9);

[0050] Figure 8 This is a comparison chart of SPECT / CT imaging after embolization with the embolic microspheres prepared in Example 1 and Comparative Example 1 (CN202010042088.9);

[0051] Fig. 9 This is a comparison chart of magnetic resonance imaging of the embolic microspheres prepared in Example 1 and Comparative Example 1 (CN202010042088.9). DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0053] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] Example 1

[0055] This embodiment provides a method for preparing radioactive iodine-loaded manganese-based metal organic framework degradable embolic microspheres, such as Figure 1 As shown, the following steps are included:

[0056] S1. Preparation of Mn-based Metal-Organic Frameworks

[0057] The solid manganese-based metal organic framework (Mn-sMOF) was synthesized by the solvothermal method, and then the hollow porous manganese-based metal framework (Mn-HMS-MOF) was obtained by heat treatment based on the principle of non-uniform shrinkage during heat treatment. The specific steps are:

[0058] S1-1, 35 mg MnCl2•4H2O, 15 mg polyvinyl pyrrolidone, 7 mg dimethyl imidazole were dissolved in 10 mL deionized water to obtain solution A; 8 mg 1,3,5-trimethylbenzene carboxylic acid was dissolved in 10 mL ethanol to obtain solution B;

[0059] S1-2, solution A and solution B were mixed, stirred at room temperature (25°C) for 20 minutes to form a uniform mixture, and then transferred to a high-pressure reactor and kept at 120°C for 10 hours; the powder obtained by the reaction was washed with anhydrous ethanol and dried at 50°C in a vacuum environment for 8 hours;

[0060] S1-3, transferring the dried Mn-sMOF to a tube furnace for heat treatment, heating to 380°C in an air atmosphere, keeping the temperature for 1.5 hours, and obtaining a sample after the tube furnace is cooled naturally;

[0061] S1-4. Add the sample into 10 mL of deionized water solution containing 10 mg of dimethylimidazole and perform ultrasonication for 5 minutes. Use differential centrifugation to remove non-nanoscale large agglomerates to obtain a hollow porous manganese-based metal framework Mn-HMS-MOF for use.

[0062] like Figure 2As shown, it is an effect verification diagram of the hollow porous manganese-based metal framework Mn-HMS-MOF prepared in this embodiment, in which A is an energy dispersion spectrum (EDS mapping), showing the main components in the Mn organic metal framework (scale is 70nm); B is an X-ray photoelectron spectroscopy (XPS), showing the main components in the Mn-MOF@PU microspheres; C is a scanning electron microscope image, showing that the final Mn-MOF@PU particle size is 20-40um, with good monodispersity.

[0063] from Figure 2 It can be seen that the manganese-based metal organic structure prepared in the present invention is used as a drug-carrying framework to stably load radioactive iodine and form a nanoscale three-dimensional 131 Compared with the traditional tyrosine residue radioiodine labeling method, the product produced by I-Mn-MOF has superior in vitro and in vivo stability and safety.

[0064] S2. Preparation of modified polyurethane microspheres

[0065] The polyurethane microspheres were prepared by self-emulsifying dispersion polymerization. The specific steps are as follows:

[0066] S2-1, take 3g of toluene diisocyanate (TDI), add polylactic acid (PLA) with a molecular weight of 3000 and polypropylene glycol with a molecular weight of 2500, and dissolve them in 20mL of acetonitrile, wherein the isocyanate content accounts for about 45% of the reaction system, the polylactic acid content accounts for about 9% of the system, and the polypropylene glycol content accounts for 4% of the reaction system. After ensuring complete dissolution by ultrasound, heat the reaction system to 65°C and stir for 2 hours to obtain a polyurethane prepolymer;

[0067] S2-2, lower the temperature of the reaction system to 40°C, add 1.5 g of trimethylolpropane (TMP), ensure that the ratio of -NCO to -OH in the added monomer is 2:1, and carry out chain extension reaction for 4 hours;

[0068] S2-3, adding 1.5 wt% triethylamine (TEA) solution as a neutralizing agent, and continuing the neutralization reaction for 30 minutes;

[0069] S2-4, after the reaction is completed, add distilled water and stir emulsify at 500 rpm for 4 hours;

[0070] S2-5. Obtain monodisperse modified polyurethane PU microspheres through centrifugation and sieve filtration for later use.

[0071] S3. Preparation 131 I-Mn-MOF@PU microspheres

[0072] The hollow porous manganese-based metal framework was used to stably bind radioactive iodine-131 at room temperature, and then the polydopamine encapsulation method was used to 131I-Mn-MOF is cured to PU microspheres. The specific steps are as follows:

[0073] S3-1. At room temperature (25°C), 50 mg of Mn-HMS-MOF was dispersed and suspended in 40 mL of tromethamine solution (pH = 8);

[0074] S3-2, add 7 mg dopamine hydrochloride and 100 mg polyurethane microspheres;

[0075] S3-3, add 10 mCi in a volume of less than 0.5 mL 131 I-NaI solution, shake at a constant speed for 4 hours;

[0076] S3-4. After the reaction is completed, the reaction product is collected, centrifuged at 3000 rpm or above for 10 minutes, and the supernatant is discarded;

[0077] S3-5, the precipitated product was washed 5 times with saline to obtain 131 I-Mn-MOF@PU microspheres.

[0078] Comparative Example 1

[0079] This comparative example provides a method for preparing collagen-polyvinyl alcohol embolization microspheres loaded with iodine 131, specifically, the microspheres are prepared by the method disclosed in patent CN202010042088.9.

[0080] like Figures 3 to 6 As shown, the method prepared by this embodiment 131 The hemolysis rate, coagulation rate and cytotoxicity of I-Mn-MOF@PU microspheres were tested, and the test results showed that 131 I-Mn-MOF@PU microspheres have a hemolysis rate of <5%, a coagulation rate of <5%, and a cytotoxicity of <5%, and have good biocompatibility. 131 Comparison of the stability of I-Mn-MOF@PU microspheres in vitro. After 16 days, Figure 7 As shown, the radioactive iodine loading rate of the microspheres prepared in Comparative Example 1 (CN202010042088.9) fell below 40%, while the radioactive iodine loading rate of the microspheres prepared by the preparation method of the present invention was still above 60%.

[0081] from Figures 3 to 7It can be seen from the test results that the present invention prepares polylactic acid-modified polyurethane microspheres as the core material of embolic microspheres. Both main materials are medical biomaterials with good biocompatibility and degradability. A certain proportion of polylactic acid is introduced into polyurethane. With the sensitivity of the ester bond of polylactic acid to chemical hydrolysis and enzymatic hydrolysis, the degradation cycle of polyurethane microspheres in the body can be adjusted; the prepared microspheres have a particle size of 20-40 microns and good monodispersity, and are suitable for intravascular embolization.

[0082] Using the 131 I-Mn-MOF@PU microspheres were administered to rats in vivo. The administration was performed by direct hepatic artery injection in rats with primary liver cancer. The in vivo distribution was monitored by SPECT / CT imaging. The specific steps are as follows:

[0083] (1) Rats were anesthetized with 2.5% isoflurane gas, and the abdominal hair was shaved. After disinfection, the abdomen was opened to expose the internal organs.

[0084] (2) Find the confluence of the common hepatic artery, proper hepatic artery, and gastroduodenal artery at the back of the liver, and use a hemostatic clip to temporarily clamp the common hepatic artery and gastroduodenal artery;

[0085] (3) Injection through the hepatic artery 131 I-Mn-MOF@PU microspheres 1mCi, microsphere mass about 5 mg, after compression hemostasis, the wound was sutured.

[0086] right 131 The drug distribution in vivo and anti-tumor effect of I microspheres were detected.

[0087] (1) On days 1, 3, 7, 14, 21, and 28 after administration, the rats were subjected to magnetic resonance imaging and SPECT-CT imaging to observe the distribution of the drug in the animals and the growth status of the tumor;

[0088] (2) When SPECT / CT imaging is performed, a high-energy collimator is used, the acquisition energy peak is 364keV, the window width is ±17.5%, the matrix is ​​128×128, the 6° dual-probe acquisition, 30 frames are acquired, each frame is 15 s, and the acquisition time for a single bed is about 10 minutes; the CT scanning tube voltage is 100kV, the tube current is 80 mAs, the matrix is ​​512×512, the scanning field of view is 18cm, and the layer thickness is 0.625mm;

[0089] (3) Magnetic resonance imaging (MRI) was performed using OAx T2 Propeller (T2WI scan), with a slice thickness of 2 mm, a slice spacing of 2 mm, a repetition time of 4000-4200 ms, an echo time of 60 ms, a field of view of 100 × 100 mm, a matrix of 256 × 256, a scan time of 119 s, and a bandwidth of 240-250 Hz.

[0090] like Figure 8 As shown, the microspheres prepared by comparative example 1 (CN202010042088.9) showed free radioactivity in the thyroid gland 3, 7, and 14 days after administration. 131 I signal (arrow), and the 131 After 28 days, the radioactive signal of I-Mn-MOF@PU microspheres was still only present in the liver administration area.

[0091] like Fig. 9 As shown, the method prepared by this embodiment 131 After I-Mn-MOF@PU microsphere embolization, the image contrast of the liver area and liver lesions is significantly better than that of comparative example 1 (CN202010042088.9). Among them, the thick arrow indicates the primary lesion, and the small arrow indicates a tiny new lesion.

[0092] The above experiments have confirmed that the radioactive microspheres prepared by the present invention 131 After embolization, I-Mn-MOF@PU can be used with the help of radioactive 131 I can perform nuclear medicine single photon emission computed tomography (SPECT) imaging, and can also use the characteristics of manganese to perform enhanced magnetic resonance imaging of liver tumor foci. Compared with comparative example 1 (CN202010042088.9), SPECT imaging can show that there is no free radioactivity in the thyroid gland. 131 I, better safety; magnetic resonance imaging (B) can show clearer tumor lesions.

[0093] Example 2

[0094] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0095] S1-1. Dissolve 20 mg MnCl2•4H2O, 10 mg polyvinyl pyrrolidone, and 5 mg dimethylimidazole in 10 mL deionized water to obtain solution A; dissolve 5 mg 1,3,5-trimethylbenzenecarboxylic acid in 10 mL ethanol to obtain solution B.

[0096] Example 3

[0097] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0098] S1-1. Dissolve 50 mg MnCl2•4H2O, 20 mg polyvinyl pyrrolidone, and 10 mg dimethylimidazole in 10 mL deionized water to obtain solution A; dissolve 10 mg 1,3,5-trimethylbenzenecarboxylic acid in 10 mL ethanol to obtain solution B.

[0099] Example 4

[0100] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0101] S2-1, take 1g of toluene diisocyanate (TDI), add polylactic acid (PLA) with a molecular weight of 2000 and polypropylene glycol with a molecular weight of 2500, and dissolve them together in 20mL of acetonitrile, wherein the isocyanate content accounts for 40% of the reaction system, the polylactic acid content accounts for 8% of the reaction system, and the polypropylene glycol content accounts for 3% of the reaction system. After ensuring complete dissolution by ultrasound, heat the reaction system to 70°C and stir for 2 hours to obtain a polyurethane prepolymer;

[0102] S2-2, lower the temperature of the reaction system to 40°C, add 1g of trimethylolpropane (TMP), ensure that the ratio of -NCO to -OH in the added monomer is 1.5:1, and carry out chain extension reaction for 4 hours;

[0103] S2-3, add 1 wt % triethylamine (TEA) solution as a neutralizing agent, and continue the neutralization reaction for 30 minutes.

[0104] Example 5

[0105] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0106] S2-1, take 5g of toluene diisocyanate (TDI), add polylactic acid (PLA) with a molecular weight of 4000 and polypropylene glycol with a molecular weight of 2500, and dissolve them together in 20mL of acetonitrile, wherein the isocyanate content accounts for 55% of the reaction system, the polylactic acid content accounts for 10% of the reaction system, and the polypropylene glycol content accounts for 5% of the reaction system. After ensuring complete dissolution by ultrasound, heat the reaction system to 70°C and stir for 2 hours to obtain a polyurethane prepolymer;

[0107] S2-2, lower the temperature of the reaction system to 40°C, add 2 g of trimethylolpropane (TMP), ensure that the ratio of -NCO to -OH in the added monomer is 2.5:1, and carry out chain extension reaction for 4 hours;

[0108] S2-3, add 2 wt % triethylamine (TEA) solution as a neutralizing agent, and continue the neutralization reaction for 30 minutes.

[0109] Example 6

[0110] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0111] S3-1. At room temperature (25°C), 10 mg of Mn-HMS-MOF was dispersed and suspended in 30 mL of tromethamine solution (pH = 8);

[0112] S3-2, add 5 mg dopamine hydrochloride and 100 mg polyurethane microspheres.

[0113] Example 7

[0114] This embodiment is based on Embodiment 1, and differs from Embodiment 1 in that:

[0115] S3-1. At room temperature (25°C), 100 mg of Mn-HMS-MOF was dispersed and suspended in 50 mL of tromethamine solution (pH = 8);

[0116] S3-2, add 10 mg of dopamine hydrochloride and 100 mg of polyurethane microspheres.

[0117] The preparation method of Examples 2 to 7 is used to prepare 131 The properties and effects of I-Mn-MOF@PU microspheres are similar to those in Example 1, and will not be elaborated here.

[0118] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing radioactive iodine-loaded manganese-based metal organic framework degradable embolic microspheres, It is characterized in that Using a hollow porous manganese-based metal framework combined with radioactive iodine-131, we can obtain 131 I-Mn-MOF, and then 131 I-Mn-MOF was solidified onto polyurethane microspheres to obtain manganese-based metal-organic framework-degradable embolic microspheres loaded with radioactive iodine.

2. A method for preparing a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere according to claim 1, It is characterized in that The following steps are involved: MnCl 2 •4H 2 O, polyvinyl pyrrolidone, dimethylimidazole, and 1,3,5-trimethylbenzene carboxylic acid as raw materials, firstly synthesizing a solid manganese-based metal organic framework by a solvothermal method, and then obtaining a hollow porous manganese-based metal framework by heat treatment; The polyurethane microspheres were prepared by self-emulsifying dispersion polymerization. First, a hollow porous manganese-based metal framework is used to stably bind radioactive iodine-131, and then the polydopamine encapsulation method is used to encapsulate the radioactive iodine-131. 131 I-Mn-MOF was solidified onto polyurethane microspheres to obtain manganese-based metal-organic framework-degradable embolic microspheres loaded with radioactive iodine.

3. A method for preparing a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere according to claim 2, It is characterized in that The method for preparing the hollow porous manganese-based metal framework comprises the following steps: S1-1, MnCl 2 •4H 2 O, polyvinyl pyrrolidone and dimethyl imidazole are dissolved in deionized water to obtain solution A; 1,3,5-trimethylbenzene carboxylic acid is dissolved in ethanol to obtain solution B; S1-2, mixing solution A and solution B to form a mixture, then transferring the mixture to a reactor for heat preservation and reaction, washing and drying the powder obtained by the reaction to obtain Mn-sMOF; S1-3, heat-treating the Mn-sMOF, first heating it up, then keeping it warm, and then cooling it down to obtain a sample; S1-4. The sample is added to a deionized water solution of dimethylimidazole for ultrasonic treatment, and then centrifuged to remove non-nanoscale large agglomerates to obtain a hollow porous manganese-based metal framework Mn-HMS-MOF.

4. The method for preparing the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres according to claim 3, It is characterized in that MnCl 2 •4H 2 The mass ratio of O, polyvinyl pyrrolidone, dimethylimidazole and 1,3,5-trimethylbenzene carboxylic acid is 20~50:10~20:5~10:5~10.

5. The method for preparing a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere according to claim 2, It is characterized in that The preparation method of the polyurethane microspheres comprises the following steps: S2-1, dissolving isocyanate, polylactic acid and polypropylene glycol in acetonitrile, heating the reaction system to 65°C to 70°C after complete reaction, stirring and reacting to obtain a polyurethane prepolymer; S2-2, lowering the temperature of the reaction system to 37-50°C and adding a chain extender; S2-3, adding triethylamine solution as a neutralizing agent to carry out a neutralization reaction; S2-4, after the reaction is completed, add distilled water and stir to emulsify; S2-5. After centrifugal filtration, monodisperse modified polyurethane microspheres are obtained.

6. A method for preparing a radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microsphere according to claim 5, It is characterized in that In step S2-1, the content of isocyanate accounts for 40% to 55% of the reaction system, the content of polylactic acid accounts for 8% to 10% of the reaction system, and the content of polypropylene glycol accounts for 3% to 5% of the reaction system.

7. The method for preparing the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres according to claim 5, It is characterized in that The ratio of -NCO to -OH in the chain extender monomer added in step S2-2 is 1.5-2.5:

1.

8. The method for preparing the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres according to claim 2, It is characterized in that Fabrication of hollow porous manganese-based metal frameworks and polyurethane microspheres 131 The method of I-Mn-MOF@PU microspheres comprises the following steps: S3-1, dispersing and suspending Mn-HMS-MOF in tromethamine solution; S3-2, adding dopamine hydrochloride and polyurethane microspheres; S3-3. Join 131 I-NaI solution reaction; S3-4. After the reaction is completed, the reaction product is collected, centrifuged and the supernatant is discarded; S3-5, the precipitated product is washed to obtain 131 I-Mn-MOF@PU microspheres.

9. The method for preparing the radioactive iodine-loaded manganese-based metal organic framework-containing degradable embolic microspheres according to claim 8, It is characterized in that The mass ratio of Mn-HMS-MOF, dopamine hydrochloride, and polyurethane microspheres is 10~100:5~10:

100.

10. A radioactive iodine-loaded manganese-based metal organic framework degradable embolic microsphere, It is characterized in that The method is prepared by any one of claims 1 to 9.

Citation Information

Patent Citations

  • A collagen-polyvinyl alcohol embolization microsphere loaded with iodine-131 and its preparation method

    CN111229139B

  • Preparation method for multifunctional composite microspheres

    CN105251420A

  • Medical degradable polyurethane with antibacterial activity and application thereof

    CN109503797A