Low-density bulk material suitable for plugging vertical fractures in oil fields and preparation method thereof
By preparing low-density bulk expansion materials, the bottom sinking problem caused by the large density of bulk expansion particles is solved, the sealing effect of longitudinal cracks and the temperature and salt resistance of the material are improved, and long-term longitudinal blocking is achieved Effect.
Patent Information
- Application Number
- CN202411140768.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing bulk expansion particle plugging materials have a high density, are prone to sink to the bottom, and are not strong enough to effectively block longitudinal cracks in the oil field.
The preparation method of low-density bulk expansion materials is adopted, and the expansion-type plug-in adjustment materials with a density less than water are prepared through system foaming or low-density filling. The raw materials such as acrylamide, acrylic acid, functional monomers are used, and density regulators such as gas are added. Agents, foam stabilizers and low-density fillers form gel blocks through free radical polymerization, granulation and dry them into microsphere products, improving the material's mild and salt resistance.
It realizes effective adjustment and blocking of longitudinal vertical seams and oblique seams, overcomes the problem of bottom sinking, improves the temperature resistance of the material to above 160℃, and the salt resistance to above 280,000 mineralization degrees, and extends the validity period of the material to 1. More than year.
Smart Images

Figure CN118652376B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas field exploitation, in particular to a low-density bulk expansion material suitable for regulating and plugging longitudinal cracks in oil fields and a preparation method thereof. Background Art
[0002] Fractured oil reservoirs are widely distributed in my country, such as the Laojunmiao Oilfield and Shiyougou Oilfield in Yumen, Huoshaoshan and Xiaoguai Oilfields in Xinjiang, Bushan and Qiuling Oilfields in Tuha, Ansai and Jing'an Oilfields in Changqing, Bonan and Daluhu Oilfields in Shengli, Xinli and Xinmin Oilfields in Jilin, Chaoyanggou and Toutai Oilfields in Daqing, etc. Most of these oil fields have the characteristics of low permeability fractured oil reservoirs. This is because low permeability reservoirs are generally dense, and the rock brittleness is relatively large. During the geological tectonic activities, cracks are easily generated. After water injection into low permeability fractured oil reservoirs, the injected water can easily penetrate along the fractures, causing the oil wells along the fracture direction to be violently flooded. The water content of the reservoir rises rapidly, and it enters the high water content stage in a very short time. The directionality of the water injection effect and flooding characteristics of the oil wells is obvious. The injection pressure of the water injection wells is low, the water absorption capacity is strong, and there is an obvious inflection point on the water injection indicator curve. How to control water and increase oil production, improve water injection development effects, and increase the ultimate recovery rate in this type of oil reservoir is a difficult and hot topic in current research at home and abroad.
[0003] The bulk-swelling granular plugging material is a kind of material that hydrates and expands, and then plugs small channels with its own deformation, or migrates to the deep formation through deformation under a certain pressure difference. It not only increases the plugging radius, but also achieves a secondary plugging effect of plugging after breakthrough migration. It is particularly suitable for high-permeability reservoirs with cracks and large pores. The density of conventional bulk-swelling granular materials is higher than that of water, and they maintain a certain degree of suspension in flowing water. However, after the injected water enters the formation, the seepage rate is very slow, and the conventional bulk-swelling granular materials tend to sink to the bottom of the area and gather at the bottom, thus failing to achieve the purpose of plugging "vertical seams" and longitudinal plugging. At the same time, the expansion of bulk-swelling granular plugging agents is greatly affected by water quality, and the strength is reduced after expansion. It is more susceptible to shear degradation, and it is easy to dehydrate at high temperature, resulting in a short plugging period. Therefore, the temperature resistance, salt resistance and long-term performance of bulk-swelling granular plugging materials are the directions that urgently need further technical improvements. Summary of the invention
[0004] In view of the problem that the current bulk expansion particle plugging materials have a high density and are easy to sink to the bottom, the present invention provides a low-density bulk expansion material suitable for plugging of longitudinal fractures in oil fields and a preparation method thereof. The bulk expansion material is a bulk expansion plugging material that can absorb water and expand, and has a density less than water, which overcomes the problem that the existing plugging agent is easy to sink to the bottom.
[0005] The low-density bulk material suitable for plugging and regulating longitudinal fractures in oil fields provided by the present invention has a preparation method as follows:
[0006] S1. Add water, acrylamide, acrylic acid, functional monomers, reaction regulator, pH regulator, crosslinking agent, initiator and density regulator into a reaction container, and stir until dissolved to form a reaction solution.
[0007] The density regulator includes one or two of a gas generating agent, a foam stabilizer, and a low-density filler.
[0008] The gas generating agent is selected from one or two of sodium bicarbonate, sodium nitrite, ammonium chloride, alumina powder and aluminum powder.
[0009] The foam stabilizer is selected from one or two of polyacrylamide, polyvinyl alcohol, cellulose, starch, sodium dodecyl sulfate, sodium polyoxyethylene fatty alcohol sulfate, and sodium dodecylbenzene sulfonate.
[0010] The low-density filler is selected from one of hollow glass microspheres, perlite, silicon micropowder, and nano-silicon dioxide.
[0011] The functional monomer is selected from any one of maleic acid MA, fumaric acid FA, maleic anhydride, itaconic acid, sodium allyl sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, sodium 2-acrylamido-2-methylpropane sulfonate, sodium p-styrene sulfonate, dimethyldiallylammonium chloride, acryloyloxyethyltrimethylammonium chloride, methyl acrylate, methyl methacrylate, dimethylaminoethyl acrylate, methacrylateoxyethyltrimethylammonium chloride, allylamine, triallylamine, diallylamine hydrochloride, diallylamine, N,N-dimethylallylamine, N-methyldiallylamine, and allyl ether.
[0012] The reaction regulator is selected from one of ammonium acetate, urea, thiourea, disodium ethylenediaminetetraacetate, oxalic acid, formic acid and citric acid.
[0013] The cross-linking agent is a supramolecular cross-linking agent that can participate in the polymerization reaction, and is selected from one of dimethyldiallylammonium chloride, triallylmethylammonium chloride, tetraallylammonium chloride, 1,4-divinylbenzene, and trivinylbenzene.
[0014] The pH regulator is selected from one of sodium hydroxide, ammonia water, triethanolamine, potassium hydroxide and sodium bicarbonate.
[0015] The initiator is selected from one or two of ammonium persulfate, potassium persulfate, sodium sulfite, sodium bisulfite, azobisisobutyronitrile, and azobisisobutyronitrile imidazoline hydrochloride.
[0016] The weight proportions of the raw material components are as follows:
[0017] 10-30 parts of acrylamide, 5-20 parts of acrylic acid, 2-15 parts of functional monomers, 30-70 parts of water, 0.2-2 parts of cross-linking agent, 0-2 parts of reaction regulator, 2-8 parts of pH regulator, 0.05-0.5 parts of initiator, 0-10 parts of gas generating agent, 0-3 parts of foam stabilizer, and 0-20 parts of density regulator.
[0018] S2. Deoxygenate with nitrogen until the oxygen concentration in the reaction vessel drops below 1%, then adjust the temperature of the reaction solution system to 20°C ± 2°C, let it stand for reaction, and free radical polymerization occurs under the action of the initiator to eventually form a gel block.
[0019] S3, granulating the gel block to obtain a granular wet material product.
[0020] S4. Dry the wet product to form dry material particles.
[0021] S5. Use a grinding device to process the dry material particles into spherical powder, which is the microsphere product.
[0022] Compared with the prior art, the present invention is beneficial in that:
[0023] (1) The present invention adopts a system foaming or low-density filling method to prepare a low-density bulk expansion plugging material. The prepared material can be a gas foaming type, specifically divided into an air-filled type, a self-generated nitrogen type and a self-generated carbon dioxide type, or a low-density pressure-resistant material-filled type; the prepared bulk expansion particle plugging agent has a density less than that of water, which is helpful for the plugging of longitudinal vertical seams and oblique seams, achieving a longitudinal plugging effect, and overcoming the problem that the existing plugging agents are easy to sink to the bottom.
[0024] (2) The present invention improves the temperature resistance of the plugging material to above 160°C.
[0025] (3) The present invention improves the salt resistance of the plugging material to above 280,000 mineralization degrees.
[0026] (4) The present invention improves the long-term effectiveness of the plugging material, and the effective period is extended to more than 1 year at 160°C.
[0027] (5) The low-density pressure-resistant material-filled product prepared by the present invention is less affected by the bottom hole pressure. The density under normal pressure on the ground is basically consistent with the density under high pressure at the bottom hole. It has better adaptability to the high temperature and high pressure environment of the reservoir, and overcomes the problem that the gas in the gas foaming product will be compressed under high pressure and the density will increase.
[0028] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1The present invention is a flow chart of a method for preparing a low-density plugging material for improving oil field recovery.
[0030] Figure 2 These are pictures of plugging agent products in different forms after processing, where (a), (b), and (c) are pictures of plugging agent products in three different forms, respectively.
[0031] Figure 3 These are photographs of the floating effect of the plugging material of Example 1 in water, wherein (a) and (b) are a front view and a top view, respectively.
[0032] Figure 4 These are photographs of the swelling effect of the plugging material of Example 1, wherein (a) and (b) are the front view and top view, respectively. DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0034] Example 1
[0035] A low-density bulk material suitable for plugging vertical fractures in oil fields, such as Figure 1 As shown, the preparation method is as follows:
[0036] S1. Taking the total amount of all raw materials as 100 parts by weight, weigh each raw material according to the following proportions:
[0037] 20 parts of acrylamide, 12 parts of acrylic acid, 8 parts of sodium 2-acrylamido-2-methylpropene sulfonate, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 6 parts of sodium hydroxide, 0.6 parts of dimethyldiallylammonium chloride, a cross-linking agent, 2 parts of sodium nitrite, 1.8 parts of ammonium chloride, 2 parts of polyvinyl alcohol, a foam stabilizer, 0.2 parts of ammonium persulfate, an initiator, 0.1 parts of sodium bisulfite, and the balance is water.
[0038] S2. Deoxygenate with nitrogen until the oxygen concentration in the reaction vessel drops below 1%, then adjust the temperature of the reaction solution system to 20℃±2℃, let it stand for reaction, and free radical polymerization occurs under the action of the initiator, eventually forming a gel block. This reaction is an exothermic reaction, and the reaction speed is slow in the early stage. As the reaction continues to release heat, the system gradually heats up, and the reaction speed accelerates in the later stage, eventually forming a high-temperature gel block. The reaction time is 2~4h. After the system temperature rises to the highest temperature and then begins to cool down by itself, it proves that the reaction is over.
[0039] S3. The gel block is prepared into granules by a granulating device to obtain a granular wet material product.
[0040] S4. Dry the wet product to form dry material particles.
[0041] S5. Process the dry material particles into microsphere powder using a grinding device, which is a microsphere product.
[0042] According to different production processes, the plugging materials can be selectively processed into wet material granules (adjustable shape, size, and moisture content), dry material granules (adjustable shape and size), and dry material microsphere powders (adjustable particle size), for example Figure 2 Different plugging agent product forms are shown in the figure, where (a), (b), and (c) are pictures of three different forms of plugging agents, respectively, to meet the plugging needs of reservoirs with different fracture sizes and fracture types.
[0043] Example 2
[0044] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0045] 12.5 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of itaconic acid, 0.2 parts of thiourea, 0.1 parts of ammonium acetate, 3.6 parts of ammonia water, 0.36 parts of tetraallylammonium chloride, 2 parts of sodium nitrite, 2 parts of ammonium chloride, 2 parts of polyvinyl alcohol as a foam stabilizer, 0.15 parts of ammonium persulfate as an initiator, 0.08 parts of sodium bisulfite as an initiator, and the balance is water.
[0046] The preparation steps are the same as those in Example 1.
[0047] Example 3
[0048] A low-density bulk material suitable for plugging vertical cracks in oil fields. Based on 100 parts by weight of the total amount of all raw materials, the dosage of each raw material component is as follows:
[0049] 20 parts of acrylamide, 12 parts of acrylic acid, 8 parts of dimethylaminoethyl acrylate, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 6 parts of sodium hydroxide, 0.6 parts of 1,4-divinylbenzene, 3 parts of sodium bicarbonate, 0.5 parts of polyacrylamide, 0.5 parts of polyvinyl alcohol, 0.2 parts of initiator ammonium persulfate, 0.1 parts of initiator sodium bisulfite, and the balance is water.
[0050] The preparation steps are the same as those in Example 1.
[0051] Example 4
[0052] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0053] 12.5 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of dimethylaminoethyl acrylate, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 3.6 parts of sodium hydroxide, 0.36 parts of 1,4-divinylbenzene, 3 parts of sodium bicarbonate, 0.5 parts of polyacrylamide, 0.5 parts of polyvinyl alcohol, 0.15 parts of initiator ammonium persulfate, 0.08 parts of initiator sodium bisulfite, and the balance is water.
[0054] The preparation steps are the same as those in Example 1.
[0055] The plugging materials prepared in Examples 1-4 are self-generated low-density products. Examples 1-2 are self-generated nitrogen foaming system low-density plugging materials. Examples 3-4 are self-generated carbon dioxide low-density plugging materials. The preparation principle is as follows:
[0056] The gas generating agent added to the system reacts at high temperature to generate gas, thereby reducing the density of the system. The free radical polymerization reaction causes the viscosity and temperature of the system to gradually increase. The initial reaction temperature of the preparation method is 20℃±2℃. As the reaction progresses, the system temperature rises to the reaction temperature of the gas generating agent, and the gas generating agent generates gas. At this time, the system has risen to a higher viscosity, and the generated gas can be stabilized in the system without dissipating, thereby forming uniform and stable low-density gel particles. Therefore, the system does not require foam stabilization measures.
[0057] Example 5
[0058] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0059] 20 parts of acrylamide, 12 parts of acrylic acid, 8 parts of methacrylic acid oxyethyl trimethyl ammonium chloride, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 6 parts of sodium hydroxide, 0.6 parts of trivinylbenzene, 0.5 parts of polyacrylamide, 0.5 parts of sodium dodecylbenzene sulfonate, 0.5 parts of polyvinyl alcohol, 0.2 parts of initiator ammonium persulfate, 0.1 parts of initiator sodium bisulfite, and the balance is water.
[0060] The preparation steps are the same as those in Example 1.
[0061] Example 6
[0062] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0063] 12.5 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of acryloyloxyethyltrimethylammonium chloride, 3.6 parts of sodium hydroxide, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 0.36 parts of trivinylbenzene, 0.5 parts of polyacrylamide, 0.5 parts of sodium dodecylbenzene sulfonate, 0.5 parts of polyvinyl alcohol, 0.15 parts of initiator ammonium persulfate, 0.08 parts of initiator sodium bisulfite, and the balance is water.
[0064] The preparation steps are the same as those in Example 1.
[0065] Examples 5 and 6 belong to air-entrained air-foamed low-density plugging materials. The preparation principle is to add a foaming agent during the preparation process, and then reduce the density of the system due to nitrogen bubbling during the nitrogen deoxygenation process. Since the bubble density is small and it will float, the system needs to take foam stabilizing measures and add a foam stabilizing agent to allow the bubbles to be evenly dispersed in the solution to ensure the uniformity of the product. Subsequently, as the viscosity of the reaction system increases, the bubble stability is further improved.
[0066] Example 7
[0067] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0068] 20 parts of acrylamide, 12 parts of acrylic acid, 8 parts of sodium 2-acrylamido-2-methylpropene sulfonate, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 6 parts of sodium hydroxide, 0.6 parts of tetraallylammonium chloride, 15 parts of hollow glass microspheres, 0.2 parts of initiator ammonium persulfate, 0.1 parts of initiator sodium bisulfite, and the balance is water.
[0069] The preparation steps are the same as those in Example 1.
[0070] Example 8
[0071] A low-density bulk material suitable for plugging vertical cracks in oil fields. The amount of each raw material component is as follows, based on 100 parts by weight of the total amount of all raw materials:
[0072] 12.5 parts of acrylamide, 7.5 parts of acrylic acid, 5 parts of sodium 2-acrylamido-2-methylpropene sulfonate, 0.2 parts of urea, 0.1 parts of disodium ethylenediaminetetraacetate, 3.6 parts of sodium hydroxide, 0.36 parts of tetraallylammonium chloride, 10 parts of silicon powder, 0.15 parts of initiator ammonium persulfate, 0.08 parts of initiator sodium bisulfite, and the balance is water.
[0073] The preparation steps are the same as those in Example 1.
[0074] Examples 7 and 8 are low-density pressure-resistant materials filled with modified low-density plugging materials. The preparation principle is: the addition of low-density hollow materials can reduce the density of the system, but since the low-density materials are lower than water, it is difficult to float and disperse them evenly and stably in aqueous solution. Therefore, the present invention uses a foam stabilizer and refers to the method of stabilizing bubbles to prepare the low-density hollow materials and the reaction system into a suspended slurry, thereby promoting the preparation of a uniform and stable product.
[0075] Comparative Example 1
[0076] On the basis of Example 1, the three components of 2 parts of sodium nitrite, 1.8 parts of ammonium chloride and 2 parts of foam stabilizer-polyvinyl alcohol were deleted from the raw materials to prepare a plugging material without low-density modification.
[0077] Comparative Example 2
[0078] On the basis of Example 3, 3 parts of sodium bicarbonate, 0.5 parts of polyacrylamide and 0.5 parts of polyvinyl alcohol were deleted from the raw materials to prepare a plugging material without low-density modification.
[0079] The performance tests of the plugging materials prepared in the above examples and comparative examples are as follows:
[0080] (1) The density test results of the plugging material are shown in Table 1.
[0081] Table 1 Density values of plugging materials prepared in some examples and comparative examples
[0082]
[0083] It can be seen from Table 1 that compared with Comparative Examples 1 and 2, the density of the plugging material after low-density modification by self-generated nitrogen, low-density modification by self-generated carbon dioxide, low-density modification by air foaming and low-density material filling is effectively reduced (less than the density of water 1.0 g / cm 3 ). Therefore, the plugging material of the present invention can effectively float in water without sticking or agglomerating. Figure 3 As shown, (a) and (b) are the front view and top view respectively. After entering the formation, it has a tendency to float upward, giving priority to plugging the upper end of the crack, and can meet the plugging requirements of the vertical crack through different density gradations. It overcomes the technical defect that the particle density of conventional plugging agent is greater than that of water, which produces sedimentation under the effect of gravity and tends to plug the bottom of the crack, resulting in poor plugging effect on the upper part of the crack.
[0084] (2) The swelling effect of the plugging material of the present invention is as follows: Figure 4As shown, (a) and (b) are the front view and top view respectively. As the plugging material absorbs water, its density will increase, but the overall density is still less than that of water. The block-shaped, flexible plugging body formed after swelling still floats in the injected water and tends to plug the top of the fracture during the migration of the reservoir, which can meet the requirements of the present invention.
[0085] (3) Temperature resistance test of plugging materials:
[0086] The plugging materials of each embodiment and comparative examples 1 and 2 were processed into dry material particles as samples to be tested, and two existing similar plugging agents (external samples 1 and 2) were taken as comparisons. External sample 1 is a gel particle prepared according to the method of Example 2 in the existing patent document CN102850488B (a low-density secondary expansion type gel particle). External sample 2 is a body expansion particle prepared according to the method of Example 1 in the patent document CN 102127410 A (slow expansion type pre-crosslinked gel body expansion particle and its preparation method). 5g of the sample to be tested was added to water at different temperatures (25°C and 160°C) respectively, and the mass change of the sample after different swelling time was tested. The test results are shown in Table 2.
[0087] Table 2. Test results of temperature resistance of plugging materials
[0088]
[0089] It can be seen from the test results of temperature resistance in Table 2 that the temperature resistance of the embodiment and the comparative example provided by the present invention is significantly improved compared with the temperature resistance of the two foreign samples. At 160°C, the validity period evaluation of the embodiment and the comparative example provided by the present invention is greater than 12 months (1 year); the validity period evaluation of the foreign samples is only 4.81 months and 2.85 months, respectively. Therefore, the present invention improves the long-term effectiveness and temperature resistance of the bulk expansion particle plugging agent, and the validity period at 160°C is extended to more than 1 year.
[0090] (4) Salt resistance test of plugging materials:
[0091] The plugging materials of each embodiment, comparative example 1 and 2 were processed into dry material granules as samples to be tested, and two existing similar plugging agents (external samples 1 and 2, which are bulk-expanding plugging granules used in oil fields) were taken as comparisons. 5g of the samples to be tested were added to water with different water quality conditions, and the mass changes of the samples were tested after swelling for 24 hours. The test results are shown in Table 3. In the table, 35000ppm, 70000ppm, 140000ppm, and 280000ppm represent different mineralizations, namely 35,000 mineralization, 70,000 mineralization, 140,000 mineralization, and 280,000 mineralization, respectively.
[0092] Table 3. Test results of salt resistance of plugging materials
[0093]
[0094] It can be seen from the test results in Table 3 that the salt resistance of the plugging material prepared by the present invention is improved to above 280,000 mineralization degrees, and the salt resistance is significantly better than that of the two foreign samples.
[0095] In summary, the present invention adopts free radical polymerization monomers and polymerizable supramolecular cross-linking agents to carry out free radical polymerization reactions, and introduces density regulators to prepare low-density water-absorbing and swelling plugging materials. At the same time, the temperature resistance, salt resistance and swelling characteristics of the plugging materials are improved, which is helpful for the plugging of longitudinal vertical seams and oblique seams, achieving a longitudinal plugging effect.
[0096] The two types of bulk expansion materials prepared by the present invention can both achieve low-density products and improve the plugging effect of longitudinal cracks in reservoirs. However, there is a shortcoming in gas foaming products: the gas is highly compressible. After the product is constructed to the bottom of the well, the gas compression causes the foaming volume to become smaller, and the density of the product will increase. As for the low-density pressure-resistant material filling type, the filling material is pressure-resistant, and the product is less affected by the bottom hole pressure. The density under normal pressure on the ground is basically the same as the density under high pressure at the bottom of the well, which solves the problem of gas foaming products. Therefore, low-density pressure-resistant material filling products have better adaptability to the high temperature and high pressure environment of the reservoir.
[0097] The above description is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a low-density bulk material suitable for plugging vertical fractures in oil fields, characterized in that: Here are the steps: S1. Add water, acrylamide, acrylic acid, functional monomers, reaction regulator, pH regulator, crosslinking agent, initiator and density regulator into a reaction container, and stir until dissolved to form a reaction solution; The functional monomer is selected from any one of maleic acid MA, fumaric acid FA, maleic anhydride, itaconic acid, sodium allyl sulfonate, 2-acrylamido-2-methylpropane sulfonic acid, sodium 2-acrylamido-2-methylpropane sulfonate, sodium p-styrene sulfonate, dimethyldiallylammonium chloride, acryloyloxyethyltrimethylammonium chloride, methyl acrylate, methyl methacrylate, dimethylaminoethyl acrylate, methacrylateoxyethyltrimethylammonium chloride, allylamine, triallylamine, diallylamine hydrochloride, diallylamine, N,N-dimethylallylamine, N-methyldiallylamine, and allyl ether; The reaction regulator is selected from one of ammonium acetate, urea, thiourea, disodium ethylenediaminetetraacetate, oxalic acid, formic acid, and citric acid; The cross-linking agent is selected from one of dimethyldiallylammonium chloride, triallylmethylammonium chloride, tetraallylammonium chloride, 1,4-divinylbenzene and trivinylbenzene; The density regulator includes one or two of a gas generating agent, a foam stabilizer, and a low-density filler; The gas generating agent is selected from one or two of sodium bicarbonate, sodium nitrite, ammonium chloride, alumina powder, and aluminum powder; The foam stabilizer is selected from one or two of polyacrylamide, polyvinyl alcohol, cellulose, starch, sodium dodecyl sulfate, sodium polyoxyethylene fatty alcohol sulfate, and sodium dodecylbenzene sulfonate; The low-density filler is selected from one of hollow glass microspheres, perlite, silica powder, and nano-silicon dioxide; S2, passing nitrogen to deoxygenate until the oxygen concentration in the reaction container is reduced to below 1%, then adjusting the temperature of the reaction solution system to 20°C ± 2°C, allowing the reaction to proceed, and a free radical polymerization reaction occurs under the action of the initiator, eventually forming a gel block; S3, granulating the gel block to obtain a granular wet material product; S4, drying the wet material product to form dry material particles; S5. Use a grinding device to process the dry material particles into spherical powder, which is the microsphere product.
2. A low-density bulk material suitable for plugging vertical fractures in oil fields, characterized in that: The method is adopted as claimed in claim 1.