Hot mix epoxy asphalt mixture and preparation method and application thereof
By using tetramethyl isophthalene diisocyanate (TMXDI) blocked prepolymer and isocyanate monomer in epoxy asphalt composition, the epoxy asphalt mixture is solved by excessive strength and low temperature ease after curing at high temperatures. The cracking problem improves its flexibility and water resistance, and meets the high-performance needs of steel bridge deck paving materials.
Patent Information
- Application Number
- CN202411133007.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing hot-mixed epoxy asphalt mixture is too strong after curing at high temperature and is not flexible enough. Especially under low temperature conditions, it is prone to fatigue cracks, and its water resistance is poor, making it difficult to meet the high level of steel bridge deck paving materials. Performance requirements.
TMXDI terminal blocking prepolymer is prepared by reacting with amino silicone oil or alkyl hydroxy silicone oil and in epoxy Isocyanate monomer is added to the asphalt composition to improve its high temperature performance and water resistance.
A good flexibility of epoxy asphalt cured colloid was obtained, which had high and low temperature performance and water resistance, significantly improved the durability and stability of epoxy asphalt mixture, and avoided the problem of low-temperature cracking and strength reduction after water soaking.
Smart Images

Figure CN118652407B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials for road and bridge construction, and specifically relates to a hot-mix epoxy asphalt mixture and a preparation method and application thereof. Background Art
[0002] Petroleum asphalt refers to an asphalt product obtained from petroleum after vacuum distillation and degassing. It has good durability and stability. As one of the main materials for road paving, it is suitable for pavement in urban roads, highways, airport runways, etc. However, as a natural thermoplastic material, petroleum asphalt has poor high-temperature strength and low-temperature crack resistance, and it is difficult to meet the performance requirements of high-grade pavement, especially steel bridge deck paving. Therefore, the development of high-performance asphalt polymer composite materials based on petroleum asphalt has become an important research direction at present.
[0003] As an important part of the bridge structure, the steel bridge deck pavement has its own characteristics that have an important impact on the durability and economy of the bridge. At present, the main materials for steel bridge deck pavement are cast asphalt mixture, asphalt mastic macadam and epoxy asphalt mixture. Among them, cast asphalt mixture and asphalt mastic macadam and other asphalt materials have low modulus and have the disadvantage of insufficient durability as the steel bridge deck pavement layer. Epoxy asphalt, as a thermosetting material, has excellent mechanical properties and can greatly improve the durability of the bridge deck pavement layer. However, the cross-linking density of epoxy resin is large after curing, resulting in poor coordination deformation ability with the steel bridge deck, especially when subjected to repeated vehicle loads or cracking in low temperature environments. Polyurethane prepolymers are multi-block polymers. The introduction of block structures such as polyether can obtain excellent flexibility, thereby improving low-temperature crack resistance. In addition, polyether polyurethane prepolymers have good compatibility with epoxy, but there is still a problem of poor high-temperature stability. At the same time, the polyether segment itself is hygroscopic, which easily leads to a decrease in the strength of epoxy asphalt mixtures after water immersion.
[0004] It can be seen from this that hot-mix epoxy resin asphalt mixture has the problem of too high strength and relatively insufficient flexibility after high-temperature curing, especially prone to fatigue cracks under low temperature conditions. It is necessary to add other resin prepolymers to toughen and modify it while taking into account strength, toughness and water resistance. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides an epoxy asphalt composition modified by a tetramethyl metaxylylene diisocyanate (TMXDI) end-capped prepolymer and a corresponding hot-mix epoxy asphalt mixture, thereby obtaining an epoxy asphalt cured colloid with good flexibility and a hot-mix epoxy asphalt mixture with excellent high and low temperature performance and water resistance.
[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0007] In the first aspect, a tetramethyl meta-xylylene diisocyanate (TMXDI) terminated prepolymer, the structure of which comprises:
[0008]
[0009] or
[0010] ;
[0011] Among them, R a With R d Any one or a combination of alkyl or alkoxy groups having 1 to 10 carbon atoms, R b With R c Any one or a combination of alkyl or aromatic groups having 1 to 6 carbon atoms, wherein n and m are integers greater than or equal to 1. Preferably, R c Any one or a combination of methyl, ethyl or phenyl;
[0012] Wherein, the TMXDI end-capped prepolymer is obtained by reacting TMXDI monomer with amino silicone oil or alkoxy silicone oil; the molar ratio of TMXDI to amino silicone oil or alkoxy silicone oil is 1.1-1.5:1; preferably, the molar ratio of TMXDI monomer to amino silicone oil or alkoxy silicone oil is 1.1-1.3:1;
[0013] Wherein, the weight average molecular weight of the TMXDI-terminated prepolymer is 500-7000; preferably, the weight average molecular weight of the TMXDI-terminated prepolymer is 500-4000;
[0014] The molecular weight of the amino silicone oil or the alkoxy silicone oil is 500-5000, and preferably, the molecular weight of the amino silicone oil or the alkoxy silicone oil is 500-2000.
[0015] In a second aspect, the method for preparing the above-mentioned TMXDI-terminated prepolymer comprises: reacting TMXDI monomer with amino silicone oil and alkylhydroxy silicone oil to obtain the prepolymer.
[0016] The reaction process is expressed as:
[0017]
[0018] or
[0019] ;
[0020] Wherein, the reaction temperature is 60-100°C, preferably, the reaction temperature is 70-90°C;
[0021] Furthermore, a catalyst is used to catalyze and accelerate the reaction during the reaction of TMXDI monomer with amino silicone oil and alkylhydroxy silicone oil. The catalyst is used to catalyze the reaction between isocyanate and hydroxyl or amino group. Preferably, the catalyst is an organic tin compound, and more preferably, the catalyst is dibutyltin dilaurate (DBTDL for short).
[0022] Preferably, the amount of the catalyst used is 0.05-0.5 wt % of the total amount of the two reactants, and more preferably, the amount of the catalyst used is 0.08-0.2 wt % of the total amount of the two reactants.
[0023] In a third aspect, an epoxy asphalt composition comprises 20-30 wt % of an epoxy resin, 40-60 wt % of an asphalt, 10-20 wt % of a curing agent, 1-3 wt % of a compatibilizer, and 1-10 wt % of the above-mentioned TMXDI-terminated prepolymer.
[0024] Among them, the epoxy resin is selected from: one or more combinations of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, polyphenol glycidyl ether epoxy resin, alicyclic epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, and hydantoin epoxy resin, and each epoxy resin molecule contains at least 2 epoxy groups.
[0025] Preferably, the epoxy resin is bisphenol A epoxy resin; more preferably, the epoxy resin is selected from E-51 or E-44 epoxy resin.
[0026] Among them, the asphalt is selected from petroleum asphalt or modified asphalt, the petroleum asphalt is obtained by concentrating the high boiling point components contained in crude oil, and the modified asphalt is selected from styrene-butadiene rubber (SBR) modified petroleum asphalt, styrene-butadiene-styrene block copolymer (SBS) or styrene-isoprene-styrene (SIS) modified petroleum asphalt.
[0027] Wherein, the curing agent is selected from: any one of an amine curing agent and an acid anhydride curing agent, the amine curing agent includes any one of m-phenylenediamine, diaminodiphenylmethane, benzyldimethylamine, benzyldimethylamine, diethylenetriamine, polyethylenepolyamine, hexamethylenediamine, triethylamine, triethanolamine, hexahydropyridine, 1,3-cyclohexanedimethylamine, isophoronediamine, dicyandiamide and 4,4'-diaminodiphenyl sulfone; the acid anhydride curing agent includes any one of phthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, methylhexahydrophthalic anhydride, polyisobutylene succinic anhydride, methyl nadic anhydride, modified methyl nadic anhydride, dodecenyl succinic anhydride, modified tung oil anhydride, polyazelaic anhydride, polyglutaric anhydride and polyethylene oxalic anhydride.
[0028] Preferably, the curing agent is selected from anhydride curing agents; more preferably, the curing agent is selected from methyltetrahydrophthalic anhydride and / or methylhexahydrophthalic anhydride.
[0029] Wherein, the compatibilizer is selected from sodium dodecylbenzene sulfonate and / or maleic anhydride.
[0030] Furthermore, in order to improve the high temperature performance of the epoxy asphalt composition, isocyanate monomer is added to the epoxy asphalt composition. The corresponding epoxy asphalt composition includes 20~30wt% of epoxy resin, 40~60wt% of asphalt or modified asphalt, 10~20wt% of curing agent, 1~3wt% of compatibilizer, 1~10wt% of TMXDI terminated prepolymer, and the amount of isocyanate monomer is 0.5~5wt%.
[0031] Preferably, the amount of the isocyanate monomer used is 0.5-3 wt %; more preferably, the amount of the isocyanate monomer used is 0.5-2 wt %.
[0032] Among them, each isocyanate monomer contains at least 2 NCO groups, and the isocyanate monomers include: liquid MDI, TDI trimer or HDI trimer. Liquid MDI is a polyisocyanate mixture including some carbodiimide groups and uretonimine groups. Liquid MDI is a modified MDI obtained by introducing carbodiimide and uretonimine groups on the basis of solid MDI. The modified MDI is a stable liquid at room temperature; TDI trimer or HDI trimer is toluene diisocyanate (TDI) or hexamethylene diisocyanate, respectively, which can undergo trimerization reaction under catalysis to form a trimer containing an isocyanurate ring.
[0033] Preferably, the isocyanate monomer is selected from liquid MDI;
[0034] Preferably, the content of NCO groups in the liquid MDI is 25-35 wt %, and more preferably, the content of NCO groups in the liquid MDI is 28-30 wt %.
[0035] In a fourth aspect, the preparation method of the above-mentioned epoxy asphalt composition comprises: stirring and mixing the epoxy resin and the TMXDI-terminated prepolymer at a temperature of 40-60°C to obtain component A, stirring and mixing asphalt or rubber-modified asphalt with a curing agent and a compatibilizer at a temperature of 120-180°C to obtain component B, and stirring and mixing component A and component B at a temperature of 120-180°C to obtain the epoxy asphalt composition.
[0036] Or, a method for preparing an epoxy asphalt composition, comprising: stirring and mixing an epoxy resin and a TMXDI-terminated prepolymer at a temperature of 40-60°C to obtain component A, stirring and mixing asphalt or rubber-modified asphalt with a curing agent and a compatibilizer at a temperature of 120-160°C to obtain component B, and stirring and mixing component A, component B and an isocyanate monomer at a temperature of 120-160°C to obtain the epoxy asphalt composition.
[0037] In a fifth aspect, an epoxy asphalt cured colloid is obtained by curing the epoxy asphalt composition described above at a temperature not lower than 150°C.
[0038] Preferably, the epoxy asphalt composition is cured at a temperature of 150-200° C. to obtain an epoxy asphalt cured colloid.
[0039] Preferably, the curing time is 4 to 10 hours.
[0040] In a sixth aspect, a hot-mix epoxy asphalt mixture comprises 1-10 wt % of the epoxy asphalt composition described above, 1-10 wt % of a filler, 40-60 wt % of a coarse aggregate, and 30-50 wt % of a fine aggregate.
[0041] The coarse aggregate and fine aggregate are selected from one or more combinations of basalt, limestone, tuff or granite, and the filler is selected from one or more combinations of basalt, limestone, tuff or granite powder. The particle sizes of the coarse aggregate, fine aggregate and filler are different, and the coarse aggregate, fine aggregate and filler of different particle sizes can be separated by screening.
[0042] Preferably, the particle size range of the coarse aggregate is 2.36 mm ≤ coarse aggregate particle size < 9.50 mm, the particle size range of the fine aggregate is 0.075 mm ≤ fine aggregate particle size < 2.360 mm, and the particle size of the filler is less than 0.06 mm;
[0043] Preferably, the weight of the epoxy asphalt composition does not exceed 8wt% of the total weight of the hot mix epoxy asphalt mixture; more preferably, the weight of the epoxy asphalt composition is 6-7wt% of the total weight of the hot mix epoxy asphalt mixture.
[0044] In the seventh aspect, the preparation method of the hot mix epoxy asphalt mixture described above comprises: stirring and mixing coarse aggregate, fine aggregate and mineral powder at a temperature of 120-180°C to obtain a mixed aggregate component C, mixing component C with an epoxy asphalt composition, and curing at a temperature not lower than 150°C to obtain a hot mix epoxy asphalt mixture.
[0045] Preferably, the coarse aggregate, fine aggregate and mineral powder are stirred and mixed at 120-150° C. to obtain the mixed aggregate component C.
[0046] Preferably, component C is mixed with the epoxy asphalt composition and then cured at 150-200° C. to obtain a hot-mix epoxy asphalt mixture.
[0047] Preferably, the curing time of component C and the epoxy asphalt composition is 4 to 10 hours.
[0048] In an eighth aspect, the hot mix epoxy asphalt mixture described above is used as a bridge deck paving material.
[0049] The present invention has the following beneficial effects:
[0050] The present invention first synthesizes a TMXDI prepolymer containing a siloxane segment. The main chain of the siloxane segment has a Si-O-Si structure, has a long bond length, a large bond angle, is easy to rotate, has a small steric hindrance to the rotation of the side chain, has a large molecular volume and a low cohesive energy density, reduces steric hindrance, and makes the free rotation of the side group easier. Therefore, the segment has high flexibility and excellent toughening effect. At the same time, the siloxane segment is more hydrophobic than polyether, which is beneficial to improving the water resistance of the epoxy asphalt composition. In addition, TMXDI belongs to aliphatic isocyanate, and the steric hindrance of the methyl groups on both sides leads to low reactivity of the NCO group, thereby controlling the TMXDI prepolymer to cross-link with the hydroxyl generated by the ring opening of the epoxy resin in the later stage of curing.
[0051] Secondly, in order to avoid a significant reduction in the strength of the epoxy asphalt composition after the addition of TMXDI prepolymer, and to improve the high temperature stability and water resistance of the hot mix epoxy asphalt mixture, it is also proposed as a preferred solution to add a highly reactive isocyanate monomer. The isocyanate monomer reacts in the initial stage of curing, which is beneficial to increase the degree of cross-linking inside the epoxy asphalt cured colloid, and the low-reactive TMXDI prepolymer undergoes cross-linking reaction on the outside, thereby obtaining an epoxy asphalt mixture that has both high temperature strength, low temperature crack resistance and water resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a scanning electron microscope image of the bonding interface of the hot mix epoxy asphalt mixture of Example 13. DETAILED DESCRIPTION
[0053] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0054] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0055] If the specific experimental conditions are not specified in the examples, they are usually based on the conventional conditions in the field or the conditions recommended by the reagent company; the materials, reagents, etc. used in the examples can be purchased through commercial channels unless otherwise specified.
[0056] Synthesis of TMXDI blocked isocyanate prepolymer: Examples 1-3.
[0057] Embodiment 1:
[0058] Hydroxypropyl terminated silicone oil with a molecular weight of 500 (IOTA-2030-5, Anhui IOTA Silicone Oil Co., Ltd., corresponding to R a = -CH2CH2OCH2CH2CH2-, R b = R c = -CH3) 420g (0.84mol) and tetramethyl metaxylene diisocyanate (TMXDI, Allnex resin) 244g (1mol) were added into a three-necked flask, stirring was started, and 0.8g of catalyst dibutyltin dilaurate (DBTDL) was added under stirring, the temperature was raised to 90°C and reacted for 2 hours, then the temperature was lowered to 50°C, unreacted TMXDI monomer was removed by vacuum distillation, and then the reaction was terminated to obtain TMXDI blocked isocyanate prepolymer, whose weight average molecular weight M w =1023g / mol.
[0059] Embodiment 2:
[0060] The 1000 molecular weight hydroxypropyl terminated silicone oil (IOTA-2030-10, Anhui IOTA Silicone Oil Co., Ltd., corresponding to R a = -CH2CH2OCH2CH2CH2-, R b = R c= -CH3) 425g (0.425mol) and tetramethyl metaxylene diisocyanate (TMXDI, Allnex resin) 122g (0.5mol) were added into a three-necked flask, and stirring was started. 0.6g of catalyst dibutyltin dilaurate (DBTDL) was added under stirring, and the temperature was raised to 90°C for reaction for 2 hours, then cooled to 50°C, and unreacted TMXDI monomer was removed by vacuum distillation. Then the reaction was terminated to obtain a TMXDI-terminated isocyanate prepolymer with a weight average molecular weight of M w =1596 g / mol.
[0061] Embodiment 3:
[0062] 2000 molecular weight amino-terminated silicone oil (Sivans ATS 2000, Sivans Materials Technology, corresponding to R in the structural formula) d = -CH2CH2CH2-, R b = R c = -CH3) 800g (0.4mol) and tetramethyl metaxylene diisocyanate (TMXDI, Allnex resin) 122g (0.5mol) were added into a three-necked flask, stirring was started, 1.0g of catalyst dibutyltin dilaurate (DBTDL) was added under stirring, the temperature was raised to 75°C and reacted for 2 hours, then the temperature was lowered to 50°C, unreacted TMXDI monomer was removed by vacuum distillation, and then the reaction was terminated to obtain TMXDI blocked isocyanate prepolymer, whose weight average molecular weight M w =2504 g / mol.
[0063] Formula of hot mix epoxy asphalt composition: Examples 4-9, Comparative Examples 1 and 2.
[0064] Embodiment 4:
[0065] Component A: 1 kg of E51 epoxy resin (Nantong Xingchen Synthetic Materials), 220 g of TMXDI blocked isocyanate prepolymer of Example 1;
[0066] Component B: Maoming Petrochemical AH-70 petroleum asphalt 2.5kg, curing agent methyl hexahydrophthalic anhydride 580g, compatibilizer maleic anhydride 80g.
[0067] Example 5 Component A includes 1 kg of E51 epoxy resin and 220 g of TMXDI blocked isocyanate prepolymer of Example 2. The rest is the same as Example 4.
[0068] Example 6 Component A includes 1 kg of E51 epoxy resin and 220 g of the TMXDI blocked isocyanate prepolymer of Example 3. The rest is the same as Example 4.
[0069] Example 7 Component A: 1 kg of E51 epoxy resin, 200 g of TMXDI blocked isocyanate prepolymer of Example 2;
[0070] Component B: Maoming Petrochemical AH-70 petroleum asphalt 2.5kg, curing agent methyl hexahydrophthalic anhydride 550g, compatibilizer maleic anhydride 80g;
[0071] The isocyanate monomer was 40 g of carbodiimide-uretonimine modified MDI (WANNATE MDI-100LL produced by Wanhua Chemical).
[0072] Example 8 Component A: 1 kg of E51 epoxy resin, 170 g of TMXDI blocked isocyanate prepolymer of Example 2;
[0073] Component B: Maoming Petrochemical AH-70 petroleum asphalt 2.5kg, curing agent methyl hexahydrophthalic anhydride 550g, compatibilizer maleic anhydride 80g;
[0074] The isocyanate monomer was 70 g of carbodiimide-uretonimine modified MDI (WANNATE MDI-100LL produced by Wanhua Chemical).
[0075] Example 9 Component A: 1 kg of E51 epoxy resin, 170 g of TMXDI blocked isocyanate prepolymer of Example 2;
[0076] Component B: Maoming Petrochemical AH-70 petroleum asphalt 2.5kg, curing agent methyl hexahydrophthalic anhydride 550g, compatibilizer maleic anhydride 80g;
[0077] The isocyanate monomer was 70 g of HDI trimer (Desmodur N3300 from Covestro).
[0078] Comparative Example 1 Component A: 1 kg of E51 epoxy resin;
[0079] Component B: Maoming Petrochemical AH-70 petroleum asphalt 2.5kg, curing agent methyl hexahydrophthalic anhydride 720g, compatibilizer maleic anhydride 80g.
[0080] Comparative Example 2 Component A: 1 kg of E51 epoxy resin, 220 g of MDI-terminated polyether polyurethane prepolymer (Olilon (Jining) Chemical Co., Ltd.), and the rest of the components were the same as in Example 4.
[0081] The hot-mix epoxy asphalt mixtures of Examples 4-8 and Comparative Examples 1 and 2 were prepared according to the following method:
[0082] (1) stirring and mixing epoxy resin and TMXDI prepolymer at 50° C. for 15 minutes to obtain a mixed component A;
[0083] (2) placing the asphalt in an oven and heating it to 130° C. for 3 hours to make it flowable liquid, adding a curing agent and a compatibilizer according to the above formula at 130° C., and mixing them at high speed for 30 minutes to obtain a mixed component B;
[0084] (3) stirring and mixing the mixed components A and B at 130° C. to obtain an epoxy asphalt composition. If there is an isocyanate monomer in the formula, add it at this time;
[0085] (4) The epoxy asphalt composition is poured into a dumbbell-shaped test mold and cured at 160°C. After curing for 6 hours, the test mold is taken out and placed in a cool place to cool down. The epoxy asphalt cured colloid obtained by demolding the test piece is used for performance testing.
[0086] Formula of hot mix epoxy asphalt mixture: Examples 10-15 and Comparative Examples 3 and 4, wherein the oil-to-stone ratio of the oil mixture formula is uniformly set to 6.7wt%.
[0087] Embodiment 10:
[0088] Component A and component B are the same as in Example 4; Component C: coarse aggregate: basalt crushed stone (2.36mm≤particle size<9.50mm) 32kg, fine aggregate: limestone machine-made sand (0.075mm≤particle size<2.360mm) 28kg, filler: limestone ore powder (particle size less than 0.06mm) 5kg.
[0089] Embodiment 11:
[0090] Component A and component B are the same as in Example 5; component C: the same as in Example 10.
[0091] Embodiment 12:
[0092] Component A and component B are the same as in Example 6; component C: the same as in Example 10.
[0093] Embodiment 13:
[0094] Component A and component B are the same as in Example 7; component C: the same as in Example 10.
[0095] Embodiment 14:
[0096] Component A and component B are the same as in Example 8; component C: the same as in Example 10.
[0097] Embodiment 15:
[0098] Component A and component B are the same as in Example 9; component C: the same as in Example 10.
[0099] Comparative Example 3:
[0100] Component A and component B are the same as those in Comparative Example 1; Component C: the same as that in Example 10.
[0101] Comparative Example 4:
[0102] Component A and component B are the same as those in Comparative Example 2; Component C: the same as that in Example 10.
[0103] The hot-mix epoxy asphalt mixtures of Examples 10-15 and Comparative Examples 3 and 4 were prepared according to the following method:
[0104] (1) Preheat the coarse aggregate, fine aggregate and mineral powder to 150° C. and stir and mix for 15 minutes to obtain component C mixed aggregate;
[0105] (2) stirring and mixing the epoxy resin and the TMXDI prepolymer at 50° C. for 15 minutes to obtain a mixed component A;
[0106] (3) mixing the petroleum asphalt, the curing agent and the compatibilizer at 130° C. for 15 minutes under high-speed shearing to obtain a mixed component B;
[0107] (4) stirring and mixing the mixed components A and B at 130° C. to obtain an epoxy asphalt composition. If there is an isocyanate monomer in the formula, add it at this time;
[0108] (5) The epoxy asphalt composition and the mixed aggregate of component C were stirred and mixed at 130° C., heated to 160° C., and maintained at this temperature for 8 hours for curing to obtain a hot-mix epoxy asphalt mixture for the next test.
[0109] Test of epoxy asphalt curing colloid:
[0110] The tensile performance test was carried out using an XLD-10KL electronic tensile testing machine at a tensile temperature of 23°C and a speed of 50 mm / min. -1 The specimen is slowly stretched at a rate until it breaks. The maximum load and deformation when the specimen breaks are obtained through the testing machine sensor. According to the cross-sectional dimensions of the specimen, the tensile strength and elongation at break of the specimen are calculated.
[0111] The bending beam rheology (BBR) test was used to test the low-temperature performance of epoxy asphalt cured colloid. The two parameters of the cured colloid, creep rate and creep stiffness modulus, were obtained using a bending rheometer. Creep stiffness characterizes the ability of the tested sample to resist permanent deformation. The greater the creep stiffness, the worse the flexibility and the greater the brittleness of the epoxy asphalt cured colloid, and the more susceptible it is to low-temperature cracking when used in pavement. The creep rate characterizes the rate of change of the stiffness of the sample under load. The larger the value of the creep rate, the smaller the value of the temperature stress inside the epoxy asphalt cured colloid, the less likely it is to accumulate low-temperature stress inside the colloid, and the stronger its low-temperature anti-cracking performance.
[0112] The results of the tensile property tests and bending beam rheological tests of Examples 4-9 and Comparative Examples 1 and 2 are shown in Table 1.
[0113] Table 1
[0114]
[0115] As can be seen from the above table, the epoxy asphalt compositions of Examples 4-6 are added with TMXDI prepolymers containing polysiloxane blocks, which contain Si-O-Si bonds. The Si-O-Si bonds are easy to rotate, have little steric hindrance to the rotation of the side chains, have large molecular volume and low cohesive energy density. By introducing segments containing Si-O-Si bonds into the epoxy asphalt compositions, the flexibility of the cured colloid can be increased and the brittleness can be reduced. The elongation at break and the creep rate are improved, but the corresponding tensile strength and stiffness modulus are reduced. Compared with the conventional polyether polyurethane prepolymer (Comparative Example 2), the addition of TMXDI prepolymer has a stronger toughening effect on the epoxy asphalt cured colloid, but the strength is also significantly reduced.
[0116] In order to balance strength and toughness, isocyanate monomers are added to the TMXDI prepolymer. The NCO group in the prepolymer has a very high reactivity, while the isocyanate in TMXDI is an aliphatic isocyanate and has the steric hindrance of two methyl groups, so the reactivity is low and the cross-linking reaction with the hydroxyl group in the epoxy asphalt composition is slower. Due to the difference in the reactivity of isocyanates with different structures, the isocyanate monomer undergoes a cross-linking reaction first during curing, and the TMXDI prepolymer undergoes a cross-linking reaction later. The resulting cured colloid has a better balance between strength and toughness.
[0117] Testing of hot mix epoxy asphalt mixture:
[0118] Low temperature crack resistance test: -10℃ small beam low temperature bending test, the fully cured hot mix epoxy asphalt mixture specimens were cut into small beam specimens with a length, width and height of 250mm×30mm×35mm. The test temperature was -10℃ and the loading rate was 50mm·min -1 The test was carried out under the conditions of
[0119] High temperature stability: Rutting test, hot mix epoxy asphalt mixture rutting test pieces are formed according to the EN12697-33-2019 procedure. After curing treatment at 60℃ / 4 days, rutting test is carried out according to EN12697-22 at 60℃ and 0.7MPa.
[0120] Immersion Marshall Test:
[0121] The water-immersion Marshall stability test is used to test the water stability of hot-mix epoxy asphalt mixtures. Marshall specimens of the hot-mix epoxy asphalt mixtures prepared in the above embodiments were prepared respectively. After curing was complete, one group of specimens was placed in a water bath for 48 hours, and the other group of specimens was placed in a water bath for 30 minutes. The water temperature of the two groups of water baths was uniformly set to 60±2°C. The two groups of specimens were subjected to Marshall tests to obtain stability, and then the stability obtained from the two groups of tests was compared to obtain the residual stability of water immersion.
[0122] Freeze-thaw splitting test:
[0123] Marshall specimens of the hot-mix epoxy asphalt mixture prepared in the above embodiment were prepared respectively. After curing was complete, one group of specimens was placed in a refrigerator at -18°C for 16 hours after vacuuming, and then placed in a 60°C water bath for 24 hours, and finally placed in warm water at 25°C for 2 hours; the other group of specimens was placed in a water bath at 25°C for 2 hours before the test. Finally, a splitting test was performed on the two groups of specimens, and the splitting strengths of the two groups of specimens were calculated. The splitting strengths obtained from the two groups of specimens were compared. The higher the freeze-thaw splitting strength ratio, the better the corresponding freeze-thaw stability.
[0124] The test results of Examples 10-15 and Comparative Examples 3 and 4 are shown in Table 2.
[0125] Table 2
[0126]
[0127] It can be seen from Table 2 that for the high temperature stability test, Examples 10-15 and Comparative Example 4 will reduce the high temperature stability and rutting resistance of the epoxy asphalt mixture to a certain extent by adding different types of isocyanate prepolymers. Among them, the high temperature stability and rutting resistance of the asphalt mixture modified by TMXDI prepolymer alone in Examples 10-12 are the most reduced. The high temperature stability and rutting resistance of the epoxy asphalt mixture in Examples 13 and 14 are improved after adding carbodiimide-modified MDI, which is slightly higher than the asphalt mixture modified by MDI prepolymer alone in Comparative Example 4. Example 15 adds HDI trimer as an isocyanate monomer, but the effect of improving the high temperature stability and rutting resistance of the epoxy asphalt mixture is not as good as the carbodiimide-modified MDI in Examples 13 and 14.
[0128] For the low-temperature crack resistance test, the bending modulus of the TMXDI prepolymer modified epoxy asphalt mixture is weakened to a certain extent. However, the bending tensile strain is improved, which shows that the introduction of TMXDI prepolymer plays a toughening role in the epoxy asphalt mixture. Among them, the low-temperature toughening effect of the TMXDI prepolymer modified epoxy asphalt mixture in Examples 10-12 is the best, while the low-temperature toughening effect of the MDI prepolymer modified asphalt mixture in Comparative Example 4 is slightly worse. Adding carbodiimide modified MDI or HDI trimer on the basis of Examples 10-12 reduces the low-temperature crack resistance.
[0129] The residual stability of water immersion and the ratio of freeze-thaw splitting strength of asphalt mixture modified by TMXDI prepolymer alone are greater than those of conventional epoxy asphalt mixture, and are close to those of MDI prepolymer modified asphalt mixture in comparative example 4. The residual stability of water immersion and the ratio of freeze-thaw splitting strength of epoxy asphalt mixture are significantly improved by adding carbodiimide modified MDI. This shows that the addition of TMXDI prepolymer has a certain effect on improving the water damage resistance and freeze-thaw resistance of epoxy asphalt mixture, but the improvement effect is not very significant. The water damage resistance and freeze-thaw resistance of epoxy asphalt mixture can be significantly improved by adding TMXDI prepolymer and carbodiimide modified MDI at the same time.
[0130] Example 13 The electron microscope scanning results of the cross section of the bonding area of the small beam specimen for low temperature crack resistance are shown in Figure 1 , magnified 25 and 35 times respectively, showing that the epoxy resin bonding layer and hot-mix epoxy asphalt mixture exhibit completely different appearances under electron microscope scanning. Figure 1 Analysis shows that the cross section of the epoxy resin bonding layer is flat, and it is immersed in the asphalt mixture in strips or blocks. There is no obvious interface separation due to different material properties, but it is tightly bonded to the surrounding asphalt mortar. This shows that there is an excellent interlayer interface bonding effect between the epoxy resin bonding layer and the asphalt mixture. There is no obvious cracking or cracking at a low temperature of -10℃, and it still maintains the wrapping effect on the asphalt mixture.
[0131] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to perform equivalent replacements on parts thereof. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention. Although the above describes the specific implementation methods of the present invention, it is not intended to limit the protection scope of the present invention. Those skilled in the art should understand that, based on the technical solution of the present invention, various modifications or deformations that can be made by those skilled in the art without creative labor are still within the protection scope of the present invention.
Claims
1. An epoxy asphalt composition, characterized in that: include: Epoxy resin 20~30wt%, asphalt 40~60wt%, curing agent 10~20wt%, compatibilizer 1~3wt%, tetramethyl meta-xylylene diisocyanate terminated prepolymer 1~10wt%; The epoxy resin is selected from the group consisting of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, polyphenol glycidyl ether epoxy resin, alicyclic epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, and hydantoin epoxy resin, or a combination thereof, and each epoxy resin molecule contains at least two epoxy groups. The asphalt is selected from petroleum asphalt, styrene-butadiene rubber modified petroleum asphalt, styrene-butadiene-styrene block copolymer or styrene-isoprene-styrene modified petroleum asphalt; The curing agent is selected from: any one of an amine curing agent and an acid anhydride curing agent, wherein the amine curing agent includes any one of m-phenylenediamine, diaminodiphenylmethane, benzyldimethylamine, benzyldimethylamine, diethylenetriamine, polyethylenepolyamine, hexamethylenediamine, triethylamine, triethanolamine, hexahydropyridine, 1,3-cyclohexanedimethylamine, isophoronediamine, dicyandiamide and 4,4'-diaminodiphenyl sulfone; the acid anhydride curing agent includes any one of phthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, trimellitic anhydride, pyromellitic dianhydride, methylhexahydrophthalic anhydride, polyisobutylene succinic anhydride, methyl nadic anhydride, modified methyl nadic anhydride, dodecenyl succinic anhydride, modified tung oil anhydride, polyazelaic anhydride, polyglutaric anhydride and polyoxalic anhydride; The compatibilizer is selected from sodium dodecylbenzene sulfonate and / or maleic anhydride; The structure of the tetramethyl meta-xylylene diisocyanate terminated prepolymer is selected from: ; or ; Among them, R a With R d Any one or a combination of alkyl or alkoxy groups having 1 to 10 carbon atoms, R b With R c Any one or a combination of alkyl or aromatic groups having 1 to 6 carbon atoms, wherein n and m are integers greater than or equal to 1.
2. An epoxy asphalt composition, characterized in that: include: Epoxy resin 20~30wt%, asphalt or modified asphalt 40~60wt%, curing agent 10~20wt%, compatibilizer 1~3wt%, tetramethyl meta-xylylene diisocyanate-terminated prepolymer 1~10wt%, isocyanate monomer 0.5~5wt%; Wherein, the structure of the tetramethyl meta-xylylene diisocyanate terminated prepolymer is selected from: ; or ; Among them, R a With R d Any one or a combination of alkyl or alkoxy groups having 1 to 10 carbon atoms, R b With R c Any one or a combination of alkyl or aromatic groups having 1 to 6 carbon atoms, wherein n and m are integers greater than or equal to 1; Wherein, each isocyanate monomer contains at least 2 NCO groups, and the isocyanate monomer includes: liquid MDI, TDI trimer or HDI trimer.
3. The epoxy asphalt composition according to any one of claims 1 to 2, characterized in that: The tetramethyl meta-xylylene diisocyanate terminated prepolymer is obtained by reacting tetramethyl meta-xylylene diisocyanate monomer with amino silicone oil or alkoxy silicone oil; the molar ratio of tetramethyl meta-xylylene diisocyanate monomer to amino silicone oil or alkoxy silicone oil is 1.1-1.5:1; and the weight average molecular weight of the prepolymer is 500-7000.
4. The epoxy asphalt composition according to claim 3, characterized in that: The molecular weight of the amino silicone oil or alkoxy silicone oil is 500-5000.
5. The epoxy asphalt composition according to any one of claims 1 to 2, characterized in that: The preparation method of the tetramethyl isophthalic acid-terminated prepolymer comprises: using a catalyst to catalyze and accelerate the reaction during the reaction of tetramethyl isophthalic acid-terminated monomer and amino silicone oil or alkylhydroxy silicone oil, the amount of the catalyst used is 0.05-0.5wt% of the total amount of the two reactants, and the reaction temperature of the tetramethyl isophthalic acid-terminated monomer and amino silicone oil or alkylhydroxy silicone oil is 60-100°C.
6. The method for preparing the epoxy asphalt composition according to any one of claims 1 to 5, characterized in that: include: The epoxy resin and tetramethyl metaxylylene diisocyanate-terminated prepolymer are stirred and mixed at a temperature of 40-60° C. to obtain component A, asphalt or rubber-modified asphalt, a curing agent and a compatibilizer are stirred and mixed at a temperature of 120-180° C. to obtain component B, and component A and component B are stirred and mixed at a temperature of 120-180° C. to obtain an epoxy asphalt composition; Alternatively, epoxy resin and tetramethyl metaxylylene diisocyanate-terminated prepolymer are stirred and mixed at a temperature of 40-60°C to obtain component A, asphalt or rubber-modified asphalt, a curing agent and a compatibilizer are stirred and mixed at a temperature of 120-160°C to obtain component B, and component A, component B and an isocyanate monomer are stirred and mixed at a temperature of 120-160°C to obtain an epoxy asphalt composition.
7. An epoxy asphalt curing colloid, characterized in that: The epoxy asphalt composition is obtained by curing the epoxy asphalt composition according to any one of claims 1 to 5 at a temperature not lower than 150°C.
8. A hot mix epoxy asphalt mixture, characterized in that: include: 1-10 wt % of the epoxy asphalt composition according to any one of claims 1 to 5, 1-10 wt % of filler, 40-60 wt % of coarse aggregate, and 30-50 wt % of fine aggregate; Wherein, the coarse aggregate and fine aggregate are selected from one or more combinations of basalt, limestone, tuff or granite, and the filler is selected from one or more combinations of basalt, limestone, tuff or granite mineral powder; the particle size range of the coarse aggregate is 2.36mm≤coarse aggregate particle size<9.50mm, the particle size range of the fine aggregate is 0.075mm≤fine aggregate particle size<2.360mm, and the particle size of the filler is less than 0.06mm; the weight of the epoxy asphalt composition does not exceed 8wt% of the total weight of the hot mix epoxy asphalt mixture.
9. The method for preparing hot mix epoxy asphalt mixture according to claim 8, characterized in that: include: The coarse aggregate, fine aggregate and mineral powder are stirred and mixed at a temperature of 120-180°C to obtain a mixed aggregate component C, and the component C is mixed with an epoxy asphalt composition, and cured at a temperature not lower than 150°C to obtain a hot-mix epoxy asphalt mixture.
10. Use of the hot mix epoxy asphalt mixture according to claim 8 as a bridge deck paving material.