A kind of preparation method and application of isocyanate curing agent

By sulfonating the reaction of titanium dioxide with polycarbonate diol, combining the hexamethylene diisocyanate trimer, a modified isocyanate curing agent is formed, which solves the problems of short stability period and poor hydrophilicity of isocyanate curing agent, and achieves the goal of achieving the problem of low stability period and poor hydrophilicity of isocyanate curing agent. Excellent UV absorption performance and storage stability.

CN118652409BActive Publication Date: 2024-11-12ZHUZHOU SHIDAI DEWEI COATING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410846493.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-12
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

The isocyanate curing agent has a short stabilization period and poor hydrophilicity, making it difficult to meet the requirements of efficient water dispersion and durability.

Method used

By using the mixed modification method, the modified polycarbonate diol is generated by reacting sulfonated titanium dioxide with polycarbonate diol, and reacting with hexamethylene diisocyanate trimer to form excellent ultraviolet absorption properties, Isocyanate curing agent with hydrophilicity and storage stability.

Benefits of technology

The thermal stability, ultraviolet absorption performance and storage stability of isocyanate curing agent are significantly improved, and the problems of large viscosity and poor water resistance are solved, and compatibility and stability with aqueous hydroxyl components are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652409B_ABST
    Figure CN118652409B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of curing agents, and discloses a preparation method and application of an isocyanate curing agent. In the present invention, 3-aminopropane sulfonic acid is reacted with epoxy-modified titanium dioxide to obtain sulfonated titanium dioxide, and the sulfonic acid group contained in the sulfonated titanium dioxide makes it have certain hydrophilicity, which is beneficial to water dispersibility; polycarbonate diol reacts with sulfonated titanium dioxide to obtain modified polycarbonate diol; the secondary amine in the modified polycarbonate diol reacts with the isocyanate group in the hexamethylene diisocyanate trimer, and the sulfonated titanium dioxide and polycarbonate diol are connected to the hexamethylene diisocyanate trimer through the connection of urea groups. The isocyanate curing agent prepared by the preparation method of the present invention has excellent hydrophilicity, storage stability and anti-ultraviolet performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of curing agents, and in particular to a preparation method and application of an isocyanate curing agent. Background Art

[0002] Isocyanate curing agents are widely used in automotive coatings, architectural coatings, woodworking coatings, marine coatings, adhesives, sealants, composite materials and other fields. Isocyanate curing agents have low viscosity and high NCO content, but their water dispersibility needs to be improved. At present, there are two methods for hydrophilic modification of isocyanates: external emulsification and internal emulsification. The external emulsification method is a method of adding surfactants to polyisocyanates to obtain better water dispersibility, and its emulsion stability is poor; the internal emulsification method is also called chemical modification, which refers to a method of preparing an isocyanate curing agent with good water dispersibility by reacting a hydrophilic compound with an isocyanate, which can be divided into non-ionic modification, ionic modification and mixed modification.

[0003] Because blocked isocyanates protect the isocyanate groups that are sensitive to water, blocked isocyanates can be used as resins or curing agents for water-based coatings and can improve the waterproofing, corrosion resistance, and mechanical properties of the coating. Usually, aliphatic isocyanates are more stable than aromatic isocyanates. Groups that can react with isocyanate groups can be used as blocking agents. Due to different scopes of use and requirements, they can be divided into amide and imide blocking agents, active methylene compounds, bisulfites, and active hydrogen-containing compounds. Among amine blocking agents, primary amines react extremely quickly with isocyanates and are difficult to control.

[0004] Chinese patent CN110776616B discloses a highly efficient wetting water-based isocyanate curing agent, the trimer structure of which contains a highly polar alkynyl group and a hydrophilic sulfonic acid group, which improves the degree of ionization and enhances the emulsification effect of the water-based isocyanate curing agent; when mixed with water-based polyurethane, the contact area of ​​the water-based polyurethane adhesive on the substrate can be increased to improve the bonding strength. However, the proportion of sulfonic acid groups in the isocyanate curing agent prepared by the present invention is not large, its hydrophilicity can be further improved, and the stability period of the isocyanate curing agent needs to be extended. Summary of the invention

[0005] The object of the present invention is to provide a preparation method of an isocyanate curing agent and application thereof, so as to solve the technical problems of short stability period and poor hydrophilicity of the isocyanate curing agent in the prior art.

[0006] Compared with the prior art, the present invention has the following beneficial effects:

[0007] 1. The titanium dioxide added in the present invention is an inorganic material, which itself has a certain heat resistance. Appropriate addition will improve the thermal stability of the matrix. At the same time, titanium dioxide can absorb and scatter ultraviolet rays under ultraviolet light irradiation. Its anti-ultraviolet principle is mainly to achieve ultraviolet resistance by absorbing ultraviolet rays and converting them into heat energy, or by scattering ultraviolet rays. At the same time, due to its small size, titanium dioxide can be effectively avoided from agglomeration after modification, and can be evenly dispersed to maintain its functional stability. γ-(2,3-epoxypropoxy)propyltrimethoxysilane is an organic silane, in which the silicon-oxygen bond energy is large, which can effectively improve the thermal stability.

[0008] 2. The sulfonic acid group in the 3-aminopropane sulfonic acid of the present invention is an anionic hydrophilic modifier commonly used in isocyanate curing agents. The amino group in the 3-aminopropane sulfonic acid is subjected to a ring-opening reaction with the epoxy group in the epoxy-modified titanium dioxide to obtain sulfonated titanium dioxide containing secondary amine, hydroxyl and sulfonic acid groups. The sulfonated titanium dioxide is reacted with the polycarbonate diol to generate a modified polycarbonate diol containing an ether bond, which greatly increases the compatibility with the hexamethylene diisocyanate trimer and increases the hydrophilicity and storage stability of the isocyanate curing agent.

[0009] 3. The polycarbonate diol of the present invention has repeated carbonate chain segments on its main chain, which has strong cohesive strength and adhesion, high strength and wear resistance, and the chain end contains hydrophilic hydroxyl groups, which are easy to react with the hydroxyl groups in the sulfonated titanium dioxide to form ether bonds; the secondary amine in the modified polycarbonate diol reacts with the isocyanate group in the isocyanate, not only to generate a more stable group urea group, but also to improve the thermal stability, avoid the cross-linking and curing of compounds containing active hydrogen atoms such as alcohols, amines and water with highly reactive isocyanate groups at room temperature, and improve the storage stability of the isocyanate curing agent and the efficiency in practical applications. The invention adopts a mixed modification method for preparing the isocyanate curing agent, which can not only solve the problems of poor water resistance and high viscosity of the polycarbonate diol modified isocyanate curing agent, but also alleviate the problem that the sulfonate ion water-based polyisocyanate curing agent is sensitive to pH, so that the prepared water-based polyisocyanate curing agent has high compatibility and stability with the water-based hydroxyl component, and the introduced titanium dioxide as a heat-resistant material further improves the thermal stability of the isocyanate curing agent.

[0010] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for preparing an isocyanate curing agent and its application. The isocyanate curing agent prepared by the preparation process of the present invention has excellent ultraviolet absorption performance, hydrophilicity and storage stability.

[0011] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0012] A method for preparing an isocyanate curing agent comprises the following steps:

[0013] Step (1), mixing anhydrous ethanol, titanium dioxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane uniformly, heating, reacting, and after the reaction is completed, filtering, washing, and drying to obtain epoxy-modified titanium dioxide;

[0014] Step (2), mixing epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and hydrochloric acid aqueous solution uniformly, reacting, and after the reaction is completed, filtering, washing and drying to obtain sulfonated titanium dioxide;

[0015] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene, heating and reacting, and after the reaction is completed, washing and drying to obtain modified polycarbonate diol;

[0016] Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, heating and reacting, filtering after the reaction is completed to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting, cooling and distilling under reduced pressure to obtain an isocyanate curing agent.

[0017] Preferably, in (1), the mass ratio of anhydrous ethanol, titanium dioxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane is (1200-2800):100:(40-80).

[0018] Preferably, in (1), the reaction conditions are 60-80° C. and the reaction time is 2-4 h.

[0019] Preferably, in (2), the mass ratio of epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and aqueous hydrochloric acid solution is 60:200:(4000-6000); the reaction conditions are 70-90°C for 1-3h; and the concentration of aqueous hydrochloric acid solution is 0.01 mol / L.

[0020] Preferably, in step (3), the mass ratio of polycarbonate diol, sulfonated titanium dioxide and toluene is 200:(60-80):(4000-6000); and the reaction conditions are 60-80° C. for 4-6 hours.

[0021] Preferably, in step (3), the molecular weight of the polycarbonate diol is 1000.

[0022] Preferably, in step (4), the mass ratio of modified polycarbonate diol, hexamethylene diisocyanate trimer, toluene and triethylamine is (200-400):(60-120):(3000-6000):(100-200);

[0023] The reaction conditions for preparing the modified isocyanate are 40-60° C. for 1-2 hours.

[0024] Preferably, in step (4), the reaction conditions of the modified isocyanate and triethylamine are 20-40° C. for 0.5-1 h.

[0025] Preferably, the isocyanate curing agent is prepared by the above method.

[0026] Preferably, a method for preparing a coating using an isocyanate curing agent comprises the following steps:

[0027] The waterborne polyurethane resin, filler, pigment and isocyanate curing agent were stirred at room temperature and a stirring speed of 100 r / min for 20 minutes to obtain a coating;

[0028] The mass ratio of polyurethane resin, active diluent, filler and curing agent is (45-60):(4-8):(2-6):(10-25).

[0029] Preferably, the coating is prepared by the above method. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a flow chart for preparing an isocyanate curing agent in the present invention;

[0031] Figure 2 Schematic diagram of the process for preparing modified polycarbonate diol in the present invention;

[0032] Figure 3 It is a schematic diagram of the reaction for preparing sulfonated titanium dioxide in the present invention;

[0033] Figure 4 It is a bar graph showing the viscosity results of the storage stability test of the isocyanate curing agents prepared in Example 1 and Comparative Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] This embodiment provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0037] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 1200:100:40, reacting at 60° C. for 4 h, and after the reaction, filtering with suction, washing the filter cake with anhydrous ethanol, and drying at 100° C. for 3 h to obtain epoxy-modified titanium dioxide;

[0038] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:4000, reacted at 70° C. for 3 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 80° C. for 4 h to obtain sulfonated titanium dioxide;

[0039] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene in a mass ratio of 200:60:4000, reacting at 60° C. for 6 hours, washing with anhydrous ethanol after the reaction, and drying at 90° C. for 3 hours to obtain modified polycarbonate diol;

[0040] Step (4), mixing modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 40°C for 2h, and filtering after the reaction to obtain modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting at 20°C for 1h, and after the reaction is completed, cooling to room temperature, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0041] The mass ratio of the modified polycarbonate diol, the hexamethylene diisocyanate trimer, the toluene and the triethylamine is 200:60:3000:100.

[0042] Example 2

[0043] This embodiment provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0044] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 1600:100:50, reacting at 65°C for 3.5 hours, and after the reaction, filtering, washing the filter cake with anhydrous ethanol, and drying at 105°C for 2.5 hours to obtain epoxy-modified titanium dioxide;

[0045] Step (2), mixing epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution in a mass ratio of 60:200:4500, reacting at 75° C. for 2.5 h, filtering after the reaction, washing the filter cake with deionized water, and drying at 85° C. for 3.5 h to obtain sulfonated titanium dioxide;

[0046] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene in a mass ratio of 200:65:4500, reacting at 65° C. for 5.5 h, washing with anhydrous ethanol after the reaction, and drying at 95° C. for 2.5 h to obtain modified polycarbonate diol;

[0047] Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 45°C for 1.7h, and filtering after the reaction to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting at 25°C for 0.9h, and after the reaction is completed, cooling to room temperature, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0048] The mass ratio of modified polycarbonate diol, hexamethylene diisocyanate trimer, toluene and triethylamine is 250:75:3750:125.

[0049] Example 3

[0050] This embodiment provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0051] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 2000:100:60, reacting at 70°C for 3 hours, and after the reaction, filtering, washing the filter cake with anhydrous ethanol, and drying at 110°C for 2 hours to obtain epoxy-modified titanium dioxide;

[0052] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:5000, reacted at 80° C. for 2 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 90° C. for 3 h to obtain sulfonated titanium dioxide;

[0053] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene in a mass ratio of 200:70:5000, reacting at 70° C. for 5 h, washing with anhydrous ethanol after the reaction, and drying at 100° C. for 2 h to obtain a modified polycarbonate diol;

[0054] Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 50° C. for 1.5 h, and filtering after the reaction to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting at 30° C. for 0.7 h, and after the reaction is completed, cooling to room temperature, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0055] The mass ratio of the modified polycarbonate diol, the hexamethylene diisocyanate trimer, the toluene and the triethylamine is 300:90:4500:150.

[0056] Example 4

[0057] This embodiment provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0058] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 2400:100:70, reacting at 75°C for 2.5 hours, and after the reaction, filtering, washing the filter cake with anhydrous ethanol, and drying at 115°C for 1.5 hours to obtain epoxy-modified titanium dioxide;

[0059] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:5500, reacted at 85° C. for 1.5 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 95° C. for 2.5 h to obtain sulfonated titanium dioxide;

[0060] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene in a mass ratio of 200:75:5500, reacting at 75° C. for 4.5 hours, washing with anhydrous ethanol after the reaction, and drying at 105° C. for 1.5 hours to obtain modified polycarbonate diol;

[0061] Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 55° C. for 1.3 h, and filtering after the reaction to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting at 35° C. for 0.6 h, and after the reaction is completed, cooling to room temperature, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0062] The mass ratio of modified polycarbonate diol, hexamethylene diisocyanate trimer, toluene and triethylamine is 350:105:5250:175.

[0063] Example 5

[0064] This embodiment provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0065] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 2800:100:80, reacting at 80° C. for 2 h, and after the reaction, filtering with suction, washing the filter cake with anhydrous ethanol, and drying at 120° C. for 1 h to obtain epoxy-modified titanium dioxide;

[0066] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:6000, reacted at 90° C. for 1 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 100° C. for 2 h to obtain sulfonated titanium dioxide;

[0067] Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene in a mass ratio of 200:80:6000, reacting at 80° C. for 4 hours, washing with anhydrous ethanol after the reaction, and drying at 110° C. for 1 hour to obtain a modified polycarbonate diol;

[0068] Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 60° C. for 1 h, and filtering after the reaction to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting at 40° C. for 0.5 h, and cooling to room temperature after the reaction to obtain an isocyanate curing agent;

[0069] The mass ratio of the modified polycarbonate diol, the hexamethylene diisocyanate trimer, the toluene and the triethylamine is 400:120:6000:200.

[0070] Comparative Example 1

[0071] This comparative example provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0072] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 1200:100:40, reacting at 60° C. for 4 h, and after the reaction, filtering with suction, washing the filter cake with anhydrous ethanol, and drying at 100° C. for 3 h to obtain epoxy-modified titanium dioxide;

[0073] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:4000, reacted at 70° C. for 3 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 80° C. for 4 h to obtain sulfonated titanium dioxide;

[0074] Step (3), mixing polycarbonate diol, hexamethylene diisocyanate trimer and toluene, reacting at 60°C for 4h, after the reaction is completed, filtering with suction, washing with anhydrous ethanol for 3 times to obtain intermediate I; adding sulfonated titanium dioxide to intermediate I, physically mixing evenly, filtering with suction, to obtain modified isocyanate; under an inert gas protection environment, adding triethylamine to the modified isocyanate, reacting at 20°C for 1h, after the reaction is completed, cooling to room temperature, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0075] The mass ratio of sulfonated titanium dioxide, polycarbonate diol, hexamethylene diisocyanate trimer, toluene and triethylamine is 60:200:60:3000:100.

[0076] Comparative Example 2

[0077] This comparative example provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0078] Step (1), mixing anhydrous ethanol, titanium dioxide, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane in a mass ratio of 1200:100:40, reacting at 60° C. for 4 h, and after the reaction, filtering with suction, washing the filter cake with anhydrous ethanol, and drying at 100° C. for 3 h to obtain epoxy-modified titanium dioxide;

[0079] Step (2), epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and 0.01 mol / L hydrochloric acid aqueous solution are mixed uniformly according to a mass ratio of 60:200:4000, reacted at 70° C. for 3 h, and after the reaction is completed, filtered, the filter cake is washed with deionized water, and dried at 80° C. for 4 h to obtain sulfonated titanium dioxide;

[0080] Step (3), uniformly mixing sulfonated titanium dioxide, hexamethylene diisocyanate trimer and toluene, reacting at 40°C for 2h, and filtering after the reaction to obtain modified isocyanate; adding triethylamine under an inert gas protection environment, reacting at 20°C for 1h, and cooling to room temperature after the reaction, and distilling under reduced pressure to obtain an isocyanate curing agent;

[0081] The mass ratio of sulfonated titanium dioxide, hexamethylene diisocyanate trimer, toluene and triethylamine is 60:60:3000:100.

[0082] Comparative Example 3

[0083] This comparative example provides a method for preparing an isocyanate curing agent, comprising the following steps:

[0084] 3-aminopropane sulfonic acid, hexamethylene diisocyanate trimer and toluene were mixed evenly, reacted at 40°C for 2h, and after the reaction was completed, filtered to obtain modified isocyanate; triethylamine was added under an inert gas protection environment, reacted at 20°C for 1h, and after the reaction was completed, cooled to room temperature, and distilled under reduced pressure to obtain an isocyanate curing agent;

[0085] The mass ratio of 3-aminopropane sulfonic acid, hexamethylene diisocyanate trimer, toluene and triethylamine is 60:60:3000:100.

[0086] In each embodiment and comparative example of the present invention, titanium dioxide was purchased from Xuancheng Jingrui New Materials Co., Ltd., model JR05, and the average particle size was 5 nm; toluene was from Tianjin Fuyu Fine Chemical Co., Ltd., CAS No. 108-88-3; hexamethylene diisocyanate trimer was purchased from Wanhua Chemical Group Co., Ltd., specification HT-100, industrial grade; triethylamine was purchased from Shanghai Mairui Chemical Technology Co., Ltd., CAS No.: 121-44-8; polycarbonate diol was purchased from Asahi Chemical T5651 of Japan, with a molecular weight of 1000; 3-aminopropane sulfonic acid was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd. CAS No.: 3687-18-1.

[0087] The isocyanate curing agents prepared in Examples 1-5 and Comparative Examples 1-3 were selected as samples and subjected to corresponding tests.

[0088] (1) Anti-ultraviolet performance test: The test was carried out using a Japanese Shimadzu UV-3600 spectrophotometer, and the test referred to the national standard GB / T2680-2021; the results of the above tests are recorded in Table 1:

[0089] Table 1

[0090]

[0091]

[0092] From the test results of Table 1, it can be seen that the isocyanate curing agent corresponding to Examples 1-5 has ultraviolet absorption performance, and the main function is the added titanium dioxide. The higher the content of titanium dioxide, the better the dispersibility, and the ultraviolet absorption performance of the titanium dioxide itself is more prominent. Compared with Example 1, titanium dioxide is not grafted into the hexamethylene diisocyanate trimer in Comparative Example 1, and its dispersibility is lower than that of Example 1, and the generation of agglomeration is not conducive to ultraviolet absorption performance; Compared with Comparative Example 1, the secondary amine in the sulfonated titanium dioxide reacts with the isocyanate in the hexamethylene diisocyanate trimer to connect the two, lacking polycarbonate diol, the chain entanglement between molecules is strengthened, the crosslinking density is high, the nitrogen atoms and oxygen atoms in the sulfonated titanium dioxide are conducive to the formation of hydrogen bonds, and the dispersibility is lower than that of Comparative Example 1, so the ultraviolet absorption performance is reduced; Compared with Comparative Example 2, Comparative Example 3 lacks titanium dioxide with ultraviolet absorption ability, and its ultraviolet absorption rate is lower than the ultraviolet absorption rate in Comparative Example 2.

[0093] (2) Storage stability test: According to the national standard GB / T6753.3-1986 "Test method for storage stability of coatings", the storage stability test of the isocyanate curing agent is carried out. The specific operation method is: the isocyanate curing agents prepared in Example 1 and Comparative Examples 1-3 are respectively loaded into 8 0.4L standard pressure-capped metal paint cans, and the samples are loaded to about 15mm from the top of the can. The two cans of samples are sealed with lids and stored, respectively placed at room temperature and in an oven at a temperature of 50±2°C. After 7 days, the values ​​of the -NCO content and viscosity of the curing agent stored in the two environments are respectively measured. The results of the above tests are recorded as shown in Table 2:

[0094] Table 2

[0095]

[0096]

[0097] As shown in Table 2, the isocyanate curing agent in Example 1 prepared by the present invention has good storage stability performance. Comparative Example 1 is compared with Example 1, and the intermediate I is obtained by polycarbonate diol and polyhexamethylene diisocyanate trimer, which has certain thermal stability. The hydrophilicity is improved by adding sulfonated titanium dioxide having both hydrophilic and heat-resistant properties, and the water dispersibility is improved, but its dispersibility is not as good as that of Example 1, so the storage stability effect is lower than that of Example 1; Comparative Example 2 is compared with Comparative Example 1, lacking polycarbonate diol added to hexamethylene diisocyanate trimer, the chain entanglement between hexamethylene diisocyanate trimer molecules is strengthened, the intermolecular force is large, and the hydration of water to isocyanate is improved, so the storage stability performance is reduced; Comparative Example 3 is compared with Comparative Example 2, and the introduction of heat-resistant material titanium dioxide and organosilicon can effectively improve the thermal stability of the two-component waterborne polyurethane coating, and the introduction of organosilicon, the silicon oxygen bond energy is large, can effectively improve the thermal stability, once it is lacking, its stability performance naturally decreases.

[0098] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing an isocyanate curing agent, It is characterized in that The following steps are involved: Step (1), mixing anhydrous ethanol, titanium dioxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane uniformly, heating, reacting, and after the reaction is completed, filtering, washing, and drying to obtain epoxy-modified titanium dioxide; Step (2), mixing epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and hydrochloric acid aqueous solution uniformly, reacting, and after the reaction is completed, filtering, washing and drying to obtain sulfonated titanium dioxide; Step (3), mixing polycarbonate diol, sulfonated titanium dioxide and toluene, heating and reacting, and after the reaction is completed, washing and drying to obtain modified polycarbonate diol; Step (4), mixing the modified polycarbonate diol, hexamethylene diisocyanate trimer and toluene, heating and reacting, filtering after the reaction is completed to obtain a modified isocyanate; adding triethylamine to the modified isocyanate system under an inert gas protection environment, reacting, cooling and distilling under reduced pressure to obtain an isocyanate curing agent.

2. A method for preparing an isocyanate curing agent according to claim 1, Features: In the above (1), the mass ratio of anhydrous ethanol, titanium dioxide and γ-(2,3-epoxypropoxy)propyltrimethoxysilane is (1200-2800):100:(40-80).

3. A method for preparing an isocyanate curing agent according to claim 1, Features: In the above (1), the reaction conditions are 60-80°C and the reaction time is 2-4h.

4. The method for preparing an isocyanate curing agent according to claim 1, Features: In the method (2), the mass ratio of epoxy-modified titanium dioxide, 3-aminopropane sulfonic acid and aqueous hydrochloric acid solution is 60:200:(4000-6000); the reaction conditions are 70-90° C. for 1-3 hours; and the concentration of aqueous hydrochloric acid solution is 0.01 mol / L.

5. The method for preparing an isocyanate curing agent according to claim 1, Features: In the step (3), the mass ratio of polycarbonate diol, sulfonated titanium dioxide and toluene is 200:(60-80):(4000-6000); the reaction conditions are 60-80° C. for 4-6 hours.

6. The method for preparing an isocyanate curing agent according to claim 1, Features: In the step (3), the molecular weight of the polycarbonate diol is 1000.

7. The method for preparing an isocyanate curing agent according to claim 1, Features: In the step (4), the mass ratio of modified polycarbonate diol, hexamethylene diisocyanate trimer, toluene and triethylamine is (200-400):(60-120):(3000-6000):(100-200); The reaction conditions for preparing the modified isocyanate are 40-60° C. for 1-2 hours.

8. The method for preparing an isocyanate curing agent according to claim 1, Features: In the step (4), the reaction conditions of the modified isocyanate and triethylamine are 20-40° C. and 0.5-1 h.

9. An isocyanate curing agent prepared by the preparation method of the isocyanate curing agent according to any one of claims 1 to 8.

10. Use of the isocyanate curing agent according to claim 9 in coatings.