A biodegradable composite material based on bamboo fiber powder and preparation method thereof
By generating nano-silica in bamboo fiber powder and modifying treatment, combined with vinyl silane coupling agent, the problems of low-temperature brittleness, heat-resistant oxygen aging and flammability of polypropylene materials are solved, and the biomass composite materials are improved Mechanical and UV aging resistance extend product life.
Patent Information
- Application Number
- CN202411134382.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing polypropylene materials have enhanced brittleness under low temperature conditions, weak thermal oxygen aging resistance, low transparency, flammable and insufficient dimensional stability, which limits their use in certain application fields.
Using the preparation method of bio-based degradable composite materials based on bamboo fiber powder, nano-silica is generated through hydrothermal reaction, and the modified bamboo fiber powder is coupled with gamma-glycidyl ether oxypropyl trimethoxysilane and vinyl silane coupling agent Treatment to enhance the mechanical and UV aging resistance of composite materials.
It improves the mechanical properties, heat resistance and UV aging resistance of composite materials, enhances structural stability and impact strength, and extends the service life of the product.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material preparation, and in particular to a bio-based degradable composite material based on bamboo fiber powder and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a thermoplastic resin with a highly crystalline structure. Its odorless, non-toxic and lightweight properties make it popular in many fields. As an important engineering plastic, PP has been widely used in the automotive industry, home appliances, packaging, building materials, furniture manufacturing and other industries due to its good physical and mechanical properties, low cost and excellent processability.
[0003] However, existing polypropylene materials still have obvious defects in some properties and are in urgent need of improvement and enhancement. First, PP has relatively poor toughness, especially under low temperature conditions, its brittleness increases, and it is easy to crack and deform; second, PP has weak thermal oxygen aging resistance, and is easily affected by oxygen and heat during long-term use, which can easily cause material degradation, discoloration, and mechanical property degradation; in addition, the low transparency of PP materials limits its application in certain fields with high visual effects requirements, and the flammability of the material also increases the risk of its use in certain environments; in addition, due to the insufficient dimensional stability of PP, especially in outdoor environments, under the influence of ultraviolet radiation, its products are prone to powdering, surface cracking, gloss loss, and a significant decrease in mechanical properties, which seriously restricts the service life and stability of PP products.
[0004] Moso bamboo is a fast-growing plant with very high biomass and cellulose content. It is widely planted in many areas of Southeast Asia and China. Moso bamboo fiber has good tensile strength and rigidity, which enables it to play a reinforcing role in composite materials. Its high modulus and low density characteristics make it practical in various engineering applications. Compared with traditional plastic materials, composite materials based on moso bamboo fiber are more easily degraded in the environment and can effectively reduce plastic pollution. Compounding moso bamboo fiber with polypropylene material is expected to solve the shortcomings of traditional polypropylene materials. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a bio-based degradable composite material based on bamboo fiber powder and a preparation method thereof, wherein the prepared composite material has excellent mechanical properties, heat resistance and UV aging resistance.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme:
[0007] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0008] S1, dispersing bamboo fiber powder in ethanol aqueous solution, then adding tetraethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate thereto, hydrothermally reacting, after the reaction is completed, filtering, washing and drying to obtain pretreated bamboo fiber powder;
[0009] S2, dispersing the pretreated bamboo fiber powder in an ethanol aqueous solution, then adding γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 40-60° C. for 1-4 hours, and after the reaction is completed, filtering, washing, and drying to obtain modified bamboo fiber powder;
[0010] S3, dispersing the chopped carbon fibers in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, stirring at 40-60° C. for 1-3 hours, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fibers;
[0011] S4, dispersing the pretreated carbon fiber in an organic solvent, then adding styrene, cinnamamide and benzoyl peroxide thereto, heating for reaction, and after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0012] S5. Add modified bamboo fiber powder, modified carbon fiber, polypropylene, PP grafted maleic anhydride, plasticizer, antioxidant and flame retardant into a high-speed mixer and mix at room temperature to obtain a premix. Then, add the premix into a twin-screw extruder for extrusion granulation and hot air drying to obtain a bio-based degradable composite material.
[0013] Specifically, in step S1, the mass ratio of bamboo fiber powder, tetraethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate is 10-15:8-12:30-50:1-1.5, wherein the mass fraction of ammonia water is 20-30%.
[0014] Specifically, in step S1, the temperature of the hydrothermal reaction is 120-150° C., and the time of the hydrothermal reaction is 12-18 hours.
[0015] Specifically, in step S2, the mass ratio of the pretreated bamboo fiber powder to γ-glycidyloxypropyltrimethoxysilane is 10-15:1-3.
[0016] Specifically, in step S3, the mass ratio of the chopped carbon fiber to the vinyl silane coupling agent is 8-12:1-3, wherein the vinyl silane coupling agent is selected from vinyl trimethoxy silane, vinyl triethoxy silane or vinyl trichlorosilane.
[0017] Specifically, in step S4, the mass ratio of the pretreated carbon fiber, styrene, cinnamamide and benzoyl peroxide is 10-15:4-8:3-6:0.5-1.
[0018] Specifically, in step S4, the heating reaction temperature is 80-90° C., and the heating reaction time is 3-5 h.
[0019] Specifically, in step S5, the mass ratio of the modified bamboo fiber powder, the modified carbon fiber, the polypropylene, the PP grafted maleic anhydride, the plasticizer, the antioxidant and the flame retardant is 40-50:4-8:60-80:5-10:2-4:1-2:1-1.5.
[0020] Specifically, in step S5, the plasticizer is selected from tributyl citrate, polyethylene glycol or polypropylene glycol, the antioxidant is selected from antioxidant 1010 or antioxidant 1076, and the flame retardant is selected from antimony trioxide or aluminum hydroxide.
[0021] The present invention also provides a bio-based degradable composite material prepared by the above preparation method.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The surface of the bamboo fiber powder provided by the present invention is formed by cellulose, hemicellulose and lignin connected by hydrogen bonds. The gaps between the fiber molecules are relatively large and the thermal stability is not ideal. The present invention generates nano-silicon dioxide in situ on the surface and in the pore structure of the bamboo fiber powder through a hydrothermal synthesis method. The nano-silicon dioxide has a large specific surface area. At high temperatures, the nano-silicon dioxide can effectively absorb and dissipate heat, reduce the local temperature of the bamboo fiber, thereby slowing down the thermal degradation rate of the bamboo fiber, and at the same time improving the anti-ultraviolet aging performance of the composite material; in addition, the nano-silicon dioxide can also enhance the mechanical properties of the bamboo fiber, thereby improving the overall structural stability of the composite material, especially improving the impact strength of the composite material.
[0024] (2) The present invention improves the compatibility between the pretreated bamboo fiber powder and other raw materials by treating the pretreated bamboo fiber powder with γ-glycidyloxypropyltrimethoxysilane, and at the same time enhances the binding force between the pretreated bamboo fiber powder and other raw materials by introducing epoxy groups, thereby enhancing the mechanical properties of the composite material.
[0025] (3) The present invention uses a vinyl silane coupling agent to pretreat the chopped carbon fibers, introduces carbon-carbon double bonds on the surface of the chopped carbon fibers, and then introduces a polymer to the surface of the chopped carbon fibers through an addition reaction between the double bonds of styrene and cinnamamide. Aromatic structural units exist between the polymer molecular chains, showing stronger conjugation than linear polypropylene. Due to the conjugation effect, electrons are delocalized, molecular bond energy tends to be averaged, energy is reduced, and stability can be maintained even at high temperatures, effectively improving the UV aging resistance of the composite material; at the same time, by grafting a high molecular weight polymer on the surface of the chopped carbon fibers, the compatibility of the chopped carbon fibers with other raw materials is improved, and the mechanical properties of the composite material are further improved. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0027] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0028] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0029] S1. Preparation of pretreated bamboo fiber powder
[0030] The bamboo fiber powder is dispersed in an ethanol aqueous solution, and then ethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate are added thereto for hydrothermal reaction. After the reaction is completed, the pretreated bamboo fiber powder is obtained by filtering, washing and drying.
[0031] In this step, the mass ratio of bamboo fiber powder, tetraethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate is 10-15:8-12:30-50:1-1.5, and more preferably 12-14:9-10:35-40:1.2-1.4.
[0032] Among them, the mass fraction of ammonia water is 20-30%. In some embodiments of the present invention, for example, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, and 30% can be selected, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] In this step, the mass fraction of the ethanol aqueous solution is 60-80%, for example, 60%, 65%, 70%, 75%, 80% can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] In this step, the temperature of the hydrothermal reaction is 120-150°C, for example, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C can be selected; the time of the hydrothermal reaction is 12-18h, for example, 12h, 13h, 14h, 15h, 16h, 17h, 18h can be selected; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0035] In this step, the surface of the bamboo fiber powder is formed by cellulose, hemicellulose, and lignin connected by hydrogen bonds, the gaps between the fiber molecules are relatively large, and the thermal stability is not ideal. The present invention generates nano-silicon dioxide in situ on the surface and pore structure of the bamboo fiber powder through a hydrothermal synthesis method. The nano-silicon dioxide has a large specific surface area. At high temperatures, the nano-silicon dioxide can effectively absorb and dissipate heat, reduce the local temperature of the bamboo fiber that is heated, thereby slowing down the thermal degradation rate of the bamboo fiber, and at the same time improving the anti-ultraviolet aging performance of the composite material; in addition, the nano-silicon dioxide can also enhance the mechanical properties of the bamboo fiber, thereby improving the overall structural stability of the composite material, especially improving the impact strength of the composite material.
[0036] S2. Preparation of modified bamboo fiber powder
[0037] The pretreated bamboo fiber powder is dispersed in an ethanol aqueous solution, and then γ-glycidyloxypropyltrimethoxysilane is added thereto, and stirred at 40-60° C. for 1-4 hours. After the reaction is completed, the modified bamboo fiber powder is obtained by filtering, washing and drying.
[0038] In this step, the mass ratio of the pretreated bamboo fiber powder to γ-glycidyloxypropyltrimethoxysilane is 10-15:1-3, and more preferably 12-14:1.5-2.
[0039] In this step, the mass fraction of the ethanol aqueous solution is 60-80%, for example, 60%, 65%, 70%, 75%, 80% can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In this step, the pretreated bamboo fiber powder is treated with γ-glycidyloxypropyltrimethoxysilane to improve the compatibility between the pretreated bamboo fiber powder and other raw materials. At the same time, by introducing epoxy groups, the binding force between the pretreated bamboo fiber powder and other raw materials is enhanced, thereby enhancing the mechanical properties of the composite material.
[0041] S3. Preparation of pretreated carbon fiber
[0042] The short chopped carbon fibers are dispersed in an ethanol aqueous solution, and then a vinyl silane coupling agent is added thereto, and stirred at 40-60° C. for 1-3 hours. After the reaction is completed, the pretreated carbon fibers are obtained by filtering, washing, and drying.
[0043] In this step, the mass ratio of the chopped carbon fiber to the vinyl silane coupling agent is 8-12:1-3, and more preferably 9-10:1.5-2.
[0044] Wherein, the vinyl silane coupling agent is selected from vinyl trimethoxy silane, vinyl triethoxy silane or vinyl trichloro silane.
[0045] In this step, the mass fraction of the ethanol aqueous solution is 60-80%, for example, 60%, 65%, 70%, 75%, 80% can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] In this step, the chopped carbon fibers are surface treated with a vinyl silane coupling agent to introduce carbon-carbon double bonds on the surface of the chopped carbon fibers, which is beneficial to the subsequent reaction.
[0047] S4. Preparation of modified carbon fiber
[0048] The pretreated carbon fiber is dispersed in an organic solvent, and then styrene, cinnamamide and benzoyl peroxide are added thereto, and heated to react. After the reaction is completed, the modified carbon fiber is obtained by filtering, washing and drying.
[0049] In this step, the mass ratio of the pretreated carbon fiber, styrene, cinnamamide and benzoyl peroxide is 10-15:4-8:3-6:0.5-1, and more preferably 12-14:5-6:4-5:0.6-0.8.
[0050] In this step, the temperature of the heating reaction is 80-90°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, and 90°C can be selected; the heating reaction time is 3-5h, for example, 3h, 3.5h, 4h, 4.5h, and 5h can be selected; but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0051] In this step, a double bond addition reaction occurs between the double bonds on the surface of the chopped carbon fibers and styrene and cinnamamide, and the polymer is introduced onto the surface of the chopped carbon fibers. Aromatic structural units exist between the polymer molecular chains, which exhibit stronger conjugation than linear polypropylene. Due to the conjugation effect, electrons are delocalized, molecular bond energy tends to be averaged, energy is reduced, and stability can be maintained even at high temperatures, thereby effectively improving the resistance of the composite material to ultraviolet aging. At the same time, cinnamamide contains amino active groups, which can chemically combine with the epoxy groups on the surface of the modified bamboo fiber powder, further enhancing the mechanical properties of the composite material.
[0052] S5. Preparation of bio-based degradable composite materials
[0053] Modified bamboo fiber powder, modified carbon fiber, polypropylene, PP grafted maleic anhydride, plasticizer, antioxidant and flame retardant are added into a high-speed mixer and mixed at room temperature to obtain a premix. Subsequently, the premix is added into a twin-screw extruder for extrusion granulation and hot air drying to obtain a bio-based degradable composite material.
[0054] In this step, the mass ratio of modified bamboo fiber powder, modified carbon fiber, polypropylene, PP grafted maleic anhydride, plasticizer, antioxidant and flame retardant is 40-50:4-8:60-80:5-10:2-4:1-2:1-1.5, and more preferably 42-46:5-6:65-70:6-8:2.5-3:1.4-1.8:1.2-1.3.
[0055] Wherein, the plasticizer is selected from tributyl citrate, polyethylene glycol or polypropylene glycol; the antioxidant is selected from antioxidant 1010 or antioxidant 1076; and the flame retardant is selected from antimony trioxide or aluminum hydroxide.
[0056] The specific process of extrusion granulation is as follows: add the above-mentioned premix into a twin-screw extruder, set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding speed is 120r / min, the screw speed is 300r / min, extrude granulate, then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a composite material.
[0057] The present invention is further illustrated by specific embodiments below. The mesh size of the bamboo fiber powder used in the present invention is 200 meshes; the chopped carbon fiber is purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd., with a diameter of 5-10 μm; the grade of polypropylene is RX3600, purchased from Shanghai Jinsuda Plastic Co., Ltd.; the model of PP grafted maleic anhydride is MP150, purchased from Wuxi Yiyuan New Materials Technology Co., Ltd.; the particle size of antimony trioxide is 80-100 nm; the mesh size of aluminum hydroxide is 3000 meshes.
[0058] Example 1
[0059] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0060] S1, 10g of bamboo fiber powder was dispersed in 100mL, 80wt% ethanol aqueous solution, and then 8g of tetraethyl orthosilicate, 30g, 25wt% ammonia water and 1g of sodium dodecylbenzene sulfonate were added thereto, and the mixture was hydrothermally reacted at 120°C for 18h. After the reaction was completed, the mixture was filtered, washed and dried to obtain pretreated bamboo fiber powder;
[0061] S2, dispersing 10g of pretreated bamboo fiber powder in 100mL, 80wt% ethanol aqueous solution, then adding 1g of γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 40°C for 3h, after the reaction is completed, filtering, washing and drying to obtain modified bamboo fiber powder;
[0062] S3, dispersing 8 g of chopped carbon fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, stirring at 40 ° C for 3 h, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fiber;
[0063] S4, dispersing 10g of pretreated carbon fiber in 150mL of organic solvent DMF, then adding 4g of styrene, 3g of cinnamamide and 0.5g of benzoyl peroxide thereto, heating at 80°C for reaction for 5h, after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0064] S5. Add 40 parts of modified bamboo fiber powder, 4 parts of modified carbon fiber, 60 parts of polypropylene, 5 parts of PP grafted maleic anhydride, 2 parts of plasticizer tributyl citrate, 1 part of antioxidant 1010 and 1 part of flame retardant antimony trioxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the premix into a twin-screw extruder. Set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a bio-based degradable composite material.
[0065] Example 2
[0066] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0067] S1, 15g of bamboo fiber powder was dispersed in 100mL, 80wt% ethanol aqueous solution, and then 12g of tetraethyl orthosilicate, 50g, 25wt% ammonia water and 1.5g of sodium dodecylbenzene sulfonate were added thereto, and the mixture was hydrothermally reacted at 150°C for 12h. After the reaction was completed, the mixture was filtered, washed and dried to obtain pretreated bamboo fiber powder;
[0068] S2, dispersing 15g of pretreated bamboo fiber powder in 100mL, 80wt% ethanol aqueous solution, then adding 3g of γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 60°C for 1h, after the reaction is completed, filtering, washing and drying to obtain modified bamboo fiber powder;
[0069] S3, dispersing 12 g of chopped carbon fibers in 100 mL of 80 wt% ethanol aqueous solution, then adding 3 g of vinyl triethoxysilane thereto, stirring at 60 ° C for 2 h, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fibers;
[0070] S4, dispersing 15g of pretreated carbon fiber in 150mL of organic solvent DMF, then adding 8g of styrene, 6g of cinnamamide and 1g of benzoyl peroxide thereto, heating at 90°C for reaction for 3h, and after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0071] S5. Add 50 parts of modified bamboo fiber powder, 6 parts of modified carbon fiber, 80 parts of polypropylene, 8 parts of PP grafted maleic anhydride, 4 parts of plasticizer polyethylene glycol 4000, 2 parts of antioxidant 1010 and 1.5 parts of flame retardant antimony trioxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the premix into a twin-screw extruder. Set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a bio-based degradable composite material.
[0072] Example 3
[0073] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0074] S1, 12g of bamboo fiber powder was dispersed in 100mL, 80wt% ethanol aqueous solution, and then 10g of tetraethyl orthosilicate, 40g, 25wt% ammonia water and 1.2g of sodium dodecylbenzene sulfonate were added thereto, and the mixture was hydrothermally reacted at 150°C for 18h. After the reaction was completed, the mixture was filtered, washed and dried to obtain pretreated bamboo fiber powder;
[0075] S2, dispersing 12g of pretreated bamboo fiber powder in 100mL, 80wt% ethanol aqueous solution, then adding 2g of γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 50°C for 3h, after the reaction is completed, filtering, washing and drying to obtain modified bamboo fiber powder;
[0076] S3, dispersing 10 g of chopped carbon fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyl triethoxysilane thereto, stirring at 60 ° C for 2 h, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fiber;
[0077] S4, dispersing 12g of pretreated carbon fiber in 150mL of organic solvent DMF, then adding 6g of styrene, 6g of cinnamamide and 1g of benzoyl peroxide thereto, heating at 80°C for reaction for 5h, after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0078] S5. Add 45 parts of modified bamboo fiber powder, 8 parts of modified carbon fiber, 65 parts of polypropylene, 10 parts of PP grafted maleic anhydride, 3 parts of plasticizer polyethylene glycol 4000, 2 parts of antioxidant 1010 and 1.5 parts of flame retardant aluminum hydroxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the premix into a twin-screw extruder. Set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a bio-based degradable composite material.
[0079] Example 4
[0080] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0081] S1, 14g of bamboo fiber powder was dispersed in 100mL, 80wt% ethanol aqueous solution, and then 9g of tetraethyl orthosilicate, 35g, 25wt% ammonia water and 1.4g of sodium dodecylbenzene sulfonate were added thereto, and the mixture was hydrothermally reacted at 130°C for 18h. After the reaction was completed, the mixture was filtered, washed and dried to obtain pretreated bamboo fiber powder;
[0082] S2, dispersing 12g of pretreated bamboo fiber powder in 100mL, 80wt% ethanol aqueous solution, then adding 2.5g of γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 50°C for 3h, after the reaction is completed, filtering, washing and drying to obtain modified bamboo fiber powder;
[0083] S3, dispersing 10 g of chopped carbon fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1.5 g of vinyl triethoxysilane thereto, stirring at 60 ° C for 2 h, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fiber;
[0084] S4, dispersing 12g of pretreated carbon fiber in 150mL of organic solvent DMF, then adding 5g of styrene, 5g of cinnamamide and 0.8g of benzoyl peroxide thereto, heating at 85°C for 4h, after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0085] S5. Add 42 parts of modified bamboo fiber powder, 5 parts of modified carbon fiber, 70 parts of polypropylene, 6 parts of PP grafted maleic anhydride, 2 parts of plasticizer tributyl citrate, 1.5 parts of antioxidant 1076 and 1.5 parts of flame retardant aluminum hydroxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the premix into a twin-screw extruder. Set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a bio-based degradable composite material.
[0086] Comparative Example 1
[0087] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0088] S1, dispersing 8 g of chopped carbon fiber in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, stirring at 40 ° C for 3 h, after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fiber;
[0089] S2, dispersing 10g of pretreated carbon fiber in 150mL of organic solvent DMF, then adding 4g of styrene, 3g of cinnamamide and 0.5g of benzoyl peroxide thereto, heating at 80°C for reaction for 5h, after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber;
[0090] S3. Add 40 parts of bamboo fiber powder, 4 parts of modified carbon fiber, 60 parts of polypropylene, 5 parts of PP grafted maleic anhydride, 2 parts of plasticizer tributyl citrate, 1 part of antioxidant 1010 and 1 part of flame retardant antimony trioxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the above premix into a twin-screw extruder, and set the twin-screw extruder to the following working parameters: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, and then dry in a hot air environment at 80°C for 3h, cool to room temperature, and obtain a bio-based degradable composite material.
[0091] Compared with Example 1, Comparative Example 1 did not perform modification treatment on the bamboo fiber powder.
[0092] Comparative Example 2
[0093] A method for preparing a bio-based degradable composite material based on bamboo fiber powder comprises the following steps:
[0094] S1, 10g of bamboo fiber powder was dispersed in 100mL, 80wt% ethanol aqueous solution, and then 8g of tetraethyl orthosilicate, 30g, 25wt% ammonia water and 1g of sodium dodecylbenzene sulfonate were added thereto, and the mixture was hydrothermally reacted at 120°C for 18h. After the reaction was completed, the mixture was filtered, washed and dried to obtain pretreated bamboo fiber powder;
[0095] S2, dispersing 10g of pretreated bamboo fiber powder in 100mL, 80wt% ethanol aqueous solution, then adding 1g of γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 40°C for 3h, after the reaction is completed, filtering, washing and drying to obtain modified bamboo fiber powder;
[0096] S3. Add 40 parts of modified bamboo fiber powder, 4 parts of chopped carbon fibers, 60 parts of polypropylene, 5 parts of PP grafted maleic anhydride, 2 parts of plasticizer tributyl citrate, 1 part of antioxidant 1010 and 1 part of flame retardant antimony trioxide into a high-speed mixer and mix at room temperature to obtain a premix. Add the premix into a twin-screw extruder. Set the working parameters of the twin-screw extruder as follows: the temperature of zone 1 is 130°C, the temperature of zone 2 is 180°C, the temperature of zone 3 is 190°C, the temperature of zone 4 is 170°C, the temperature of zone 5 is 180°C, the temperature of die head is 160°C, the feeding rate is 120r / min, the screw speed is 300r / min, extrude and granulate, then dry in a hot air environment at 80°C for 3h, and cool to room temperature to obtain a bio-based degradable composite material.
[0097] Compared with Example 1, in Comparative Example 2, the chopped carbon fibers were not modified.
[0098] The composite materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to performance tests, as follows:
[0099] Tensile property test: According to GB / T 1040-2006 standard, at a temperature of 25±1℃, dumbbell-shaped samples were used for measurement, and the measurement rate was 50mm / min. Each group of samples was tested 3 times and the average value was taken.
[0100] Impact resistance test: The sample material is hot pressed into a 3mm×10mm×80mm specimen at 200℃, and then a 45° V-shaped notch (upper radius is 0.25mm, notch depth is 2mm) is processed in the middle of the sample as the test sample. All tests are carried out at room temperature, and each group of samples is tested 3 times and the average value is taken;
[0101] Thermal stability test: The thermal stability test was conducted by thermogravimetric analysis in a nitrogen environment. The sample mass was 5 mg, the heating rate was 10 °C / min, and the test temperature range was from room temperature to 600 °C. Each group of samples was tested 3 times and the average value was taken.
[0102] The test results are shown in Table 1 below:
[0103] Table 1
[0104] Tensile strength (MPa) <![CDATA[Notched impact strength (kJ / m 2 ).]]> Initial thermal decomposition temperature (℃) Example 1 32.43 14.31 326.4 Example 2 31.56 15.02 317.3 Example 3 32.71 14.48 331.6 Example 4 31.85 14.86 320.9 Comparative Example 1 27.37 9.75 289.1 Comparative Example 2 26.82 12.64 311.2
[0105] The composite materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to ultraviolet irradiation. A 500W Ga-In ultraviolet lamp was used to irradiate each group of materials for 48 hours. The tensile strength and notched impact strength of each group of materials were then tested. The test results are shown in Table 2:
[0106] Table 2
[0107] Tensile strength (MPa) <![CDATA[Notched impact strength (kJ / m 2 ).]]> Example 1 32.04 13.86 Example 2 30.96 14.29 Example 3 32.17 13.75 Example 4 31.23 14.12 Comparative Example 1 22.59 7.48 Comparative Example 2 19.45 7.11
[0108] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A method for preparing a bio-based degradable composite material based on bamboo fiber powder, characterized in that: The steps include: S1, dispersing bamboo fiber powder in ethanol aqueous solution, then adding tetraethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate thereto, hydrothermally reacting, after the reaction is completed, filtering, washing and drying to obtain pretreated bamboo fiber powder; S2, dispersing the pretreated bamboo fiber powder in an ethanol aqueous solution, then adding γ-glycidyloxypropyltrimethoxysilane thereto, stirring at 40-60° C. for 1-4 hours, and after the reaction is completed, filtering, washing, and drying to obtain modified bamboo fiber powder; S3, dispersing the chopped carbon fibers in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, stirring at 40-60° C. for 1-3 hours, and after the reaction is completed, filtering, washing, and drying to obtain pretreated carbon fibers; S4, dispersing the pretreated carbon fiber in an organic solvent, then adding styrene, cinnamamide and benzoyl peroxide thereto, heating for reaction, and after the reaction is completed, filtering, washing and drying to obtain modified carbon fiber; S5, adding modified bamboo fiber powder, modified carbon fiber, polypropylene, PP grafted maleic anhydride, plasticizer, antioxidant and flame retardant into a high-speed mixer and mixing at room temperature to obtain a premix, then adding the premix into a twin-screw extruder for extrusion granulation, and hot air drying to obtain a bio-based degradable composite material; Wherein, in step S1, the mass ratio of bamboo fiber powder, tetraethyl orthosilicate, ammonia water and sodium dodecylbenzene sulfonate is 10-15:8-12:30-50:1-1.5, wherein the mass fraction of ammonia water is 20-30%; In step S1, the temperature of the hydrothermal reaction is 120-150° C., and the time of the hydrothermal reaction is 12-18 hours; In step S2, the mass ratio of the pretreated bamboo fiber powder to γ-glycidyloxypropyltrimethoxysilane is 10-15:1-3; In step S3, the mass ratio of the chopped carbon fiber to the vinyl silane coupling agent is 8-12:1-3, wherein the vinyl silane coupling agent is selected from vinyl trimethoxy silane, vinyl triethoxy silane or vinyl trichloro silane; In step S4, the mass ratio of the pretreated carbon fiber, styrene, cinnamamide and benzoyl peroxide is 10-15:4-8:3-6:0.5-1; In step S4, the heating reaction temperature is 80-90°C and the heating reaction time is 3-5h; In step S5, the mass ratio of the modified bamboo fiber powder, the modified carbon fiber, the polypropylene, the PP grafted maleic anhydride, the plasticizer, the antioxidant and the flame retardant is 40-50:4-8:60-80:5-10:2-4:1-2:1-1.
5.
2. The preparation method according to claim 1, characterized in that: In step S5, the plasticizer is selected from tributyl citrate, polyethylene glycol or polypropylene glycol, the antioxidant is selected from antioxidant 1010 or antioxidant 1076, and the flame retardant is selected from antimony trioxide or aluminum hydroxide.
3. The bio-based degradable composite material prepared by the preparation method according to any one of claims 1 to 2.