A flame retardant composite material and preparation method thereof

By using melamine tripolythiocyanate and ammonium polyphosphate as composite flame retardant in organic phase change materials, combined with core-shell structure, the flame retardant performance is significantly improved, and the flammability problem of traditional organic phase change materials is solved, achieving the realization of the ignition of traditional organic phase change materials. The need for application in strict fire protection environments.

CN118652533BActive Publication Date: 2024-11-26CATARC AUTOMOTIVE TEST CENT (GUANGZHOU) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411134877.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Traditional organic phase change materials have flammability problems and cannot meet the needs of application in strict fire-proof environments. The existing flame-retardant materials have low flame retardant properties, which are unable to effectively meet the needs of practical applications.

Method used

Using a flame retardant composite material, including phase change substrate, epoxy resin, thermal filler and composite flame retardant, the composite flame retardant consists of melamine trithiocyanate and ammonium polyphosphate, and forms a stable carbon layer. and dilute the oxygen concentration to improve flame retardant performance, and combine the core-shell structure to further enhance flame retardant performance.

Benefits of technology

It realizes a composite functional material that has both heat absorption and temperature control, thermal conductivity and flame retardant properties in energy storage equipment or electronic equipment, significantly improves the flame retardant performance of the material, overcomes flammability problems, and meets thermal management and thermal energy conversion. Storage requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118652533B_ABST
    Figure CN118652533B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of flame retardant materials, and specifically discloses a flame retardant composite material and a preparation method thereof. The flame retardant composite material of the present invention comprises the following components in percentage by mass: 50-70% of a phase change substrate, 10-20% of an epoxy resin, 1-4% of a thermally conductive filler, and 10-30% of a composite flame retardant; the composite flame retardant material comprises melamine thiocyanate and ammonium polyphosphate. The flame retardant composite material of the present invention overcomes the problem of flammability of phase change materials used in energy storage devices or electronic devices, and realizes a composite functional material with heat absorption and temperature control capabilities, thermal conductivity, and flame retardant properties as a whole, which can be used for thermal management, thermal energy conversion, and storage in energy storage devices or electronic devices and related energy fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of flame retardant materials, and particularly relates to a flame retardant composite material and a preparation method thereof. Background Art

[0002] With the rapid development of modern industry and construction, there is a growing demand for materials that can effectively manage thermal energy and improve energy efficiency. Phase change materials have attracted much attention due to their ability to absorb and release a large amount of latent heat during phase change, and are widely used in thermal energy storage, temperature control, and energy saving. However, traditional organic phase change materials have flammability issues, which limits their application in a wider range of occasions, especially in environments that require strict fire protection requirements.

[0003] To solve this problem, researchers have been exploring various flame retardant technologies to improve the safety of phase change materials. Early flame retardant strategies focused on using halogen compounds as flame retardants, but these substances release toxic gases when burned, which have a negative impact on the environment and human health. Therefore, the development of halogen-free, environmentally friendly flame retardants has become a research hotspot.

[0004] In recent years, people have found that some phosphorus and nitrogen compounds have excellent flame retardant properties. They can form a stable carbon layer during the combustion process to isolate oxygen and heat, thereby achieving the purpose of flame retardancy. However, in existing flame retardant materials, such phosphorus and nitrogen compounds have poor effects in combination with other components as flame retardants, resulting in low flame retardant properties of the material as a whole. In particular, when used in organic phase change materials, the flame retardant properties do not meet the standards and cannot meet the needs of practical applications. Summary of the invention

[0005] In view of the problems of poor flame retardancy of organic phase change materials involved in the above-mentioned prior art, the present invention provides a flame retardant composite material and a preparation method thereof.

[0006] To achieve the above purpose, the following technical solutions are specifically included:

[0007] A flame retardant composite material, comprising the following components in percentage by weight:

[0008] Phase change substrate 50-70%, epoxy resin 10-20%, thermal conductive filler 1-4%, composite flame retardant 10-30%; the composite flame retardant includes melamine thiocyanate and ammonium polyphosphate.

[0009] In the flame-retardant composite material of the present invention, the phase change substrate serves as a matrix of the phase change and provides a basis for the phase change, the epoxy resin serves as a material supporting the skeleton of the flame-retardant composite material, the thermally conductive filler provides good thermal conductivity, and the synergistic effect of melamine thiocyanate and ammonium polyphosphate significantly improves the flame retardant property, thereby overcoming the flammability problem of the phase change material used for energy storage devices or electronic devices, and realizing an overall composite functional material with heat absorption and temperature control capabilities, thermal conductivity and flame retardant properties, which can be used for thermal management, thermal energy conversion and storage of energy storage devices or electronic devices and related energy fields.

[0010] As a new type of halogen-free flame retardant, melamine thiocyanate can produce non-combustible gas during pyrolysis to dilute the oxygen concentration, thereby effectively improving the flame retardant properties of the material; ammonium polyphosphate can effectively improve the flame retardant properties of the material due to its ability to form a dense carbon layer in the condensed phase. Melamine thiocyanate and ammonium polyphosphate work together to comprehensively improve the flame retardant properties of phase change materials.

[0011] Preferably, the flame retardant composite material comprises the following components in percentage by weight: 65-69% of phase change substrate, 12-16% of epoxy resin, 1.2-2% of thermal conductive filler, and 15-18% of composite flame retardant.

[0012] Preferably, the composite flame retardant is a core-shell structure, wherein the core is ammonium polyphosphate and the shell is melamine thiocyanate.

[0013] When the composite flame retardant is a core-shell structure, melamine-thiocyanate is coated on the surface of ammonium polyphosphate particles, and other substances are coated on the surface of the composite flame retardant with the core-shell structure to form a core-shell structure. During the combustion process, a chain reaction can occur. The melamine-thiocyanate on the shell layer of the composite flame retardant can produce fire-resistant gas to dilute the oxygen concentration at the ignition site. At the same time, the core ammonium polyphosphate in the composite flame retardant can provide an acid source to promote the formation of residual carbon, enhance the density and thickness of the residual carbon generated in the condensed phase, form a more stable and dense expanded carbon layer, provide heat insulation protection and block flame combustion, and further improve the flame retardant properties of the material.

[0014] Preferably, the mass ratio of melamine thiocyanate to ammonium polyphosphate is (5-25): (5-25).

[0015] More preferably, the mass ratio of melamine thiocyanate to ammonium polyphosphate is (9-21):(8-21).

[0016] Under the above ratio, the composite flame retardant material has better flame retardant properties.

[0017] Preferably, the phase change substrate comprises polyethylene glycol, and the phase change temperature of polyethylene glycol is 50-52° C. and the phase change latent heat is 90 kJ / kg.

[0018] Preferably, the thermally conductive filler comprises expanded graphite.

[0019] Preferably, the epoxy resin is obtained by cross-linking and curing epoxy resin glue and a curing agent for epoxy resin glue.

[0020] The present invention also provides a method for preparing the flame-retardant composite material, using method (I) or method (II);

[0021] The method (I) comprises the following steps:

[0022] (1) Mix melamine, ammonium polyphosphate and water evenly, then add thiocyanate to react and obtain a composite flame retardant;

[0023] (2) melting the phase change substrate, adding epoxy resin glue, thermal conductive filler and the composite flame retardant in sequence, and mixing them evenly; then adding a curing agent for the epoxy resin glue, and curing to obtain the flame retardant composite material;

[0024] The method (II) comprises the following steps:

[0025] (1) melamine and water are mixed evenly, and then thiocyanuric acid is added to react to obtain melamine thiocyanate;

[0026] (2) Melting the phase change substrate, adding epoxy resin glue, thermal conductive filler, ammonium polyphosphate and the melamine thiocyanate in sequence, and mixing them evenly; then adding a curing agent for the epoxy resin glue, and curing to obtain the flame retardant composite material.

[0027] The preparation method of the invention is simple, has mild conditions and low operation requirements.

[0028] The method (I) or the method (II) satisfies the following parameters or conditions preferably.

[0029] Preferably, the mass ratio of melamine, ammonium polyphosphate and water is melamine:ammonium polyphosphate:water=(3-10):(8-25):(100-300);

[0030] Preferably, the mass ratio of the ammonium polyphosphate to thiocyanuric acid is (8-25): (5-15).

[0031] Preferably, the reaction temperature is 60-100° C., and the reaction time is 1-6 h.

[0032] Preferably, the uniform mixing time is 0.5-3h.

[0033] Preferably, the mass ratio of the epoxy resin glue to the curing agent of the epoxy resin glue is 1:(0.95-1.05).

[0034] Preferably, the curing temperature is ≤70°C.

[0035] Preferably, the melting temperature is 60-80°C.

[0036] Compared with the prior art, the present invention has the following beneficial effects: in the flame-retardant composite material of the present invention, the phase change substrate serves as the matrix of the phase change, the epoxy resin serves as the material of the supporting skeleton of the flame-retardant composite material, the thermal conductive filler provides good thermal conductivity, and the synergistic effect of melamine thiocyanate and ammonium polyphosphate significantly improves the flame retardant performance, thereby overcoming the flammability problem of the phase change material used in energy storage devices or electronic devices, and realizing as a whole a composite functional material having both heat absorption and temperature control capabilities, thermal conductivity and flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a graph showing the UL-94 test results of the flame retardant composite material to which only melamine-thiocyanate is added in Comparative Example 1.

[0038] Figure 2 This is a graph showing the UL-94 test results of the flame retardant composite material to which only ammonium polyphosphate was added in Comparative Example 2.

[0039] Figure 3 This is a graph showing the UL-94 test results of the flame retardant composite material in Example 4 in which melamine-trithiocyanate and ammonium polyphosphate were added but no core-shell structure was formed.

[0040] Figure 4 This is a graph showing the UL-94 test results of the flame retardant composite material of Example 1.

[0041] Figure 5 This is a graph showing the UL-94 test results of the flame retardant composite material of Example 2.

[0042] Figure 6 This is a graph showing the UL-94 test results of the flame retardant composite material of Example 3.

[0043] Figure 7 This is a graph showing the UL-94 test results for the material in Comparative Example 3.

[0044] Figure 8 This is the SEM image of the flame retardant composite material in Example 1.

[0045] Fig. 9 This is the SEM image of ammonium polyphosphate raw material. DETAILED DESCRIPTION

[0046] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below through specific examples. The test methods used in the examples and / or comparative examples are conventional methods unless otherwise specified; the materials, reagents, etc. used can be obtained from commercial channels unless otherwise specified. Among them, the polyethylene glycol used below is PEG2000, and the parallel examples and comparative examples all use the same raw materials; the brand of epoxy resin is Eric, and it is used in the form of AB glue with a dosage ratio of 1:1.

[0047] Example 1

[0048] A method for preparing a flame retardant composite material, comprising the following steps:

[0049] (1) 6.3 g of melamine and 15.16 g of ammonium polyphosphate were added to 200 mL of deionized water and placed in a magnetically stirred oil bath at a constant temperature of 90 °C. After the mixture was stirred evenly, 8.86 g of thiocyanuric acid was added and the magnetic stirring was continued for 3 h. Then, the mixture was filtered and vacuum dried to obtain a light yellow powder, which was the composite flame retardant.

[0050] (2) Melt 100 g of polyethylene glycol in a magnetic stirring oil bath at 65°C. When the polyethylene glycol is completely melted, add 9 g of epoxy resin glue while maintaining the temperature. After stirring evenly, add 2 g of expanded graphite; then add 25 g of the composite flame retardant prepared in step (1) and continue stirring for 1 hour; finally, add 9 g of epoxy curing agent and stir evenly;

[0051] (3) The mixture obtained in step (2) is poured into a mold and cured at room temperature to obtain a flame retardant composite material.

[0052] Example 2-3

[0053] Compared with Example 1, Example 2-3 differs in that the amounts of melamine, thiocyanuric acid and ammonium polyphosphate used in preparing the composite flame retardant in step (1) are different, as shown in Table 1 for details.

[0054] Example 4

[0055] A method for preparing a flame retardant composite material, comprising the following steps:

[0056] (1) 6.3 g of melamine was added to 200 mL of deionized water and placed in a magnetically stirred oil bath at a constant temperature of 90°C. After the mixture was stirred evenly, 8.86 g of thiocyanuric acid was added and the magnetic stirring was continued for 3 h. Then, the mixture was filtered and vacuum dried to obtain a light yellow powder, which was melamine thiocyanate.

[0057] (2) Melt 100 g of polyethylene glycol in a magnetic stirring oil bath at 65° C. When the polyethylene glycol is completely melted, add 9 g of epoxy resin glue while maintaining the temperature. After stirring evenly, add 2 g of expanded graphite; then add 7.5 g of melamine thiocyanate prepared in step (1) and 17.5 g of ammonium polyphosphate, and continue stirring for 1 hour; finally, add 9 g of epoxy curing agent and stir evenly;

[0058] (3) The mixture obtained in step (2) is poured into a mold and cured at room temperature to obtain a flame retardant composite material.

[0059] Comparative Example 1

[0060] A method for preparing a flame retardant composite material, comprising the following steps:

[0061] (1) 12.6 g of ammonium melamine was added to 200 mL of deionized water and placed in a magnetically stirred oil bath at a constant temperature of 90°C. After the mixture was stirred evenly, 17.72 g of thiocyanuric acid was added and magnetically stirred for 3 h. Then, the mixture was filtered and vacuum dried to obtain a light yellow powder, which was melamine thiocyanate.

[0062] (2) Melt 100 g of polyethylene glycol in a magnetic stirring oil bath at 65° C. When the polyethylene glycol is completely melted, add 9 g of epoxy resin glue while maintaining the temperature. After stirring evenly, add 2 g of expanded graphite; then add 25 g of melamine thiocyanate obtained in step (1) and continue stirring for 1 hour; finally, add 9 g of epoxy curing agent and stir evenly;

[0063] (3) The mixture obtained in step (2) is poured into a mold and cured at room temperature to obtain a flame retardant composite material.

[0064] Comparative Example 2

[0065] A method for preparing a flame retardant composite material, comprising the following steps:

[0066] (1) Melt 100g of polyethylene glycol in a magnetic stirring oil bath at 65°C. When the polyethylene glycol is completely melted, add 9g of epoxy resin glue while maintaining the temperature. After stirring evenly, add 2g of expanded graphite; then add 25g of ammonium polyphosphate and continue stirring for 1h; finally, add 9g of epoxy curing agent and stir evenly;

[0067] (2) The mixture obtained in step (1) is poured into a mold and cured at room temperature to obtain a flame retardant composite material.

[0068] Comparative Example 3

[0069] A method for preparing a phase change material, in which there is no flame retardant, the steps are as follows:

[0070] (1) Melt 100g of polyethylene glycol in a magnetic stirring oil bath at 65°C. When the polyethylene glycol is completely melted, add 9g of epoxy resin glue while maintaining the temperature. After stirring evenly, add 2g of expanded graphite and continue stirring for 1h. Finally, add 9g of epoxy curing agent and stir evenly.

[0071] (2) The mixture obtained in step (1) is poured into a mold and cured at room temperature to obtain a flame retardant composite material.

[0072] Table 1

[0073]

[0074] The composite flame retardant and ammonium polyphosphate raw material prepared in step (1) of Example 1 were subjected to scanning electron microscopy (SEM) detection. The SEM results are shown in the attached figure. Figure 8-9 As shown, comparative analysis shows that the composite flame retardant is a core-shell structure, and melamine thiocyanate is coated on the surface of ammonium polyphosphate particles.

[0075] The flame retardant composite materials prepared in the above examples and comparative examples were subjected to a vertical combustion test according to UL-94-2016 to verify the flame retardant properties of the flame retardant composite materials. The test results are shown in the attached Figure 1-7 As shown, the time for the flames in Comparative Example 1-2, Example 4 and Example 1-3 to be extinguished is 46s, 40s, 34s, 28s, 34s ​​and 11s respectively, and the flame in Comparative Example 3 continues to burn until the material is completely burned out.

[0076] It can be seen from Examples 1-3 and Comparative Examples 1-2 and 4 that in Example 1, there is a composite flame retardant with a core-shell structure formed by compounding melamine-thiocyanate and ammonium polyphosphate, and in Comparative Example 1-2, there is only one of melamine-thiocyanate and ammonium polyphosphate. The flame retardancy of Example 1 is much better than that of Comparative Examples 1-2 and 4. It can be seen that the compounding of melamine-thiocyanate and ammonium polyphosphate can synergistically improve the flame retardant properties of the composite material.

[0077] It can be seen from Example 1 and Example 4 that melamine-thiocyanate and ammonium polyphosphate form a core-shell structure in Example 1, and no core-shell structure is formed in Example 4. Although the flame extinguishing time is the same, the flame of Example 4 is larger, indicating that the formation of a core-shell structure is more conducive to the improvement of flame retardant performance; and the core-shell structure is mainly reflected in that the two flame retardants can exist in a small area at the same time. After the flame-retardant composite material is prepared to form a corresponding product, it can overcome the defect of uneven dispersion of the two flame retardants due to repeated use or long-term use (flame retardant deposition due to the increase in time and excessive use will cause uneven dispersion of the flame retardant), thereby improving the service life of the product.

[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A flame retardant composite material, characterized in that: The following components are included in the mass percentage: Phase change substrate 50-70%, epoxy resin 10-20%, thermal conductive filler 1-4%, composite flame retardant 10-30%; the composite flame retardant includes melamine thiocyanate and ammonium polyphosphate; the composite flame retardant is a core-shell structure, wherein the core is ammonium polyphosphate and the shell is melamine thiocyanate.

2. The flame retardant composite material according to claim 1, characterized in that: The mass ratio of melamine thiocyanate to ammonium polyphosphate is (5-25): (5-25).

3. The flame retardant composite material according to claim 1, characterized in that: The phase change matrix includes polyethylene glycol.

4. The flame retardant composite material according to claim 1, characterized in that: The thermally conductive filler includes expanded graphite.

5. A method for preparing the flame retardant composite material according to any one of claims 1 to 4, characterized in that: The steps include: (1) Mix melamine, ammonium polyphosphate and water evenly, then add thiocyanate to react and obtain a composite flame retardant; (2) Melting the phase change substrate, adding epoxy resin glue, thermal conductive filler and the composite flame retardant in sequence, and mixing them evenly; then adding a curing agent for the epoxy resin glue, and curing to obtain the flame retardant composite material.

6. The method for preparing a flame retardant composite material according to claim 5, characterized in that: The mass ratio of melamine, ammonium polyphosphate and water is melamine:ammonium polyphosphate:water=(3-10):(8-25):(100-300); the mass ratio of ammonium polyphosphate and thiocyanuric acid is (8-25):(5-15).

7. The method for preparing a flame retardant composite material according to claim 5, characterized in that: The reaction temperature is 60-100° C., and the reaction time is 1-6 hours.

8. The method for preparing a flame retardant composite material according to claim 5, characterized in that: The mixing time is 0.5-3h.

9. The method for preparing a flame retardant composite material according to claim 5, characterized in that: The mass ratio of the epoxy resin glue to the curing agent of the epoxy resin glue is 1:(0.95-1.05).

Citation Information

Patent Citations

  • Microencapsulation expansion type flame retardant and application in epoxy resin composite material thereof

    CN101812186A

  • Anti-flaming phase-change energy storage, heat preservation and heat insulation material and preparation method thereof

    CN106750174A

  • Halogen-free flame retardant composition and application thereof

    CN110951113A

  • Phase change composite material as well as preparation method and application thereof

    CN115466600A

  • A composite phase change material and its method of preparation thereof

    US20230183539A1