A kind of anticorrosive and anti-seepage polyurea material used in seawater desalination and its preparation method
By adding amino-modified graphene/Zn/porous carbon composite and ethylene vinyl acetate copolymer to polyurea materials, a uniformly dispersed conductive network is formed, which solves the problem of poor dispersion of graphene and zinc powder in the prior art, improves corrosion resistance and impermeability, and enhances adhesion to steel substrates.
Patent Information
- Application Number
- CN202411092213.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-09
AI Technical Summary
In existing spray-applied polyurea anti-corrosion coatings, the poor dispersibility of graphene, carbon nanotubes, and zinc powder limits their role in polyurea materials, making it impossible to effectively improve the utilization efficiency and corrosion resistance of zinc powder, and also limiting the improvement in anti-corrosion and anti-permeability performance.
By preparing amino-modified graphene/Zn/porous carbon composites and synergistically combining them with ethylene-vinyl acetate copolymers and butadiene-benzoxazine copolymers, a uniformly dispersed conductive network is formed, which enhances the density and adhesion of polyurea materials and improves their corrosion resistance.
The process achieves uniform dispersion of graphene, zinc powder, and porous carbon, forming a continuous conductive network. This improves the corrosion resistance and impermeability of polyurea materials, enhances their adhesion to steel substrates, and extends their service life.
Smart Images

Figure CN118652616B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurea materials, in particular to an anti-corrosion and anti-seepage polyurea material used in seawater desalination and a preparation method thereof. Background Art
[0002] The importance and significance of seawater desalination projects are self-evident. The ocean is a highly corrosive and harsh environment. The seawater absorption, transportation, and treatment devices involved in seawater desalination projects all have high requirements for anti-corrosion coatings. At present, spray-type polyurea anti-corrosion coatings are widely used in seawater desalination project anti-corrosion due to their advantages such as high strength, long life, and high construction efficiency.
[0003] In the prior art, spray-type polyurea anticorrosive coatings are used for both concrete and steel bases. When used for steel bases, it is necessary to consider not only the material adhesion problem similar to that of concrete bases, but also the material's resistance to cathodic stripping strength. Therefore, zinc powder is generally added to polyurea anticorrosive coatings for steel bases. Zinc powder has active chemical properties, electrochemical cathodic protection, and excellent water resistance and rust prevention properties. In order to give full play to the cathodic protection effect of zinc powder, graphene and porous carbon are also added to the coating to form a conductive path between zinc powder particles, thereby improving the efficiency and effect of zinc powder. For example, Chinese patent application No. 202010692158.5 discloses a nano-modified polyaspartic acid ester polyurea heavy anticorrosion coating and its preparation method, which uses polyaspartic acid esters of different reactivity as the main resin of the anticorrosion coating, and at the same time, a certain amount of low-polarity, low-surface-energy hydroxyl resin is added, and low-viscosity aliphatic isocyanate is used as a curing agent. Graphene and carbon nanotubes are added to the coating system to form a conductive path between zinc powder particles, thereby improving the use efficiency of zinc powder in the coating, reducing the amount of zinc powder, and changing the bottom, middle, and surface three-layer system of the traditional anticorrosion coating into a one-layer system, thereby improving the coating efficiency. However, in this technical solution, graphene, carbon nanotubes, and zinc powder are added to the organic system respectively. Under the premise of not modifying them in any way, even if various additives are added to promote their dispersion, they can only play a promoting role, and cannot truly achieve a relatively uniform distribution between the three components of graphene, carbon nanotubes, and zinc powder. Therefore, the actual role of graphene and carbon nanotubes in reducing the amount of zinc powder used and improving the use effect of zinc powder is very limited. In addition, although graphene added to the polyurea system can to a certain extent block the corrosive medium from penetrating into the coating through pores and cracks, due to poor dispersibility, the corrosion resistance cannot be fully exerted, and the anti-corrosion and anti-permeability properties of the polyurea material cannot be significantly improved by relying solely on graphene.
[0004] To this end, this application is filed. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides an anti-corrosion and anti-seepage polyurea material for seawater desalination and a preparation method thereof.
[0006] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0007] On the one hand, the present application provides a method for preparing an anti-corrosion and anti-seepage polyurea material for seawater desalination, wherein the anti-corrosion and anti-seepage polyurea material is prepared from component A and component B;
[0008] Component A is obtained by prepolymerization of polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate. The preparation method is as follows: under N2 protection, the polyether polyol is heated to 105°C, first dehydrated under vacuum, then cooled, aliphatic polyisocyanate and aromatic polyisocyanate are added, and then reacted at 80-110°C for 2-6h to obtain the obtained component;
[0009] Component B includes amino polyether, amine chain extender, fluorocarbon resin with fluorine content ≥26%, ethylene vinyl acetate copolymer, butadiene-benzoxazine copolymer, amino modified graphene / Zn / porous carbon composite and additives, and the preparation method is: amino polyether, amine chain extender, fluorocarbon resin, amino modified graphene / Zn / porous carbon composite and part of the additives are mixed and stirred to obtain a first premix, ethylene vinyl acetate copolymer, butadiene-benzoxazine copolymer and the remaining additives are mixed and stirred to obtain a second premix, and the second premix is added to the first premix and stirred to obtain component B;
[0010] When in use, firstly use an electron accelerator to irradiate component B with beta rays in an inert atmosphere, the irradiation time is 15-25 minutes, the irradiation dose is 30-40 kGy, then mix component A and component B, stir evenly, and spray to form.
[0011] Compared with the prior art, the main improvements of the present invention are:
[0012] (1) By adding fluorocarbon resin, ethylene vinyl acetate copolymer and butadiene-benzoxazine copolymer to component B, the resins or copolymers with different molecular weights work synergistically and strengthen each other, which significantly improves the density and flexibility of the polyurea material, fundamentally avoids the penetration of corrosive media, and improves the corrosion resistance and impermeability of the polyurea material.
[0013] Fluorocarbon resin added to polyurea material helps to improve its weather resistance, corrosion resistance, heat resistance, cold resistance and anti-fouling performance, making polyurea material show better stability and durability. Butadiene-benzoxazine copolymer has the effect of improving the adhesion between single hydrocarbon resin and metal. However, when it is added alone to polyurea material, the adhesion between polyurea material and steel base is not significantly improved. Later, the applicant tried a large number of formulas and unexpectedly found that when it was added together with ethylene vinyl acetate copolymer and irradiated, it showed a significant improvement in adhesion. The applicant speculated that on the one hand, ethylene vinyl acetate copolymer has viscosity and excellent flexibility. After its addition, it can not only improve the viscosity and toughness of polyurea material, but also produce macromolecular peroxide after irradiation. Under the action of the macromolecular peroxide, butadiene-benzoxazine copolymer and amino polyether are grafted, which may generate polyurea material with interpenetrating network structure. It is dense, continuous and stable, not only showing good anti-corrosion and anti-seepage performance, but also has a strong bonding effect with the steel-based spray surface.
[0014] (2) By forming a composite of graphene, zinc powder and porous carbon and performing amino modification, the problem of uneven dispersion caused by adding graphene, zinc powder and porous carbon separately in the prior art is overcome, and the uniform dispersion of graphene, zinc powder and porous carbon is fundamentally achieved. After amino modification, the composite has good compatibility with amino polyether, further improving the dispersion effect of the obtained composite in component B, and achieving uniform dispersion of graphene, porous carbon and zinc powder under synergistic effect; graphene and porous carbon are dual conductive and can form a continuous conductive network with a small amount of zinc powder, thereby playing a cathodic protection role, which not only helps to reduce the use of zinc powder, but also improves the corrosion resistance of the material; and the porous carbon structure is also an effective filler for improving the physical properties of polyurea materials such as strength, hardness and wear resistance. While fluorocarbon resin, ethylene vinyl acetate copolymer and butadiene-benzoxazine copolymer are toughened and enhance the peel strength, the impact resistance and wear resistance of the polyurea material are improved, so that the final product has good comprehensive performance.
[0015] The present invention improves the anti-corrosion and anti-seepage performance of polyurea materials from two aspects. On the one hand, the flexibility, density and adhesion of polyurea materials to the steel-based spray surface are improved by compounding different resins and copolymers, which fundamentally improves the anti-corrosion and anti-seepage capabilities of polyurea materials. On the other hand, by synthesizing amino-modified graphene / Zn / porous carbon composites, graphene, Zn and porous carbon are uniformly dispersed in the polyurea material and form a labyrinth structure for blocking corrosive media, further improving the anti-corrosion and anti-seepage capabilities of polyurea materials. The two methods influence and synergize each other, and together promote the anti-corrosion and anti-seepage polyurea materials used in seawater desalination proposed by the present invention to have excellent anti-corrosion and anti-seepage capabilities and physical strength.
[0016] Preferably, the preparation steps of the amino-modified graphene / Zn / porous carbon composite are as follows:
[0017] S1. Preparation of graphene / Zn / porous carbon composites
[0018] Ultrasonic dispersion of graphite oxide in deionized water, first adding EDTA and zinc chloride and stirring until dissolved, then adding chitosan and stirring until dissolved, and finally reacting in a water reactor at 120-140° C. for at least 24 hours to obtain a precursor mixture;
[0019] The precursor mixture is first heated to remove water, then dried, and finally calcined at 550-620° C. for at least 1 hour under an inert atmosphere, and then ground to obtain a graphene / Zn / porous carbon composite;
[0020] S2. Amino modification of graphene / Zn / porous carbon composite
[0021] The amino polyether is dissolved in DMF to obtain a modifier, the graphene / Zn / porous carbon composite is dispersed in deionized water containing PVP to obtain a mixture to be modified, the mixture to be modified is added to the modifier and stirred evenly to obtain a mixed system, under the protection of an inert gas, the mixed system is refluxed and stirred at 100-110° C. for at least 5 hours, then cooled to room temperature and a solid phase is collected, the solid phase is washed with DMF, and vacuum dried to obtain an amino-modified graphene / Zn / porous carbon composite.
[0022] In S1, graphite oxide was exfoliated into single-layer graphene oxide under ultrasound and dispersed in deionized water. Zn 2+ The Zn complex is coordinated with EDTA, and the Zn complex is loaded on the surface of graphene oxide through intermolecular forces. In the subsequent hydrothermal reaction, the high pressure in the water reactor causes the epoxy bonds on the graphene oxide to break and then be removed in the form of CO2, thereby realizing the conversion of graphene oxide into graphene. After the precursor mixture is heated and dehydrated, the chitosan and the graphene loaded with the Zn complex are evenly mixed, and calcined under an inert atmosphere to form nano zinc and porous carbon with a high specific surface area and porosity. The graphene is in the form of two-dimensional sheets, and the Zn is in the form of three-dimensional granular nano zinc. After the chitosan is carbonized, hard carbon with a rich porous structure is formed. The synergistic effect of the components and morphology helps to form a maze structure that blocks the corrosive medium in multiple dimensions, so that the composite has better corrosion resistance and anti-seepage properties.
[0023] In S2, the graphene / Zn / porous carbon composite is modified by amino functionalization, so that it has good compatibility with the polyurea matrix, and then it is guaranteed from the outside that it has good dispersibility in component B. The graphene / Zn / porous carbon composite is the internal cause, and the amino modification is the external cause. The synergistic effect of the internal and external factors realizes the uniform dispersion of graphene, Zn and porous carbon in the polyurea body, and finally effectively improves the corrosion resistance and impermeability of the polyurea material.
[0024] It should be noted that in order to obtain well-dispersed graphene oxide, the ultrasound in S1 preferably adopts graded ultrasound, firstly breaking up the graphite oxide into multi-layer graphene oxide by high-power, low-frequency, and high-amplitude ultrasound, and then breaking up the multi-layer graphene oxide into a few-layer graphene oxide by medium-power, medium-frequency, and medium-amplitude ultrasound, and finally obtaining a single-layer graphene oxide suspension by low-power, high-frequency, and low-amplitude ultrasound, and then adding EDTA and zinc chloride on the basis of maintaining the graphene oxide in a suspended state by ultrasound.
[0025] Preferably, the molar ratio of EDTA to zinc chloride is (1-3):1. Under this condition, Zn 2+ The maximum complexation; the mass ratio of the graphite oxide, zinc chloride, and chitosan is 3: (0.8-2): (0.5-1.1), preferably 3: (1-1.5): (0.7-0.9), and further preferably 3: 1.2: 0.8. Under the above ratio, the obtained composite has a proper ratio of graphene, Zn, and porous carbon, which helps to better play a synergistic role. If the content of graphite oxide is too little, less graphene oxide is formed after ultrasound, resulting in the generated composite being unable to rely on the flake structure of graphene oxide to achieve the purpose of improving its dispersibility; Too much graphite oxide content and too much graphene oxide formed after ultrasound are beneficial to improving the dispersibility of the composite, but the content of zinc powder and porous carbon is relatively low, and the cathodic protection effect of zinc powder and the physical enhancement effect of porous carbon cannot be effectively exerted; if there is too much porous carbon, its rich porous structure may cause the corrosive medium to penetrate slowly, deteriorating the anti-corrosion and anti-permeability properties of the polyurea material; if there is too little porous carbon, it cannot be effectively embedded in the interpenetrating polyurea network structure, and the improvement of the physical strength of the polyurea material, such as wear resistance and impact resistance, is not obvious, and the comprehensive performance cannot be optimized. The applicant has found that under the above-mentioned ratio, the addition of amino-modified graphene / Zn / porous carbon composites to the polyurea matrix in an appropriate proportion helps to obtain a polyurea material with both good physical properties and anti-corrosion and anti-permeability properties.
[0026] Preferably, the preparation method of the butadiene-benzoxazine copolymer in component B is: adding paraformaldehyde, bisphenol A or bisphenol F or bisphenol S, and allylamine to DMF, reacting at 95-102° C. for 3-5 hours to obtain a benzoxazine monomer, and then copolymerizing the benzoxazine monomer and butadiene at 65-72° C. with an azo or peroxide free radical initiator, and controlling the reaction time within 3 hours to obtain the copolymer.
[0027] The preparation method of butadiene-benzoxazine copolymer is prior art. In this embodiment, the molar ratio of benzoxazine monomer to butadiene is 1:(1-5), and the mass of the free radical initiator is 5-8wt% of the total mass of benzoxazine monomer and butadiene. In this embodiment, the azo initiator can be selected from at least one of azobisisobutyronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, etc., and the peroxide initiator can be selected from at least one of hydrogen peroxide, benzoyl peroxide, diisopropylbenzene peroxide, etc.
[0028] It should be noted that: the copolymerization reaction of benzoxazine monomer and butadiene must strictly control the temperature to 65-72°C and the time to no more than 3h. The butadiene-benzoxazine copolymer used in this application is precisely a butadiene-benzoxazine oligomer containing some butadiene monomers and benzoxazine monomers that have not reacted completely. If the temperature is too high, the copolymerization product is a mixture of butadiene-benzoxazine oligomers and butadiene-benzoxazine polymers, which is not beneficial to improving the performance of polyurea materials. If the time is too long, butadiene monomers and benzoxazine monomers are fully involved in the copolymerization reaction, which is not conducive to the subsequent stable grafting of butadiene-benzoxazine copolymers with amino polyethers. Preferably, the molar ratio of -NCO in component A to -NH in component B is 1:(1.05-1.1).
[0029] Preferably, component A is obtained by prepolymerizing polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate in a mass ratio of 100:(60-80):(20-40); the contents of each component in component B are 30-40wt% of amino polyether, 10-20wt% of amine chain extender, 10-15wt% of fluorocarbon resin, 8-20wt% of ethylene vinyl acetate copolymer, 10-15wt% of butadiene-benzoxazine copolymer, 5-12wt% of amino-modified graphene / Zn / porous carbon composite, and the remainder is auxiliary agent.
[0030] In this embodiment, the aliphatic polyisocyanate curing agent is hexamethylene diisocyanate, the aromatic polyisocyanate curing agent is selected from at least one of p-phenylene diisocyanate, m-phenylene diisocyanate, toluene-2,6-diisocyanate, diphenylmethane-4,4'-diisocyanate, chlorobenzene-2,4-isocyanate, naphthalene-1,5-diisocyanate, biphenyl-4,4'-diisocyanate, 3-methyldiphenylmethane-4,4'-diisocyanate, diphenyl ether diisocyanate, and triphenylmethane triisocyanate, the amine chain extender is selected from aromatic diamines or aliphatic diamines, and the aromatic diamine is selected from 3,5-diethyltoluenediamine, 3,3'-dichloro-4,4'-diaminodiphenylmethane, 3,3 At least one of '-diethyl-4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, 2,4-diamino-3,5-dimethylthiochlorobenzene, bis-sec-butylaminodiphenylmethane and N,N'-dialkylphenylenediamine; the aliphatic diamine is selected from at least one of isophoronediamine, dimethyl-diamino-dicyclohexylmethane, 4,4'-bis-sec-butylaminodicyclohexylmethane or 3,3'-dimethyl-4,4'-bis-sec-butylamino-dicyclohexylmethane.
[0031] Preferably, the auxiliary agent is selected from one or more of the following components: pigment, diluent, defoamer, wetting agent, leveling agent, thickener, hydrophobic plasticizer, adhesion promoter, anti-settling agent;
[0032] The pigment is at least one of titanium dioxide, barium dioxide, zinc dioxide, chromium oxide green, iron oxide red, iron oxide yellow, chrome yellow, iron black, carbon black and organic pigments; the diluent is a composition of propylene carbonate, ethyl carbonate and dibutyl phthalate in a mass ratio of 1:1:1; the defoamer is one of polyether-modified polysiloxane, high molecular polymer and fluorine-modified acrylic polymer; the wetting agent is a modified silicone wetting agent; the leveling agent is an acrylic copolymer leveling agent; the thickener is a non-ionic polyurethane associative thickener; the hydrophobic plasticizer is one of dioctyl phthalate, dioctyl terephthalate and dioctyl adipate; the adhesion promoter is one of γ-glycidyloxypropyl trimethylsilane, γ-glycidyloxypropyl triethoxysilane and β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane; and the anti-settling agent is a compound of polyamide wax and hydrogenated castor oil in a ratio of 1:2.
[0033] On the other hand, the present invention provides an anti-corrosion and anti-seepage polyurea material used in seawater desalination, which is prepared by the above preparation method.
[0034] The polyurea coating formed by the anti-corrosion and anti-seepage polyurea material proposed in the present invention is continuous, dense, and has strong adhesion. It can effectively isolate the steel base or concrete base from the external corrosive medium, and then play a lasting and effective protective role. It is simple to construct, has a smooth and beautiful appearance, has good anti-corrosion and anti-seepage effects, a long service life and good comprehensive performance, and is specially used as an anti-corrosion coating required for seawater desalination projects such as seawater absorption, desalination, post-mineralization, transportation and distribution. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 This is a photo of the polyasparagine protective material described in Example 1 of the present invention after spraying in a seawater desalination project in a certain place;
[0037] Figure 2 This is a photo of the polyasparagine protective material described in Example 1 of the present invention before spraying in a seawater desalination project in a certain place;
[0038] Figure 3 The photograph is of a seawater desalination project in a certain place, in which the polyasparagine protective material described in Example 1 of the present invention was sprayed and used for 3 years. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0040] The raw materials involved in the following examples and comparative examples were all commercially available. Ethylene vinyl acetate copolymer was purchased from Beijing Mairida Technology Co., Ltd. with the item number P815475-1kg. Chitosan is specifically water-soluble chitosan, purchased from Suzhou Meigaomei Biotechnology Co., Ltd., food grade, with an effective substance content of 99%, and a packaging specification of 25kg. The polyether polyol is specifically polytetramethylene furan polyether diol, the aliphatic polyisocyanate curing agent is specifically hexamethylene diisocyanate, the aromatic polyisocyanate curing agent is diphenylmethane-4,4'-diisocyanate, and the amine chain extender is specifically dimethylthiotoluene diamine and 4,4'-diisocyanate in a mass ratio of 2:1. ,- a mixture of di-sec-butylaminodiphenylmethane; the amino polyether is polytetramethylene ether diparaaminobenzoate; 10 parts of additives contain: 2 parts of pigment, 2 parts of defoamer, 4 parts of wetting agent, 0.5 parts of leveling agent, 0.5 parts of hydrophobic plasticizer, 0.6 parts of adhesion promoter, and 0.4 parts of anti-settling agent. The pigment is specifically a mixture of R706 titanium dioxide and industrial chromium oxide green in a mass ratio of 10:1, the defoamer is specifically a fluorine-modified acrylic polymer, the wetting agent is specifically a modified silicone wetting agent, the leveling agent is specifically an acrylic copolymer leveling agent, the hydrophobic plasticizer is dioctyl phthalate, the adhesion promoter is specifically γ-glycidyl ether oxypropyl triethoxy silane, and the anti-settling agent is specifically a compound of polyamide wax and hydrogenated castor oil in a ratio of 1:2; other raw materials, unless otherwise specified, are conventional raw materials in the field and are not limited to their sources.
[0041] Preparation method of amino-modified graphene / Zn / porous carbon composite A: Amino-modified graphene / Zn / porous carbon composite A is prepared according to the following operation: graphite oxide is ultrasonically dispersed in deionized water, EDTA and zinc chloride are first added and stirred until dissolved, chitosan is added and stirred until dissolved, and finally reacted in a water reactor at 130°C for 24h to obtain a precursor mixture; the precursor mixture is first heated to 100°C to continuously remove water, then dried at 60°C in vacuum, and finally calcined at 600°C for 5h under N2 protection, and the graphene / Zn / porous carbon composite is obtained after grinding; amino polyether is dissolved in D A modifier is obtained from MF, a graphene / Zn / porous carbon composite is dispersed in deionized water containing PVP to obtain a mixture to be modified, the mixture to be modified is added to the modifier and stirred evenly to obtain a mixed system, under N2 protection, the mixed system is refluxed and stirred at 100°C for 5 hours, then cooled to room temperature and the solid phase is collected, the solid phase is washed 3 times with DMF and dried at 60°C in a vacuum to obtain an amino-modified graphene / Zn / porous carbon composite; wherein the mass ratio of graphite oxide, zinc chloride and chitosan is 3:1.2:0.8; and the molar ratio of EDTA to zinc chloride is 3:1.
[0042] The amino-modified graphene / Zn / porous carbon composite B was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:0.8:1.1.
[0043] An amino-modified graphene / Zn / porous carbon composite C was prepared according to a similar operation as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:2:0.5.
[0044] An amino-modified graphene / Zn / porous carbon composite D was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1:0.9.
[0045] The amino-modified graphene / Zn / porous carbon composite E was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1.5:0.7.
[0046] An amino-modified graphene / Zn / porous carbon composite F was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1.5:0.7.
[0047] An amino-modified graphene / Zn / porous carbon composite F was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1.5:0.7.
[0048] The amino-modified graphene / Zn / porous carbon composite G was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1.2:0.3.
[0049] The amino-modified graphene / Zn / porous carbon composite H was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 3:1.2:1.5.
[0050] Amino-modified graphene / Zn / porous carbon composite I was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 1:1.2:0.8.
[0051] The amino-modified graphene / Zn / porous carbon composite J was prepared according to similar operations as above, which was different from the “preparation method of amino-modified graphene / Zn / porous carbon composite A” in that the mass ratio of graphite oxide, zinc chloride, and chitosan was 5:1.2:0.8.
[0052] An amino-modified graphene / Zn / porous carbon composite K was prepared according to the similar operation as above, which was different from the “method for preparing amino-modified graphene / Zn / porous carbon composite A” in that chitosan was not added.
[0053] Preparation method of butadiene-benzoxazine copolymer A: add polyformaldehyde, bisphenol F and allylamine to DMF at a molar ratio of 5:1:2, mix well and react at 98°C for 4 hours, then add anhydrous magnesium sulfate and stir continuously, then filter and distill the filtrate under reduced pressure to obtain benzoxazine monomer, then add 6wt% of azobisisobutyronitrile to the benzoxazine monomer and butadiene at a molar ratio of 1:3 at 68°C and react for 2 hours, collect the product after the reaction and distill under reduced pressure to obtain the product.
[0054] A butadiene-benzoxazine copolymer B was prepared according to the similar operation as above, which was different from the "method for preparing butadiene-benzoxazine copolymer A" in that the copolymerization temperature of benzoxazine monomer and butadiene was 90°C.
[0055] A butadiene-benzoxazine copolymer C was prepared according to the above similar operation, which was different from the “method for preparing butadiene-benzoxazine copolymer A” in that the copolymerization time of benzoxazine monomer and butadiene was 5 h.
[0056] Example 1
[0057] A method for preparing an anti-corrosion and anti-seepage polyurea material used in seawater desalination, which is prepared from component A and component B;
[0058] The preparation method of component A is as follows: under the protection of N2, the polyether polyol is heated to 105°C, first dehydrated under vacuum, then cooled and added with aliphatic polyisocyanate and aromatic polyisocyanate, and then reacted at 100°C for 5h, and the polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate are prepolymerized in a mass ratio of 100:70:30 to obtain the component;
[0059] The preparation method of component B is as follows: amino polyether, amine chain extender, fluorocarbon resin, amino-modified graphene / Zn / porous carbon composite A and part of the auxiliary agent are mixed and stirred to obtain a first premix, ethylene vinyl acetate copolymer, butadiene-benzoxazine copolymer A and the remaining auxiliary agent are mixed and stirred to obtain a second premix, and the second premix is added to the first premix and stirred to obtain component B, wherein: amino polyether 35wt%, amine chain extender 15wt%, fluorocarbon resin 12wt%, ethylene vinyl acetate copolymer 15wt%, butadiene-benzoxazine copolymer 12wt%, amino-modified graphene / Zn / porous carbon composite 8wt%, and the balance is auxiliary agent;
[0060] When in use, first use an electron accelerator to irradiate component B with β rays in an inert atmosphere, the irradiation time is 20 minutes, and the irradiation dose is 35 kGy. Then, component A and component B are mixed and stirred evenly. The molar ratio of -NCO in component A to -NH in component B is 1:1.08. The mixture is polymerized at room temperature and sprayed.
[0061] like Figure 2 As shown, the base to be sprayed in a seawater desalination project in a certain place is a concrete base; the photo after spraying with the product obtained in Example 1 is as shown in Figure 1 As shown in the figure, the coating is dense, flat, smooth, and has a gray-green appearance with high aesthetic value to the naked eye; after three years of use, its appearance is as shown in the figure below. Figure 3 As shown, the coating has no obvious peeling or cracking, and its adhesion to the concrete substrate is still good, and it can still continue to play a protective role, which shows that its service life is long.
[0062] Example 2
[0063] Compared with Example 1, component A is obtained by prepolymerizing polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate in a mass ratio of 100:60:40.
[0064] Example 3
[0065] Compared with Example 1, component A is obtained by prepolymerization of polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate in a mass ratio of 100:80:20.
[0066] Example 4
[0067] Compared with Example 1, the composition of component B is changed, specifically 40wt% amino polyether, 15wt% amine chain extender, 10wt% fluorocarbon resin, 20wt% ethylene vinyl acetate copolymer, 12wt% butadiene-benzoxazine copolymer, 5wt% amino-modified graphene / Zn / porous carbon composite, and the balance is auxiliary agent.
[0068] Example 5
[0069] Compared with Example 1, the composition of component B is changed, specifically 35wt% amino polyether, 10wt% amine chain extender, 15wt% fluorocarbon resin, 15wt% ethylene vinyl acetate copolymer, 10wt% butadiene-benzoxazine copolymer, 12wt% amino-modified graphene / Zn / porous carbon composite, and the balance is auxiliary agent.
[0070] Example 6
[0071] Compared with Example 1, the composition of component B is changed, specifically 30wt% amino polyether, 20wt% amine chain extender, 12wt% fluorocarbon resin, 8wt% ethylene vinyl acetate copolymer, 15wt% butadiene-benzoxazine copolymer, 10wt% amino-modified graphene / Zn / porous carbon composite, and the remainder is auxiliary agent.
[0072] Example 7
[0073] Compared with Example 1, the irradiation conditions were adjusted to 15 min of irradiation time and 40 kGy of irradiation dose. The rest were the same as Example 1.
[0074] Example 8
[0075] Compared with Example 1, the irradiation conditions were adjusted to 25 min of irradiation time and 30 kGy of irradiation dose. The rest were the same as Example 1.
[0076] Comparative Example 1
[0077] On the basis of Example 1, the amino-modified graphene / Zn / porous carbon composite A was adjusted to an equal amount of the amino-modified graphene / Zn / porous carbon composite G.
[0078] Comparative Example 2
[0079] On the basis of Example 1, the amino-modified graphene / Zn / porous carbon composite A was adjusted to an equal amount of the amino-modified graphene / Zn / porous carbon composite H.
[0080] Comparative Example 3
[0081] On the basis of Example 1, the amino-modified graphene / Zn / porous carbon composite A was adjusted to an equal amount of the amino-modified graphene / Zn / porous carbon composite I.
[0082] Comparative Example 4
[0083] On the basis of Example 1, the amino-modified graphene / Zn / porous carbon composite A was adjusted to an equal amount of the amino-modified graphene / Zn / porous carbon composite J.
[0084] Comparative Example 5
[0085] Compared with Example 1, ethylene vinyl acetate copolymer is not added to component B, and the rest is the same as Example 1.
[0086] Comparative Example 6
[0087] Compared with Example 1, component B is not irradiated before use. The rest is the same as Example 1.
[0088] Comparative Example 7
[0089] Compared with Example 1, the irradiation conditions of component B before use are: irradiation time 10 minutes, irradiation dose 20 kGy. The rest are the same as Example 1.
[0090] Comparative Example 8
[0091] Compared with Example 1, the irradiation conditions of component B before use are: irradiation time 30 minutes, irradiation dose 50 kGy. The rest are the same as Example 1.
[0092] Comparative Example 9
[0093] Compared with Example 1, the amount of amino-modified graphene / Zn / porous carbon composite A was adjusted to be equal to the amount of amino-modified graphene / Zn / porous carbon composite K.
[0094] Comparative Example 10
[0095] Compared with Example 1, the ethylene vinyl acetate copolymer was adjusted to an equal amount of the vinyl styrene-based copolymer.
[0096] Comparative Example 11
[0097] Compared with Example 1, the ethylene-vinyl acetate copolymer was adjusted to an equal amount of the vinyl chloride-vinyl acetate copolymer.
[0098] Comparative Example 12
[0099] Compared with Example 1, the ethylene-vinyl acetate copolymer was adjusted to an equal amount of ethylene-tetrafluoroethylene copolymer.
[0100] Comparative Example 13
[0101] Compared with Example 1, the amount of amino-modified graphene / Zn / porous carbon composite A in component B was reduced by half. The rest was the same as Example 1.
[0102] Comparative Example 14
[0103] Compared with Example 1, the amount of amino-modified graphene / Zn / porous carbon composite A in component B is doubled. The rest is the same as Example 1.
[0104] Comparative Example 15
[0105] Compared with Example 1, the butadiene-benzoxazine copolymer A in component B is adjusted to an equal amount of butadiene-benzoxazine copolymer B.
[0106] Comparative Example 16
[0107] Compared with Example 1, the butadiene-benzoxazine copolymer A in component B is adjusted to an equal amount of butadiene-benzoxazine copolymer C.
[0108] The components A and B obtained in Examples 1 to 8 and Comparative Examples 1 to 16 were quickly mixed and poured into a mold within 5 seconds, and molded using a flat vulcanizer at 100°C to obtain test specimens. The hardness, tensile strength, elongation at break, and corrosion resistance A tests were performed on each test specimen. The hardness was measured according to GB / T531.1-2008; the tensile strength and elongation at break were measured according to GB / T528-2009; the specific operation of the corrosion resistance A test was as follows: first weigh the original mass of each test specimen, then place it in the same pressure-resistant and sealed digestion tank, soak it in a 150°C, 5% by mass NaOH solution for 8 hours, take it out, wash it with water, dry it, and weigh it again to calculate the mass loss rate. Then test the adhesion according to the GB / T 5210-2006 paint and varnish pull-off adhesion test.
[0109] The polyurea materials obtained in Examples 1 to 8 and Comparative Examples 1 to 16 were sprayed and then subjected to corrosion resistance test B. The specific spraying scheme is as follows: a stainless steel plate with a size of 600 mm×600 mm×5 mm was used as the spraying substrate, and was pickled, passivated and sandblasted before spraying to make its surface reach sa2 level, and then a high-pressure manual spray gun was used as the spraying equipment, and the spraying process parameters were: fluid temperature 50-70°C, fluid pressure 10-15 MPa, about 40 cm from the plate surface, and the A component and the B component mixed according to the molar ratio of -NCO to -NH 1:1.08 were sprayed on the spraying substrate from bottom to top, and the spraying thickness was 2 mm, and the sprayed and cured coating below was covered with a plastic film. The test plan is as follows: place all the sprayed stainless steel plates together in the same closed container, which is placed outdoors and filled with simulated seawater. Half of the stainless steel plates to be tested are immersed in the simulated seawater and half are exposed to the air. The temperature of the closed container is controlled at 50°C, and there is a simulated seawater spray device on the top. The test duration is 1 year.
[0110] The above test results are specifically shown in Table 1 below.
[0111] Table 1 Performance test results of various embodiments and comparative examples
[0112]
[0113]
[0114]
[0115] From Table 1, we can see that:
[0116] (1) From the test data of Examples 1 to 8, it can be seen that the anti-corrosion and anti-seepage polyurea material obtained under the experimental conditions specified in this application has good hardness, tensile strength, elongation at break, adhesion and corrosion resistance, especially adhesion and corrosion resistance. Generally speaking, the adhesion between the coating material and the steel base of the seawater desalination device is not less than 8MPa. The adhesion of each embodiment of the present invention is about 19-21MPa, which is much greater than 8MPa; and the corrosion resistance is outstanding. After a simulated seawater corrosion test for 1 year, there is no obvious rust on the surface of the coating and the steel plate. After being immersed in a 150°C, 5% by mass NaOH solution for 8 hours, the mass loss rate is only 0.9%-1.5%.
[0117] (2) From the comparison of the test data of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 9, it can be seen that when preparing the amino-modified graphene / Zn / porous carbon composite, if the proportion of chitosan is too large, the proportion of porous carbon in the composite increases, and the hardness and tensile strength of the obtained polyurea material are improved to varying degrees, but the corrosion resistance is deteriorated; if the proportion of chitosan is small, the proportion of porous carbon in the composite decreases, and the corrosion resistance of the obtained polyurea material is good, but the hardness and tensile strength are significantly reduced. Obviously, the content of porous carbon in the composite needs to be limited to the range required by this application in order to obtain a polyurea material with better comprehensive performance.
[0118] From the comparison of the test data of Example 1, Comparative Example 3 and Comparative Example 4, it can be seen that when preparing the amino-modified graphene / Zn / porous carbon composite, if the proportion of graphite oxide is too small, its flaky structure cannot be used to improve the dispersibility of the composite. If the proportion of graphite oxide is relatively large, the content of zinc powder and porous carbon in the composite is relatively small, and the cathodic protection effect of the obtained polyurea material is weak. Both situations will result in slightly poor corrosion resistance of the obtained polyurea material and decreased physical properties.
[0119] The effective effect of the amino-modified graphene / Zn / porous carbon composite also depends on its addition amount. Too little or too much cannot effectively improve the physical properties and corrosion resistance of the polyurea material. Specifically, as shown in the test data of Example 1, Comparative Example 13, and Comparative Example 14: When too little is added, compared with Example 1, the corrosion resistance is slightly reduced, but the hardness, tensile strength, and elongation at break are significantly deteriorated; when too much is added, compared with Example 1, the hardness is significantly increased, but the tensile strength and elongation at break are reduced, and the corrosion resistance is significantly deteriorated. It may be that excessive addition, on the one hand, causes the system to be unable to bear the load, and its dispersibility becomes poor. On the other hand, too much porous carbon causes the corrosive medium to penetrate slowly, deteriorating the corrosion resistance.
[0120] (3) In the present application, ethylene vinyl acetate copolymer is a key raw material for improving the anti-corrosion and anti-permeability properties of polyurea materials and their adhesion to the steel-based spray surface. From the comparison of the test data of Example 1, Comparative Example 5, Comparative Example 10, Comparative Example 11, and Comparative Example 12, it can be seen that when ethylene vinyl acetate copolymer is not added or is replaced by an equal amount of other copolymers such as vinyl styrene-based copolymer, vinyl chloride-vinyl acetate copolymer, and ethylene-tetrafluoroethylene copolymer, it does not play a positive role in the main material of polyurea, and even some properties of the polyurea material are deteriorated.
[0121] Furthermore, the effect of ethylene vinyl acetate copolymer is subject to certain restrictions, that is, component B must be irradiated before use. If it is not irradiated, it will hardly have a significant effect on the polyurea main material after addition. If the irradiation time and dosage are not appropriate, although there is a certain degree of positive effect, it cannot achieve a satisfactory effect. The reason is that if the irradiation time is too long and the dosage is too large, the generated macromolecular peroxide may fail. If the irradiation time is too short and the dosage is too small, the content of the generated macromolecular peroxide is limited. In both cases, it is impossible to effectively promote the grafting of butadiene-benzoxazine copolymer and amino polyether, which is not conducive to the formation of polyurea materials with an interconductive network structure. Therefore, it has limited effect on improving the anti-corrosion and anti-seepage properties of polyurea materials.
[0122] Moreover, the butadiene-benzoxazine copolymer used in the present application is a butadiene-benzoxazine oligomer containing butadiene and benzoxazine. This is very important for improving the anti-corrosion and anti-seepage properties of the material. From the comparison of the test data of Example 1, Comparative Example 15, and Comparative Example 16, it can be seen that: when the copolymerization temperature of butadiene and benzoxazine is 90°C or the copolymerization time is too long, the resulting products butadiene-benzoxazine copolymer B and butadiene-benzoxazine copolymer C are used in this application and cannot achieve better use effects. The applicant speculates that a copolymerization temperature of 90°C may lead to excessive copolymerization to generate a high polymer product, which has no obvious effect on improving the anti-corrosion and anti-seepage properties of the polyurea material; if the copolymerization time is too long, the copolymerized monomers butadiene and benzoxazine are exhausted, and cannot play an auxiliary role in the subsequent process to promote the stable grafting of butadiene-benzoxazine copolymers with amino polyethers.
[0123] In summary, the polyurea coating formed by the anti-corrosion and anti-seepage polyurea material proposed in the present invention is continuous, dense, and has strong adhesion. It can effectively isolate the steel base or concrete base from the external corrosive medium, and then play a lasting and effective protective role. It is simple to construct, has a smooth and beautiful appearance, has good anti-corrosion and anti-seepage effects, a long service life and good comprehensive performance, and is specially used as an anti-corrosion coating required for seawater desalination projects such as seawater absorption, desalination, post-mineralization, transportation and distribution.
[0124] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Those skilled in the art may change, modify, replace and deform the above embodiments within the scope of the present invention. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.
Claims
1. A method for preparing an anticorrosive and anti-seepage polyurea material for seawater desalination, characterized in that: The anti-corrosion and anti-seepage polyurea material is prepared from component A and component B; Component A is an isocyanate-terminated semi-prepolymer obtained by prepolymerization of polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate; Component B includes amino polyether, amine chain extender, fluorocarbon resin with fluorine content ≥26%, ethylene vinyl acetate copolymer, butadiene-benzoxazine copolymer, amino modified graphene / Zn / porous carbon composite and additives, and the preparation method is: amino polyether, amine chain extender, fluorocarbon resin, amino modified graphene / Zn / porous carbon composite and part of the additives are mixed and stirred to obtain a first premix, ethylene vinyl acetate copolymer, butadiene-benzoxazine copolymer and the remaining additives are mixed and stirred to obtain a second premix, and the second premix is added to the first premix and stirred to obtain component B; When in use, first use an electron accelerator to irradiate component B with β rays in an inert atmosphere, the irradiation time is 15-25 minutes, the irradiation dose is 30-40 kGy, then mix component A and component B, stir evenly, and spray to form; The preparation steps of the amino-modified graphene / Zn / porous carbon composite are as follows: S1, preparing the graphene / Zn / porous carbon composite: ultrasonically dispersing graphite oxide in deionized water, first adding EDTA and zinc chloride and stirring until dissolved, then adding chitosan and stirring until dissolved, and finally reacting in a water reactor at 120-140°C for at least 24 hours to obtain a precursor mixture, wherein the mass ratio of the graphite oxide, zinc chloride, and chitosan is 3:(0.8-2):(0.5-1.1); first heating the precursor mixture to remove water, then drying, and finally calcining at 550-620°C in an inert atmosphere for at least 1 h, and obtain a graphene / Zn / porous carbon composite after grinding; S2, amino-modifying the graphene / Zn / porous carbon composite: dissolving the amino polyether in DMF to obtain a modifier, dispersing the graphene / Zn / porous carbon composite in deionized water containing PVP to obtain a mixture to be modified, adding the mixture to be modified to the modifier and stirring evenly to obtain a mixed system, under the protection of an inert gas, refluxing and stirring the mixed system at 100-110° C. for at least 5 h, then cooling to room temperature and collecting a solid phase, washing the solid phase with DMF, and vacuum drying to obtain an amino-modified graphene / Zn / porous carbon composite; The preparation method of the butadiene-benzoxazine copolymer in component B is as follows: adding paraformaldehyde, bisphenol A or bisphenol F or bisphenol S, and allylamine to DMF, reacting at 95-102° C. for 3-5 hours to obtain a benzoxazine monomer, and then adding an azo or peroxide free radical initiator to the benzoxazine monomer and butadiene at 65-72° C. for copolymerization, and the reaction time is controlled within 3 hours; the molar ratio of the benzoxazine monomer to butadiene is 1:(1-5), and the mass of the free radical initiator is 5-8wt% of the total mass of the benzoxazine monomer and butadiene.
2. The method for preparing the anticorrosive and anti-seepage polyurea material for seawater desalination according to claim 1, characterized in that: The molar ratio of -NCO in component A to -NH in component B is 1:(1.05-1.1).
3. The method for preparing the anticorrosive and anti-seepage polyurea material for seawater desalination according to claim 1 or 2, characterized in that: Component A is specifically obtained by prepolymerizing polyether polyol, aliphatic polyisocyanate and aromatic polyisocyanate in a mass ratio of 100:(60-80):(20-40); the contents of each component in component B are respectively 30-40wt% of amino polyether, 10-20wt% of amine chain extender, 10-15wt% of fluorocarbon resin, 8-20wt% of ethylene vinyl acetate copolymer, 10-15wt% of butadiene-benzoxazine copolymer, 5-12wt% of amino-modified graphene / Zn / porous carbon composite, and the remainder is auxiliary agent.
4. The method for preparing the anticorrosive and anti-seepage polyurea material for seawater desalination according to claim 3, characterized in that: The auxiliary agent is selected from one or more of the following components: pigment, diluent, defoamer, wetting agent, leveling agent, thickener, hydrophobic plasticizer, adhesion promoter, anti-settling agent; The pigment is at least one of titanium dioxide, barium dioxide, zinc dioxide, chromium oxide green, iron oxide red, iron oxide yellow, chrome yellow, iron black, carbon black and organic pigments; the diluent is a composition of propylene carbonate, ethyl carbonate and dibutyl phthalate in a mass ratio of 1:1:1; the defoamer is one of polyether-modified polysiloxane, high molecular polymer and fluorine-modified acrylic polymer; the wetting agent is a modified silicone wetting agent; the leveling agent is an acrylic copolymer leveling agent; the thickener is a non-ionic polyurethane associative thickener; the hydrophobic plasticizer is one of dioctyl phthalate, dioctyl terephthalate and dioctyl adipate; the adhesion promoter is one of γ-glycidyloxypropyltrimethylsilane, γ-glycidyloxypropyltriethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and the anti-settling agent is a compound of polyamide wax and hydrogenated castor oil.
5. An anti-corrosion and anti-seepage polyurea material used in seawater desalination, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Nano-modified polyaspartate polyurea heavy anti-corrosion coating and preparation method thereof
CN111662623A
Amino functionalized graphene modified polyurea long-acting anticorrosive coating layer and preparation method thereof
CN111500170A
Modified graphene enhanced impact-resistant polyurea coating and preparation method thereof
CN114015333A
Preparation method of zinc-doped three-dimensional graphene / hierarchical porous carbon water-based anticorrosive paint
CN114836119A
Graphene-modified Elastomer Material and Its Preparation Method