Cationic nano plugging agent for drilling coal rock horizontal wells and preparation method thereof
By preparing cationic modified nano-plugging agents with a particle size of less than 300 nm, the problem of sealing coal and rock cleavage and micro-fractures in deep coalbed methane horizontal wells was solved, achieving efficient sealing of coal and rock and wellbore stability, thus ensuring drilling safety.
Patent Information
- Application Number
- CN202411103175.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Existing drilling fluids are ineffective at sealing coal and rock cleavage and microfractures in deep coalbed methane horizontal wells, leading to a high risk of wellbore collapse. Furthermore, existing plugging agents have poor adsorption on coal and rock surfaces and insufficient sealing capacity.
A cationic modified nano-blocking agent with a particle size of less than 300 nm was prepared by surface modification of nano-silica particles and free radical polymerization reaction, which enhances the adsorption capacity and blocking effect on coal and rock.
It effectively seals micro- and nano-pores and fractures in coal and rock, stabilizes the wellbore, reduces the risk of wellbore collapse, and is suitable for safe drilling of deep coalbed methane horizontal wells.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petroleum drilling, and in particular relates to a cationic nano plugging agent for drilling coal rock horizontal wells and a preparation method thereof. Background Art
[0002] Deep coal rock has developed cleats and fissures, and the interbedded coal rock sections are prone to breaking and falling off. The problem of wellbore collapse during horizontal well drilling is particularly prominent, which restricts the safe and efficient construction of deep coalbed methane horizontal wells. Therefore, how to use water-based drilling fluid to plug coal rock cleats and micro-cracks, prevent liquid intrusion, and prevent wellbore collapse in deep coalbed methane horizontal well drilling is a prerequisite for the successful use of water-based drilling fluid and to ensure safe drilling. At present, the anti-collapse plugging agents in drilling fluids mainly include asphalt, polyol, nano-latex, and polymer-modified nanoparticles, which are used to plug formation pores and micro-cracks and prevent liquid intrusion. However, there are still many problems in adsorption on the coal rock surface and plugging of cleats and cracks. In the invention patent "Anti-temperature and anti-salt zwitterionic micro / nano cross-linked plugging agent and its preparation and application", Ren Yanjun et al. used 3-methacryloyl dopamine as a cross-linking monomer, 2-acrylamide-2-methylpropane sulfonic acid as an anionic monomer, N-vinyl pyrrolidone as a neutral monomer, and (3-acrylamide propyl) trimethyl ammonium chloride as an ionic liquid, and prepared a high-temperature and salt-resistant nano plugging agent for plugging shale pores at a molar ratio of (0.2-0.5): 1:1:1. Chinese patent CN114805709A discloses a method for preparing an ultra-high temperature resistant nano plugging agent with emulsion stability and its application in oil-based drilling fluid. Styrene, nano ZrO2 particles, flexible hydrophobic monomers, ionic liquids, high-temperature resistant hydrophilic monomers and emulsifiers are used for emulsification to obtain an oil-in-water emulsion, and then an initiator is added under nitrogen protection and the temperature is raised to 70-80°C and stirred, and the high-temperature and salt-resistant nano plugging agent is obtained after the reaction. However, this type of plugging agent has poor adsorption effect on the surface of coal rock, and its ability to plug the micro cracks of coal rock is not strong. Liu Jingping published a method for preparing a strong adsorption nano plugging agent by modified silica, ionic liquid, non-ionic monomer, pH regulator, and initiator in the patent "A strong adsorption plugging agent resistant to ultra-high temperature and high salt, and its preparation method and application". The plugging agent improves the plugging ability of the plugging agent by adsorbing the positive charge provided by the ionic liquid with the negative charge of the well wall, so that it can bridge and fill the formation cracks and pores through adsorption, thereby forming a dense and pressure-bearing plugging layer. However, the adsorption and plugging effect ability with coal rock needs to be verified. Chinese patent CN114957571A discloses a nano-spherical amphoteric polyelectrolyte brush plugging agent for water-based drilling fluid, its preparation method and application, and discloses an amino modification method for nano-SiO2 particles, but the monomer type used to prepare the plugging agent is zwitterion, which is not as good as cation in adsorption to coal rock. Patents CN108484828A and CN110734751A use cation-modified nano-SiO2 particles, and different cation types have different effects.
[0003] Therefore, the present invention provides a cationic modified nano plugging agent for water-based drilling fluid suitable for deep coalbed methane horizontal well drilling, which enhances the adsorption of nanoparticles to coal rock through the modification of multiple ionic liquids, and improves the plugging ability of cleats and microcracks. The cationic modified nano plugging agent can effectively plug micro-nano pores to prevent liquid phase from invading coal rock formations, and has a certain inhibitory effect, inhibiting the hydration of coal gangue in coal rock. It can be used in coalbed methane horizontal wells and shale horizontal wells to effectively plug micro-nano pores and cracks and keep the well wall stable. Summary of the invention
[0004] In view of the limitations of the prior art, the present invention provides a cationic nano plugging agent for drilling coal rock horizontal wells and a preparation method thereof. The provided composite plugging agent has a particle size of less than 300 nm and has a good plugging effect.
[0005] A cationic nano plugging agent for drilling coal rock horizontal wells, comprising the following components in parts by weight: 20-30 parts of nano silicon dioxide, 20-30 parts of silane coupling agent, 8-12 parts of substituent, 10-15 parts of catalyst A, 5-10 parts of initiator, 30-40 parts of ionic liquid, 1-3 parts of catalyst B, and 15-20 parts of non-ionic monomer;
[0006] The catalyst A is triethylamine; the catalyst B is C-94;
[0007] The ionic liquid is one or more of N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate.
[0008] Preferably, the mass ratio of the ionic liquid N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate is (0-6): (0-4): (0-6): (0-4).
[0009] Preferably, the ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate in a weight ratio of 4:6.
[0010] Preferably, the C-94 is a titanium / silicon oxide copolymer, wherein the Ti / Si molar mass ratio is 9:1.
[0011] Preferably, the silane coupling agent is one of γ-aminopropyltriethoxysilane coupling agent, γ-aminopropyltrimethoxysilane, and anilinemethyltrimethoxysilane; the substituent is 2-bromoisobutyryl; and the initiator is cuprous bromide.
[0012] Preferably, the nonionic monomer is styrene or parastyrene.
[0013] Preferably, the particle size of the nano-silicon dioxide is 70-100 nm.
[0014] A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well comprises the following steps:
[0015] (1) Dispersing nano-silicon dioxide to obtain a uniform suspension;
[0016] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1) to fully react to obtain amino-modified nano-silica particles;
[0017] (3) adding the nano-silica particles obtained in step (2) into toluene for dispersion, adding a substituent and a catalyst A for condensation reaction to obtain modified nano-silica particles, precipitating, filtering, and drying to obtain purified modified nano-silica particles;
[0018] (4) The purified and modified nano-silica particles and the initiator are dissolved in deionized water to prepare a solution with a mass concentration of 30%. After stirring and deoxygenation, non-ionic monomers are added under nitrogen protection to cause free radical polymerization. Ionic liquid and catalyst B are then added in sequence to prepare a cationic nano-blocking agent after a condensation reaction.
[0019] Preferably, the stirring speed of the free radical polymerization reaction in step (4) is 1500 rpm-2500 rpm.
[0020] Preferably, the reaction time of the free radical polymerization reaction in step (4) is 3h-5h.
[0021] Advantages of the present invention:
[0022] The cationic nano plugging agent for drilling coal rock horizontal wells provided by the present invention has a particle size of less than 300nm, and the surface of the nano plugging agent is flexibly coated with cationic groups, and has strong adsorption and deformation plugging capabilities with clay minerals or coal rock surfaces. The plugging agent particles are evenly dispersed in the solution, and have good plugging and inhibition properties, and can effectively stabilize the well wall to ensure safe drilling of coalbed methane horizontal wells when using water-based drilling fluids. Moreover, the plugging agent has good temperature resistance and stable product performance, and can be applied to the drilling needs of long horizontal sections of deep coalbed methane horizontal wells. DETAILED DESCRIPTION
[0023] Example 1
[0024] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 20 parts of nano silicon dioxide, 25 parts of silane coupling agent, 10 parts of substituent, 10 parts of catalyst A, 5 parts of initiator, 35 parts of ionic liquid, 3 parts of catalyst B, and 15 parts of non-ionic monomer;
[0025] The ionic liquid is 1-butyl-3-methylimidazolium bromide;
[0026] The silane coupling agent is γ-aminopropyltriethoxysilane coupling agent;
[0027] The nonionic monomer is p-styrene;
[0028] The substituent is 2-bromoisobutyryl;
[0029] The catalyst A is triethylamine;
[0030] The catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1;
[0031] The initiator is cuprous bromide.
[0032] 2. A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well, comprising the following steps:
[0033] (1) 70 nanometers of silica was dispersed in toluene to obtain a uniform suspension;
[0034] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1), and reacting the mixture at 85° C. for 2 h to obtain amino-modified nano-silica particles;
[0035] (3) adding the amino-modified nano-silica particles obtained in step (2) into toluene for dispersion, then adding a substituent and a catalyst A thereto for condensation reaction to obtain modified nano-silica particles, adding sufficient acetone for precipitation, filtering, and drying in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;
[0036] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. The solution was stirred and deoxygenated, and then non-ionic monomers were added under nitrogen protection. Free radical polymerization was carried out at a stirring speed of 1500 rpm for 5 h. Then, ionic liquid and catalyst B were added in sequence. After condensation reaction for 2 h, a cationic nano-blocking agent was prepared.
[0037] Example 2
[0038] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 30 parts of nano silicon dioxide, 30 parts of silane coupling agent, 8 parts of substituent, 15 parts of catalyst A, 7 parts of initiator, 35 parts of ionic liquid, 2 parts of catalyst B, and 20 parts of non-ionic monomer;
[0039] The ionic liquid is N-ethylpyridinium hexafluorophosphate
[0040] The silane coupling agent is aniline methyl trimethoxy silane;
[0041] The nonionic monomer is p-styrene;
[0042] The substituent is 2-bromoisobutyryl;
[0043] The catalyst A is triethylamine;
[0044] The catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1;
[0045] The initiator is cuprous bromide.
[0046] 2. A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well, comprising the following steps:
[0047] (1) 90 nanometers of silica was dispersed in toluene to obtain a uniform suspension;
[0048] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1), and reacting the mixture at 85° C. for 2 h to obtain amino-modified nano-silica particles;
[0049] (3) adding the amino-modified nano-silica particles obtained in step (2) into toluene for dispersion, then adding a substituent and a catalyst A thereto for condensation reaction to obtain modified nano-silica particles, adding sufficient acetone for precipitation, filtering, and drying in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;
[0050] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. After stirring and deoxygenation, non-ionic monomers were added under nitrogen protection. Free radical polymerization was carried out at a stirring speed of 2500 rpm for 3 hours. Then, ionic liquid and catalyst B were added in sequence. After condensation reaction for 2 hours, a cationic nano-blocking agent was prepared.
[0051] Example 3
[0052] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 27 parts of nano silicon dioxide, 24 parts of silane coupling agent, 12 parts of substituent, 13 parts of catalyst A, 10 parts of initiator, 30 parts of ionic liquid, 1 part of catalyst B, and 20 parts of non-ionic monomer;
[0053] The ionic liquid is 1-octyl-3-methylimidazolium trifluoromethanesulfonate;
[0054] The silane coupling agent is γ-aminopropyltrimethoxysilane;
[0055] The nonionic monomer is styrene;
[0056] The substituent is 2-bromoisobutyryl;
[0057] The catalyst A is triethylamine;
[0058] The catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1;
[0059] The initiator is cuprous bromide.
[0060] 2. A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well, comprising the following steps:
[0061] (1) 100 nanometers of silica was dispersed in toluene to obtain a uniform suspension;
[0062] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1), and reacting the mixture at 85° C. for 2 h to obtain amino-modified nano-silica particles;
[0063] (3) adding the amino-modified nano-silica particles obtained in step (2) into toluene for dispersion, then adding a substituent and a catalyst A thereto for condensation reaction to obtain modified nano-silica particles, adding sufficient acetone for precipitation, filtering, and drying in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;
[0064] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. The solution was stirred and deoxygenated, and then non-ionic monomers were added under nitrogen protection. Free radical polymerization was carried out at a stirring speed of 2200 rpm for 3.5 hours. Then, ionic liquid and catalyst B were added in sequence. After condensation reaction for 2 hours, a cationic nano-blocking agent was prepared.
[0065] Example 4
[0066] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 27 parts of nano silicon dioxide, 25 parts of silane coupling agent, 10 parts of substituent, 12 parts of catalyst A, 7 parts of initiator, 38 parts of ionic liquid, 2 parts of catalyst B, and 17 parts of non-ionic monomer;
[0067] The ionic liquid is 1-butyl-3-methylimidazole methyl sulfate;
[0068] The silane coupling agent is aniline methyl trimethoxy silane;
[0069] The nonionic monomer is styrene;
[0070] The substituent is 2-bromoisobutyryl;
[0071] The catalyst A is triethylamine;
[0072] The catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1;
[0073] The initiator is cuprous bromide.
[0074] The preparation method is the same as that in Example 3.
[0075] Example 5
[0076] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 25 parts of nano silicon dioxide, 20 parts of silane coupling agent, 10 parts of substituent, 12 parts of catalyst A, 5 parts of initiator, 38 parts of ionic liquid, 2 parts of catalyst B, and 17 parts of non-ionic monomer;
[0077] The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-butyl-3-methylimidazolium methyl sulfate, and the weight ratio is 4:4;
[0078] The silane coupling agent is aniline methyl trimethoxy silane;
[0079] The nonionic monomer is styrene;
[0080] The substituent is 2-bromoisobutyryl;
[0081] The catalyst A is triethylamine;
[0082] The catalyst B is C-94, which is a titanium / silicon oxide copolymer, wherein the molar mass ratio of Ti / Si is 9:1;
[0083] The initiator is cuprous bromide.
[0084] The preparation method is the same as that in Example 3.
[0085] Example 6
[0086] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 25 parts of nano silicon dioxide, 23 parts of silane coupling agent, 10 parts of substituent, 12 parts of catalyst A, 5 parts of initiator, 38 parts of ionic liquid, 2 parts of catalyst B, and 18 parts of non-ionic monomer;
[0087] The ionic liquid is 1-butyl-3-methylimidazolium bromide and N-ethylpyridinium hexafluorophosphate, and the weight ratio thereof is 4:6;
[0088] The silane coupling agent, substituent, catalyst A, initiator, catalyst B and non-ionic monomer are the same as those in Example 5.
[0089] 2. A method for preparing a cationic nano plugging agent for drilling coal rock horizontal wells, same as Example 3.
[0090] Example 7
[0091] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer;
[0092] The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 4:6;
[0093] The silane coupling agent, substituent, catalyst A, initiator, catalyst B and non-ionic monomer are the same as those in Example 3.
[0094] 2. A method for preparing a cationic nano plugging agent for drilling coal rock horizontal wells, same as Example 3.
[0095] Example 8
[0096] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 27 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer;
[0097] The ionic liquid is N-ethylpyridinium hexafluorophosphate and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 6:6;
[0098] The silane coupling agent, substituent, catalyst A, initiator, catalyst B and non-ionic monomer are the same as those in Example 3.
[0099] 2. A method for preparing a cationic nano plugging agent for drilling coal rock horizontal wells, same as Example 3.
[0100] Example 9
[0101] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer;
[0102] The ionic liquid is N-ethylpyridinium hexafluorophosphate and 1-butyl-3-methylimidazole methyl sulfate, with a weight ratio of 6:1;
[0103] The silane coupling agent, substituent, catalyst A, initiator, catalyst B and non-ionic monomer are the same as those in Example 3.
[0104] 2. A method for preparing a cationic nano plugging agent for drilling coal rock horizontal wells, same as Example 3.
[0105] Comparative Example 1
[0106] The ionic liquid was replaced with dimethyldiallylammonium chloride, and the rest was the same as in Example 7.
[0107] Comparative Example 2
[0108] No nonionic monomer is added, and the rest is the same as in Example 7, specifically:
[0109] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, and 3 parts of catalyst B;
[0110] The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 4:6;
[0111] The silane coupling agent, substituent, catalyst A, initiator and catalyst B are the same as those in Example 7.
[0112] 2. A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well, comprising the following steps:
[0113] (1) 100 nanometers of silica was dispersed in toluene to obtain a uniform suspension;
[0114] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1), and reacting the mixture at 85° C. for 2 h to obtain amino-modified nano-silica particles;
[0115] (3) adding the amino-modified nano-silica particles obtained in step (2) into toluene for dispersion, then adding a substituent and a catalyst A thereto for condensation reaction to obtain modified nano-silica particles, adding sufficient acetone for precipitation, filtering, and drying in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;
[0116] (4) The purified and modified nano-silica particles and the initiator were dissolved in deionized water to prepare a solution with a mass concentration of 30%. After stirring and deoxygenation, ionic liquid and catalyst B were added in sequence under nitrogen protection. After condensation reaction for 2 hours, a cationic modified nano-SiO2 plugging agent was prepared.
[0117] Comparative Example 3
[0118] The nonionic monomer, ionic liquid and catalyst B are added together, and the rest is the same as in Example 6, specifically:
[0119] 1. A cationic nano plugging agent for drilling coal rock horizontal wells, composed of the following components in parts by weight: 23 parts of nano silicon dioxide, 25 parts of silane coupling agent, 12 parts of substituent, 10 parts of catalyst A, 7 parts of initiator, 40 parts of ionic liquid, 3 parts of catalyst B, and 20 parts of non-ionic monomer;
[0120] The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 4:6;
[0121] The silane coupling agent, substituent, catalyst A, initiator, catalyst B and non-ionic monomer are the same as those in Example 3.
[0122] 2. A method for preparing a cationic nano plugging agent for drilling a coal rock horizontal well, comprising the following steps:
[0123] (1) 100 nanometers of silica was dispersed in toluene to obtain a uniform suspension;
[0124] (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1), and reacting the mixture at 85° C. for 2 h to obtain amino-modified nano-silica particles;
[0125] (3) adding the amino-modified nano-silica particles obtained in step (2) into toluene for dispersion, then adding a substituent and a catalyst A thereto for condensation reaction to obtain modified nano-silica particles, adding sufficient acetone for precipitation, filtering, and drying in a vacuum environment at 80°C for 8 hours to obtain purified modified nano-silica particles;
[0126] (4) The purified and modified nano-silica particles and the initiator are dissolved in deionized water to prepare a solution with a mass concentration of 30%. After stirring and deoxygenation, non-ionic monomers, ionic liquids, and catalyst B are added in sequence under nitrogen protection. After sufficient reaction, a cationic nano-blocking agent is prepared.
[0127] Experimental example:
[0128] The plugging agents synthesized in the examples and comparative examples were evaluated as follows: particle size distribution test, API filtration loss test, and plugging rate test.
[0129] 1. Particle size distribution test
[0130] Deionized water was used to prepare 2% mass fraction sample solutions of the embodiments and comparative examples. 5 mL of each sample solution of the embodiments and comparative examples was taken. The particle size distribution of each embodiment and comparative example was measured using a Malvern Zetasizer Nano ZS particle size analyzer according to the instrument operation steps. The results are shown in Table 1.
[0131] Table 1 Evaluation results of particle size distribution of nano plugging agents
[0132]
[0133] From the experimental results in Table 1, it can be seen that the cationic modified nano plugging agent D prepared in Examples 1 to 9 90 The particle size distribution range is 106-764nm, D 50 The particle size distribution range is 48-228nm, which is nanometer level.
[0134] Wherein D of Example 7 90 The particle size is 106nm, with the best particle size and distribution range. Under the action of the bottom hole pressure difference, the plugging agent can effectively plug the micro-nano cleats and cracks in the coal rock, reduce the intrusion of the water phase, and thus stabilize the wellbore. After changing the monomer components, proportions and preparation conditions, the particle size distribution range of the plugging agent becomes larger. Compared with Examples 1-4, the ionic liquid is a single type, and the prepared plugging agent D 90 The particle size distribution is 384-764nm, and the particle size is relatively large. Example 5-9, plugging agent D prepared when there are two types of ionic liquids 90 The particle size distribution is 106-296nm, all below 300nm, with a smaller particle size and a better particle size distribution range. Especially when the ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethane sulfonate, the weight ratio is 4:6, the prepared plugging agent D 50 Particle size 48nm, D 90 The particle size is 106nm, which meets the nanoscale requirements and has the best particle size distribution range.
[0135] Compared with Example 7, Comparative Example 2 does not add nonionic monomers, the ionic liquid in Comparative Example 1 is dimethyldiallyl ammonium chloride, and in Comparative Example 3, a nonionic monomer, an ionic liquid, and a catalyst are added together to prepare a plugging agent. 90 The particle size distribution is between 1964-3860nm, and the particle size is too large to meet the technical requirements of nano-blocking.
[0136] 2. API filtration loss test
[0137] Preparation of base slurry: Measure 400 mL of clean water and place it in a high-stirring cup, stir at high speed (5000 r / min), then slowly add 16 g of drilling-grade bentonite and 0.56 g of NaCO3 into the cup respectively, seal and stir at low speed at room temperature for 24 hours to obtain 4% bentonite base slurry. Prepare multiple portions of the above base slurry for later use.
[0138] This experiment uses an API medium-pressure filter loss meter. First, 2% of the plugging agent prepared in the embodiment and the comparative example was added to a 4% bentonite slurry, and then the slurry was put into an aging tank and aged at 120°C for 16 hours. The aged slurry was put into the API medium-pressure filter loss meter, and the filtration loss of the base slurry and the sample slurry was tested for 30 minutes under 0.7MPa. The experimental results are shown in Table 2.
[0139] 3. Blockage rate test
[0140] The preparation process of base slurry and sample slurry is as in Experimental Example 2. The plugging rate is evaluated by using a low permeability sand disk plugging instrument. The test conditions are 120°C and a pressure difference of 3.5 MPa for 30 min. The plugging rate is calculated by testing the original permeability P0 of the simulated core. The permeability of the core after the plugging agent solution acts is P1, and the plugging rate R0=(P0-P1) / P0×100%. The experimental results are shown in Table 2.
[0141] Table 2 Evaluation results of filtration reduction and plugging performance of nano plugging agents
[0142]
[0143] From the results in Table 2, it can be seen that after using the plugging agent prepared by the present invention, the filtration loss of the base slurry is reduced and the plugging rate is significantly improved, which shows that the prepared plugging agent has good plugging ability. In Examples 1-4, the ionic liquid is a single type, and the filtration loss of the prepared plugging agent is 14.6-15.5mL, and the plugging rate is 70.2-71.6%; as in Examples 5-9, when there are two ionic liquids, especially in Example 7, the ionic liquids are 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and the weight ratio is 4:6, the medium pressure filtration loss of the prepared plugging agent after hot rolling is 9.8mL, and the plugging rate reaches 88.4%, and the filtration loss reduction and plugging ability of the prepared plugging agent are significantly enhanced.
[0144] Compared with Example 7, no non-ionic monomer was added in Comparative Example 2, the ionic liquid in Comparative Example 1 was dimethyldiallyl ammonium chloride, and the plugging agent prepared by adding non-ionic monomer, ionic liquid and catalyst together in Comparative Example 3 had a significantly increased filtration loss and a decreased plugging rate.
Claims
1. A cationic nano plugging agent for drilling coal rock horizontal wells, Features: The invention is composed of the following components in parts by weight: 20-30 parts of nano silicon dioxide, 20-30 parts of silane coupling agent, 8-12 parts of substituent, 10-15 parts of catalyst A, 5-10 parts of initiator, 30-40 parts of ionic liquid, 1-3 parts of catalyst B and 15-20 parts of non-ionic monomer; The catalyst A is triethylamine; the catalyst B is C-94; The ionic liquid is one or more of N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate; The substituent is 2-bromoisobutyryl; The nonionic monomer is styrene.
2. The cationic nano plugging agent for drilling coal rock horizontal wells according to claim 1, Features: The mass ratio of the ionic liquid N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate is (0-6): (0-4): (0-6): (0-4), and the amounts of the ionic liquid N-ethylpyridinium hexafluorophosphate, 1-butyl-3-methylimidazolium bromide, 1-octyl-3-methylimidazolium trifluoromethanesulfonate, and 1-butyl-3-methylimidazolium methyl sulfate cannot be zero at the same time.
3. The cationic nano plugging agent for drilling coal rock horizontal wells according to claim 1 or 2, Features: The ionic liquid is 1-butyl-3-methylimidazolium bromide and 1-octyl-3-methylimidazolium trifluoromethanesulfonate, with a weight ratio of 4:
6.
4. The cationic nano plugging agent for drilling coal rock horizontal wells according to claim 1, Features: The silane coupling agent is one of γ-aminopropyltriethoxysilane coupling agent, γ-aminopropyltrimethoxysilane and anilinemethyltrimethoxysilane; and the initiator is cuprous bromide.
5. The cationic nano plugging agent for drilling coal rock horizontal wells according to claim 1, Features: The particle size of the nano silicon dioxide is 70-100 nm.
6. A method for preparing a cationic nano plugging agent for drilling coal and rock horizontal wells according to any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) Dispersing nano-silicon dioxide to obtain a uniform suspension; (2) adding a silane coupling agent dropwise to the uniform suspension obtained in step (1) to fully react to obtain amino-modified nano-silica particles; (3) adding the nano-silica particles obtained in step (2) into toluene for dispersion, adding a substituent and a catalyst A for condensation reaction to obtain modified nano-silica particles, precipitating, filtering, and drying to obtain purified modified nano-silica particles; (4) The purified and modified nano-silica particles and the initiator are dissolved in deionized water to prepare a solution with a mass concentration of 30%. After stirring and deoxygenation, a non-ionic monomer is added under nitrogen protection to cause a free radical polymerization reaction. Then, the ionic liquid and catalyst B are added in sequence to obtain a cationic nano-blocking agent after a condensation reaction.
7. The method for preparing the cationic nano plugging agent for drilling coal rock horizontal wells according to claim 6, It is characterized in that The stirring speed of the free radical polymerization reaction in step (4) is 1500rpm-2500rpm.
8. The method for preparing the cationic nano plugging agent for drilling coal rock horizontal wells according to claim 6, Features: The reaction time of the free radical polymerization reaction in step (4) is 3h-5h.