A method for recycling tungsten wire for waste diamond wire

Through calcination, wet grinding, ultrasonic centrifugation and reducing gas treatment, the problems of excessive use of chemical reagents and environmental pollution in the existing tungsten wire recycling process are solved, and efficient and low-cost tungsten wire recycling is achieved, which improves the regenerated tungsten powder purity and recovery rate.

CN118653062BActive Publication Date: 2024-12-03GANZHOU NONFERROUS METALLURGICAL RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411154532.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-12-03
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing tungsten wire recycling process requires a large amount of chemical reagents, which leads to high costs and environmental pollution, limiting its industrialization development.

Method used

By using calcining, wet milling, ultrasonic centrifugal separation and reducing gas reduction methods, the dependence on chemical reagents is reduced and the recovery and purity is improved.

Benefits of technology

It realizes efficient and low-cost tungsten wire recycling, reduces the risk of environmental pollution, simplifies equipment and processes, and improves the purity and recovery rate of recycled tungsten powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653062B_ABST
    Figure CN118653062B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of tungsten wire recovery, and in particular to a method for recovering tungsten wire for waste diamond wire. The method provided by the present invention comprises the following steps: first calcining the cleaned waste tungsten wire to obtain calcined tungsten wire; wet grinding the calcined tungsten wire under dispersant conditions and then sieving to obtain a mixed powder of tungsten trioxide powder and tungsten particles; mixing the mixed powder with water, and sequentially ultrasonicating and centrifuging the obtained mixed liquid to obtain tungsten particles with residual dispersant and tungsten trioxide powder respectively; cyclically calcining, wet grinding, sieving, ultrasonicating and centrifuging the tungsten particles; removing the dispersant from the above-obtained tungsten trioxide powder to obtain pure tungsten trioxide powder; reducing the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder. The present invention has a short process, simple equipment, does not require a large amount of chemical reagents, has low cost, and has little environmental pollution, and can realize industrial rapid recovery of waste tungsten wires of diamond wires.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tungsten wire recovery, and in particular to a method for recovering tungsten wire for waste diamond wire. Background Art

[0002] Tungsten diamond wire has the excellent characteristics of high hardness, high strength, high temperature resistance and corrosion resistance, and has been widely used in the silicon material cutting industry. With the continuous increase in the market demand for silicon wafers, the demand for tungsten diamond wire is increasing. At present, the yield rate of tungsten diamond wire production is around 50%, which leads to the production of a large amount of waste tungsten wire for diamond wire. As an important strategic resource, the recycling of metal tungsten is of great strategic significance.

[0003] Chinese patent 202410408452.7 proposes a process for recycling nickel-plated tungsten wire diamond cutting wire, which uses concentrated sulfuric acid for acid leaching to remove nickel from the surface of the tungsten wire, and uses hydrogen peroxide to catalyze the reaction, thereby quickly separating the tungsten wire busbar. This method requires the use of a large amount of solution reagents, which is costly and has potential environmental pollution risks. Chinese patent 202310283839.X proposes a method for electrolytic recovery of tungsten wire, which can reduce the use of solution reagents to a certain extent, but still requires the use of alkaline solution to complete the final recovery process. At present, the mainstream process for recycling tungsten wire waste is hydrometallurgical technology, which generally requires the use of solution reagents, including concentrated sulfuric acid, hydrogen peroxide and sodium hydroxide. The use of these reagents will lead to high recovery costs on the one hand, and on the other hand, there are certain environmental pollution problems, which greatly limits its industrial development. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a method for recycling tungsten wire for waste diamond wire. The method provided by the present invention has a short process, simple equipment, no need for a large amount of chemical reagents, low cost, and the obtained recycled tungsten powder has a high recovery rate and purity.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for recycling tungsten wire for waste diamond wire, comprising the following steps:

[0007] (1) calcining the cleaned waste tungsten wire to obtain calcined tungsten wire;

[0008] (2) Wet-grinding the calcined tungsten wire under dispersant conditions and then sieving to obtain a mixed powder of tungsten trioxide powder and tungsten particles;

[0009] (3) mixing the mixed powder with water, and subjecting the obtained mixed solution to ultrasonic and centrifugal separation in sequence to obtain tungsten particles with residual dispersant and tungsten trioxide powder, respectively;

[0010] (4) subjecting the tungsten particles obtained in step (3) to a first calcination, wet grinding, screening, ultrasonication and centrifugal separation in a cycle;

[0011] (5) removing the dispersant from the tungsten trioxide powder obtained in step (3) and step (4) to obtain pure tungsten trioxide powder;

[0012] (6) Reducing the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder.

[0013] Preferably, the first calcination is performed in an oxygen-rich atmosphere, the temperature of the first calcination is 700-1200° C., and the holding time is 1-8 h.

[0014] Preferably, the ball-to-material ratio of the wet grinding is (4-12):1, the rotation speed is 300-600 rpm, and the wet grinding time is 30-180 min; the wet grinding medium includes water or ethanol.

[0015] Preferably, the reduction temperature is 800-1000° C., and the reduction time is 30-120 min.

[0016] Preferably, the dispersant is a carboxylate dispersant and / or a polyol dispersant.

[0017] Preferably, the polyol dispersant includes isopropyl alcohol and / or polyethylene glycol.

[0018] Preferably, the oxygen-rich atmosphere comprises oxygen or air.

[0019] Preferably, the reducing gas comprises H2 or CO.

[0020] Preferably, the cleaned waste tungsten wire is obtained by ultrasonically cleaning the waste tungsten wire.

[0021] Preferably, the method of removing the dispersant is a second calcination; the temperature of the second calcination is 500-1000° C., and the calcination time is 20-90 min.

[0022] The present invention provides a method for recycling tungsten wire for waste diamond wire, comprising the following steps: (1) first calcining the cleaned waste tungsten wire to obtain calcined tungsten wire; (2) wet-grinding the calcined tungsten wire under dispersant conditions and then sieving to obtain a mixed powder of tungsten trioxide powder and tungsten particles; (3) mixing the mixed powder with water, and sequentially subjecting the obtained mixed solution to ultrasonic and centrifugal separation to obtain tungsten particles with residual dispersant and tungsten trioxide powder respectively; (4) cyclically subjecting the tungsten particles obtained in step (3) to first calcination, wet-grinding, sieving, ultrasonic and centrifugal separation; (5) removing the dispersant from the tungsten trioxide powder obtained in steps (3) and (4) to obtain pure tungsten trioxide powder; (6) reducing the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder. The present invention adopts the centrifugal separation technology to separate the tungsten particles and the tungsten trioxide particles, thereby ensuring that the oxide layer on the surface of the waste tungsten wire is peeled off and the internal tungsten wire can continue to be oxidized, thereby improving both the production efficiency and the oxidation rate of the waste tungsten wire. The invention obtains regenerated tungsten powder with high purity and recovery rate by fully oxidizing the tungsten wire and then fully reducing it.

[0023] In addition, the present invention has a short process, simple equipment, does not require a large amount of chemical reagents, has low cost, and causes little environmental pollution, and can realize industrial rapid recovery of diamond wire and tungsten wire waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the method for recycling tungsten wire for waste diamond wire in Examples 1 to 5. DETAILED DESCRIPTION

[0025] The present invention provides a method for recycling tungsten wire for waste diamond wire, comprising the following steps:

[0026] (1) calcining the cleaned waste tungsten wire to obtain calcined tungsten wire;

[0027] (2) Wet-grinding the calcined tungsten wire under dispersant conditions and then sieving to obtain a mixed powder of tungsten trioxide powder and tungsten particles;

[0028] (3) mixing the mixed powder with water, and subjecting the obtained mixed solution to ultrasonic and centrifugal separation in sequence to obtain tungsten particles with residual dispersant and tungsten trioxide powder, respectively;

[0029] (4) subjecting the tungsten particles obtained in step (3) to a first calcination, wet grinding, screening, ultrasonication and centrifugal separation in a cycle;

[0030] (5) removing the dispersant from the tungsten trioxide powder obtained in step (3) and step (4) to obtain pure tungsten trioxide powder;

[0031] (6) Reducing the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder.

[0032] The present invention performs a first calcination on the cleaned waste tungsten wire to obtain a calcined tungsten wire.

[0033] In the present invention, the cleaned waste tungsten wire is preferably obtained by ultrasonically cleaning the waste tungsten wire.

[0034] In the present invention, the diameter of the waste tungsten wire is preferably 30-2000 μm, more preferably 50-1500 μm.

[0035] In the present invention, the first calcination is preferably carried out in an oxygen-rich atmosphere, and the oxygen-rich atmosphere preferably includes oxygen or air, and more preferably oxygen. The temperature of the first calcination is preferably 700-1200°C, and more preferably 800-1000°C; the holding time is preferably 1-8 h, and more preferably 2-6 h. In the present invention, the heating rate to the temperature of the first calcination is preferably 5-15°C / min, and more preferably 8-10°C / min.

[0036] After obtaining the calcined tungsten wire, the present invention wet-grinds the calcined tungsten wire under dispersant conditions and then sieves it to obtain a mixed powder of tungsten trioxide powder and tungsten particles.

[0037] In the present invention, the dispersant is preferably a carboxylate dispersant and / or a polyol dispersant. In the present invention, the carboxylate dispersant preferably includes polyacrylic acid and / or maleic acid / acrylic acid copolymer. In the present invention, the polyol dispersant preferably includes isopropyl alcohol and / or polyethylene glycol.

[0038] In the present invention, the mass ratio of the calcined tungsten wire to the dispersant is preferably (100-200):1, more preferably (120-160):1.

[0039] In the present invention, the ball-to-material ratio of the wet grinding is preferably (4-12):1, more preferably (5-10):1; the rotation speed is preferably 300-600 rpm, more preferably 500 rpm; the wet grinding time is preferably 30-180 min, more preferably 50-150 min; and the wet grinding medium preferably includes water or ethanol.

[0040] In the present invention, the particle size of the sieve is preferably 150-300 mesh, more preferably 200-250 mesh.

[0041] After sieving, the sieve material is preferably subjected to repeated first calcination, wet grinding and sieving to obtain the sieve material, that is, a mixed powder of tungsten trioxide powder and tungsten particles. In the present invention, the repetition number is preferably 1 to 2 times.

[0042] In the present invention, when the diameter of the waste tungsten wire is 30-50 μm, the first calcination, wet grinding and screening do not need to be repeated, because the particle size is very fine and the combustion is very complete (containing a small amount of tungsten particles), so it does not need to be recycled again, which will not affect the subsequent industrial process and can save energy.

[0043] After obtaining the mixed powder of tungsten trioxide powder and tungsten particles, the present invention mixes the mixed powder with water, and the obtained mixed solution is subjected to ultrasonic and centrifugal separation in sequence to obtain tungsten particles with residual dispersant and tungsten trioxide powder, respectively.

[0044] In the present invention, the mass ratio of the mixed powder to water is preferably 1:(10-20), more preferably 1:(14-16).

[0045] In the present invention, the frequency of the ultrasound is preferably 20-80 Hz, more preferably 40-60 Hz, and the time is preferably 30-90 min, more preferably 40-60 min. In the present invention, the speed of the centrifugal separation is preferably 3000-8000 rpm, more preferably 5000-6000 rpm, and the time is preferably 10-60 min, more preferably 20-40 min.

[0046] After obtaining the tungsten particles, the present invention cycles through the steps of first calcination, wet grinding, screening, ultrasonication and centrifugal separation.

[0047] In the present invention, the number of cycles is preferably 1 to 2 times.

[0048] The present invention removes the dispersant from the obtained tungsten trioxide powder to obtain pure tungsten trioxide powder.

[0049] In the present invention, the method for removing the dispersant is preferably a second calcination; the temperature of the second calcination is preferably 500-1000°C, more preferably 700-900°C, and the calcination time is preferably 20-90 min, more preferably 30-70 min. In the present invention, the heating rate to the temperature of the second calcination is preferably 5-15°C / min, more preferably 8-10°C / min.

[0050] After obtaining the pure tungsten trioxide powder, the present invention reduces the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder.

[0051] In the present invention, the reducing gas preferably includes H2 or CO, more preferably H2. In the present invention, the reduction temperature is preferably 800-1000°C, more preferably 900°C, and the reduction time is preferably 30-120 min, preferably 50-100 min. In the present invention, the heating rate to the reduction temperature is preferably 5-15°C / min, more preferably 8-10°C / min.

[0052] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention. Example 1

[0053] Figure 1 Schematic diagram of the method for recycling tungsten wire for waste diamond wire in Examples 1 to 5, as shown in Figure 1 As shown, the recycling method is:

[0054] (1) 1000 g of waste diamond wire tungsten wire (diameter 2000 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0055] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 800°C (heating rate of 10°C / min) and a calcination time of 3 h to obtain 1100 g of calcined tungsten wire.

[0056] (3) The calcined tungsten wire obtained in step (2) and 11 g of polyethylene glycol were mixed and wet-milled using a high-energy ball mill with a ball-to-material ratio of 4:1, a rotation speed of 300 rpm, H2O as the wet milling medium, and a wet milling time of 180 min.

[0057] (4) The material after wet grinding in step (3) was sieved through a 300-mesh sieve to obtain the undersize, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles; the oversize was calcined, wet-milled and sieved twice to obtain 1170 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0058] 17.5 kg of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency was 50 Hz, time was 60 min) and centrifugal separation (speed was 5000 rpm, time was 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively.

[0059] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0060] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 800°C (heating rate is 10°C / min) and the calcination time is 120 min.

[0061] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 995.3 g of regenerated tungsten powder. The reduction temperature was 1000°C (heating rate was 10°C / min) and the reduction time was 30 min.

[0062] After calculation, the recovery rate of tungsten element is 99.53%. Example 2

[0063] (1) 1000 g of waste diamond wire tungsten wire (with a diameter of 1000 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0064] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 700°C (heating rate of 10°C / min) and a calcination time of 8 h to obtain 1120 g of calcined tungsten wire.

[0065] (3) The calcined tungsten wire obtained in step (2) was mixed with 7.84 g of isopropanol using a high-energy ball mill, and then wet-milled at a ball-to-material ratio of 4:1, a rotation speed of 450 rpm, ethanol as the wet milling medium, and a wet milling time of 120 min.

[0066] (4) The material after wet grinding in step (3) is sieved through a 250-mesh sieve to obtain the undersize material, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles; the oversize material is calcined, wet-milled, and sieved twice to obtain 1190 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0067] 17.8 kg of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency was 50 Hz, time was 60 min) and centrifugal separation (speed was 5000 rpm, time was 30 min) to obtain tungsten particles and tungsten trioxide powder respectively, and then the obtained tungsten particles and tungsten trioxide powder were separated;

[0068] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0069] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 500°C (heating rate is 10°C / min) and the calcination time is 120 min.

[0070] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 998.1 g of regenerated tungsten powder. The reduction temperature was 900°C (heating rate was 10°C / min) and the reduction time was 60 min.

[0071] After calculation, the recovery rate of tungsten element is 99.81%. Example 3

[0072] (1) 1000 g of waste diamond wire tungsten wire (with a diameter of 50 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0073] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 800°C (heating rate of 10°C / min) and a calcination time of 6 h to obtain 1160 g of calcined tungsten wire.

[0074] (3) The calcined tungsten wire obtained in step (2) and 8.12 g of polyethylene glycol were wet-milled using a high-energy ball mill with a ball-to-material ratio of 8:1, a rotation speed of 450 rpm, water as the wet milling medium, and a wet milling time of 120 min.

[0075] (4) The material after wet grinding in step (3) is passed through a 200-mesh sieve to obtain the undersize material, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles; the oversize material is subjected to the steps of calcination, wet grinding and sieving once to obtain 1195 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0076] 18.0 kg of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency was 50 Hz, time was 60 min) and centrifugal separation (speed was 5000 rpm, time was 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively.

[0077] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0078] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 600°C (heating rate is 10°C / min) and the calcination time is 100 min.

[0079] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 996.5 g of regenerated tungsten powder. The reduction temperature was 900°C (heating rate was 10°C / min) and the reduction time was 60 min.

[0080] After calculation, the recovery rate of tungsten element is 99.65%. Example 4

[0081] (1) 1000 g of waste diamond wire tungsten wire (with a diameter of 500 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0082] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 900°C (heating rate of 10°C / min) and a calcination time of 4 h to obtain 1140 g of calcined tungsten wire.

[0083] (3) The calcined tungsten wire obtained in step (2) was mixed with 7.98 g of isopropanol using a high-energy ball mill, and then wet-milled at a ball-to-material ratio of 8:1, a rotation speed of 450 rpm, water as the wet milling medium, and a wet milling time of 90 min.

[0084] (4) The material after wet grinding in step (3) is passed through a 200-mesh sieve to obtain the undersize material, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles; the oversize material is subjected to the steps of calcination, wet grinding and sieving twice to obtain 1180 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0085] 17.7 kg of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency was 50 Hz, time was 60 min) and centrifugal separation (speed was 5000 rpm, time was 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively.

[0086] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0087] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 800°C (heating rate is 10°C / min) and the calcination time is 60 min.

[0088] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 996.2 g of regenerated tungsten powder. The reduction temperature was 1000°C (heating rate was 10°C / min) and the reduction time was 30 min.

[0089] After calculation, the recovery rate of tungsten element is 99.62%. Example 5

[0090] (1) 1000 g of waste diamond wire tungsten wire (with a diameter of 1000 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0091] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 1000°C (heating rate of 10°C / min) and a calcination time of 3 h to obtain 1130 g of calcined tungsten wire.

[0092] (3) The calcined tungsten wire obtained in step (2) and 7.91 g of polyethylene glycol were wet-milled using a high-energy ball mill with a ball-to-material ratio of 8:1, a rotation speed of 600 rpm, a solution medium of water, and a wet-milling time of 90 min.

[0093] (4) The material after wet grinding in step (3) is sieved through a 250-mesh sieve to obtain the undersize material, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles; the oversize material is subjected to the steps of calcination, wet grinding and sieving twice to obtain 1180 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0094] 17.7 g of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency of 50 Hz, time of 60 min) and centrifugal separation (speed of 5000 rpm, time of 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively.

[0095] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0096] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 900°C (heating rate is 10°C / min) and the calcination time is 40 min.

[0097] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 997.5 g of regenerated tungsten powder. The reduction temperature was 850°C (heating rate was 10°C / min) and the reduction time was 60 min.

[0098] After calculation, the recovery rate of tungsten element is 99.75%. Example 6

[0099] (1) 1000 g of waste diamond wire tungsten wire (with a diameter of 50 μm) was ultrasonically cleaned to obtain cleaned waste tungsten wire.

[0100] (2) The cleaned waste tungsten wire was calcined in a calcination furnace at a temperature of 1100°C (heating rate of 10°C / min) and a calcination time of 2 h to obtain 1190 g of calcined tungsten wire.

[0101] (3) The calcined tungsten wire obtained in step (2) was mixed with 8.3 g of isopropanol and then wet-milled using a high-energy ball mill. The ball-to-material ratio was 12:1, the rotation speed was 300 rpm, the wet milling medium was water, and the wet milling time was 60 minn.

[0102] (4) The material after wet grinding in step (3) was passed through a 150-mesh sieve to obtain the sieve-under material, i.e., a mixed powder containing tungsten trioxide powder and tungsten particles, to obtain 1195 g of a mixed powder containing tungsten trioxide powder and tungsten particles;

[0103] 17.93 kg of water was added to the mixed powder, and ultrasonic centrifuge was used for ultrasonication (ultrasonic frequency of 50 Hz, time of 60 min) and centrifugal separation (speed of 5000 rpm, time of 30 min) to obtain tungsten particles and tungsten trioxide powder, respectively.

[0104] (5) Using a calcining furnace, the tungsten particles obtained in step (4) are returned to step (2) for calcination, and the process of steps (3) and (4) is repeated once.

[0105] (6) The tungsten trioxide powder in step (4) and step (5) is placed in a calcining furnace for calcination to remove the dispersant to obtain tungsten trioxide powder. The calcination temperature is 900°C (heating rate is 10°C / min) and the calcination time is 30 min.

[0106] (7) Using a rotary reduction furnace, the tungsten trioxide powder in step (6) was reduced in hydrogen to obtain 998.6 g of regenerated tungsten powder. The reduction temperature was 900°C (heating rate was 10°C / min) and the reduction time was 60 min.

[0107] After calculation, the recovery rate of tungsten element is 99.86%.

[0108] Comparative Example 1

[0109] The waste tungsten wire is electrolyzed, with the waste tungsten wire as the anode, the inert electrode as the cathode, and a 3 mol / L hydrochloric acid solution as the electrolyte. The electrolysis lasts for 8 minutes, and the nickel on the surface of the tungsten wire is dissolved in the electrolyte to obtain the tungsten wire;

[0110] The tungsten wire is subjected to high temperature rapid cooling and embrittlement (the temperature at high temperature is 800°C, and the final temperature during cooling is 80°C), and then crushed to obtain tungsten particles;

[0111] The tungsten particles are activated and oxidized at high temperature (temperature is 900°C), and the tungsten particles are oxidized to obtain tungsten trioxide particles;

[0112] The tungsten trioxide particles are immersed in a 0.6 mol / L sodium hydroxide solution for alkali leaching for 2 h to obtain alkali metal tungstate.

[0113] The final recovery rate of tungsten element was 99.21%.

[0114] Comparative Example 2

[0115] The waste tungsten wire is electrolyzed, with the waste tungsten wire as the anode, the inert electrode as the cathode, and a 3 mol / L hydrochloric acid solution as the electrolyte. The electrolysis lasts for 12 minutes, and the nickel on the surface of the tungsten wire is dissolved in the electrolyte to obtain the tungsten wire;

[0116] The tungsten wire is subjected to high temperature rapid cooling and embrittlement (the temperature at high temperature is 800°C, and the final temperature during cooling is 80°C), and then crushed to obtain tungsten particles;

[0117] The tungsten particles are activated and oxidized at high temperature (temperature is 900°C), and the tungsten particles are oxidized to obtain tungsten trioxide particles;

[0118] The tungsten trioxide particles are immersed in a 0.6 mol / L sodium hydroxide solution for alkali leaching for 4 hours to obtain alkali metal tungstate.

[0119] The final recovery rate of tungsten element was 99.38%.

[0120] Comparative Example 3

[0121] The waste tungsten wire is electrolyzed, with the waste tungsten wire as the anode, the inert electrode as the cathode, and a 3 mol / L hydrochloric acid solution as the electrolyte. The electrolysis is carried out for 20 minutes, and the nickel on the surface of the tungsten wire is dissolved in the electrolyte to obtain the tungsten wire;

[0122] The tungsten wire is subjected to high temperature rapid cooling and embrittlement (the temperature at high temperature is 800°C, and the final temperature during cooling is 80°C), and then crushed to obtain tungsten particles;

[0123] The tungsten particles are activated and oxidized at high temperature (temperature is 900°C), and the tungsten particles are oxidized to obtain tungsten trioxide particles;

[0124] The tungsten trioxide particles are immersed in a 0.6 mol / L sodium hydroxide solution for alkali leaching for 6 hours to obtain alkali metal tungstate.

[0125] The final recovery rate of tungsten element was 99.43%.

[0126] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for recycling tungsten wire for waste diamond wire, characterized in that: The following steps are involved: (1) calcining the cleaned waste tungsten wire to obtain calcined tungsten wire; (2) Wet-grinding the calcined tungsten wire under dispersant conditions and then sieving to obtain a mixed powder of tungsten trioxide powder and tungsten particles; (3) mixing the mixed powder with water, and subjecting the obtained mixed solution to ultrasonic and centrifugal separation in sequence to obtain tungsten particles with residual dispersant and tungsten trioxide powder, respectively; (4) subjecting the tungsten particles obtained in step (3) to a first calcination, wet grinding, screening, ultrasonication and centrifugal separation in a cycle; (5) removing the dispersant from the tungsten trioxide powder obtained in step (3) and step (4) to obtain pure tungsten trioxide powder; (6) Reducing the pure tungsten trioxide powder in a reducing gas to obtain regenerated tungsten powder; The dispersant is a carboxylate dispersant and / or a polyol dispersant.

2. The method according to claim 1, characterized in that The first calcination is performed in an oxygen-rich atmosphere, the temperature of the first calcination is 700-1200° C., and the holding time is 1-8 h.

3. The method according to claim 1, characterized in that The ball-to-material ratio of the wet grinding is (4-12):1, the rotation speed is 300-600 rpm, and the wet grinding time is 30-180 min; the medium of the wet grinding includes water or ethanol.

4. The method according to claim 1, characterized in that The reduction temperature is 800-1000°C, and the reduction time is 30-120 min.

5. The method according to claim 1, characterized in that The polyol dispersant includes isopropyl alcohol and / or polyethylene glycol.

6. The method according to claim 2, characterized in that The oxygen-rich atmosphere includes oxygen or air.

7. The method according to claim 1, characterized in that The reducing gas includes H2 or CO.

8. The method according to claim 1, characterized in that The cleaned waste tungsten wire is obtained by ultrasonically cleaning the waste tungsten wire.

9. The method according to claim 8, characterized in that The method for removing the dispersant is a second calcination; the temperature of the second calcination is 500-1000° C., and the calcination time is 20-90 min.