A kind of eutectoid carbon cold heading steel wire rod for 13.9 grade bolts and its manufacturing method

Through the design of eutectoid carbon chemical composition and the online molten salt strong isothermal and hot air roller strong slow cooling technology, the microstructure of cold heading steel strips is regulated, and the cost and brittleness problems of high alloys and microalloys are solved, achieving high Cold heading steel strips for grade 13.9 bolts that match strength and plasticity reduce material costs and improve material yield.

CN118653096BActive Publication Date: 2024-11-29JIANGSU YONGGANG GROUP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411133216.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing cold heading steel strips for grade 13.9 bolts have challenges in improving strength and cost. High alloy content and microalloy composition increase material costs, and are prone to brittleness and crack sensitivity, affecting material formation rate and plastic toughness properties.

Method used

Using eutectoid carbon chemical composition design, the content of C, Si, Mn is controlled, and through solid solution strengthening and microstructure regulation, a microstructure including tempered soxunite and tempered pearlite is formed, combined with online molten salt strength Isotherm hot air roller strong and slow cooling technology regulates the structure and cooling speed of the strips to reduce brittleness and crack sensitivity.

Benefits of technology

The tensile strength is 1150~1200MPa and the cross-section shrinkage rate is 43%~48%, which reduces the brittleness and tensile hardening ability of cold-headed steel strips, significantly reduces the material cost, improves the material yield and plasticity, and is suitable for In manufacturing fasteners such as 13.9-level bolts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118653096B_ABST
    Figure CN118653096B_ABST
Patent Text Reader

Abstract

The invention relates to a eutectoid carbon cold heading steel wire rod for 13.9-grade bolts and a manufacturing method thereof. After controlled rolling and spinning into a wire rod based on the chemical composition of the eutectoid carbon, online molten salt strong isothermal treatment is performed, so that the wire rod is cooled to a pearlite phase region at a cooling rate of ≥35°C / s for strong isothermal phase transformation, pearlite and troostite phase transformation is promoted and high-temperature tempering occurs, and finally, the wire rod is subjected to strong slow cooling through a hot air roller to be made into a cold heading steel wire rod having a microstructure including a small portion of tempered pearlite and a large portion of tempered troostite. The cold heading steel wire rod can achieve a tensile strength of 1150-1200MPa, a cross-sectional shrinkage of 43%-48%, and a network carbide level of 0, effectively reducing the brittleness, crack sensitivity and tensile hardening resistance of the cold heading steel wire rod, achieving high strength and plasticity matching, and is used for manufacturing fasteners such as 13.9-grade bolts, and can significantly reduce the material cost of steel mills and downstream users, improve the yield rate, and has good industrial adaptability and market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a eutectoid carbon cold-heading steel wire rod for 13.9-grade bolts and a manufacturing method thereof. Background Art

[0002] Fasteners such as bolts and nuts are standard connectors and are widely used in various manufacturing fields such as automobiles, metallurgical industry, high-speed trains, and ships. The main fasteners currently used are mainly grade 8.8 and grade 10.9. With the increase in strength grade, higher requirements are placed on the process design and equipment performance of steel mills and fastener product manufacturing. The existing cold heading steel wire rod for 13.9 grade bolts will use 42CrMo material, adding V, Nb and other micro-alloys to strengthen the raw material matrix strength. After the bolt factory is cold-headed, it forms a composite strengthening process through rolling fillet and shot peening process to improve the strength of the finished cold heading steel to meet the performance requirements of 13.9 grade bolts. For example: Patent CN116288056A discloses a bolt steel and its production method and heat treatment method, which adopts C-Si-Mn-Al-Mo-Cr-Ni-Tb composition design, combines low-temperature wire drawing and Stelmor wire insulation cooling process to obtain pearlite + ferrite + a small amount of bainite structure, and then heat treatment to achieve the performance level, but on the one hand, the high alloy content and micro-alloy composition The addition of microalloy components increases the material cost. At the same time, in order to avoid the formation of hard and brittle martensitic structure under high cooling rate, the pearlite structure interlamellar spacing is large and the strength is insufficient after the wire rod is cooled through the Stelmor line. In order to reduce the material cost, reducing the alloy content or omitting the alloy component will bring obvious strength loss. On the other hand, the addition of high alloy content and microalloy components increases the hardenability of the material, making it easier to obtain bainite under low cooling rate conditions. Although the matrix strength is improved, the dislocation density and distortion of the bainitic structure are high, which seriously damages the plasticity and toughness of the wire rod and is prone to brittle fracture, which is not conducive to the coiling, transportation and uncoiling of the wire rod, and will lead to waste of raw materials and a decrease in the yield rate, which brings cost pressure to steel mills and downstream users.

[0003] As a basic and economical element in steel, the addition of carbon instead of other alloys is conducive to reducing material costs. However, the high-carbon component system for drawing is mainly used in applications such as cords, tire rims, and hoses. Due to the limited cooling capacity of the Stelmor air-cooled wire, the spinning temperature will be appropriately increased to extend the time of the wire rod in the troostite transformation temperature range, thereby increasing the troostite content in the organization. The troostite ratio is generally above 85% to increase the strength and drawing performance of the wire rod. The technical difficulties and causes of its component system and organization being difficult to apply to cold heading steel wire rods for 13.9 grade bolts are:

[0004] On the one hand, compared with hypoeutectoid steel, eutectoid steel has higher material strength, hardness and wear resistance. With the increase of carbon content, the cooling rate of the wire rod after rolling and spinning is reduced. Although it is beneficial to the incubation of troostite in the wire rod structure, if the cooling rate is too slow, it will stay in the secondary cementite interval and the tertiary cementite peak interval for a long time. The carbon atoms on the grain boundaries have greater free energy and are easy to precipitate in the grain boundaries in a network, severing the connection between the tissues, increasing the brittleness and crack sensitivity of the material, and aggravating the occurrence of intergranular fracture of high carbon steel wire rod drawing. If the spinning temperature is excessively increased, there will also be a risk of decarburization causing drawing fracture during the rolling process, which can easily cause grain coarsening and affect the strength and toughness of the wire rod.

[0005] On the other hand, the minimum cooling capacity of the Stelmore air-cooling line is limited. Even if the wire rod is slowly cooled by heat preservation after spinning, the transformation time in the troostite phase region under continuous cooling is still relatively short, which will lead to a larger spacing between troostite lamellae. At the same time, after troostite inoculation, the wire rod is already in a low temperature state, and the troostite dislocation density is large, which will produce a large drawing hardening, which is not conducive to deep drawing and cold heading. If the spinning temperature is appropriately lowered and the cooling rate of the wire rod after spinning is increased to reduce the troostite content in the organization and increase the pearlite or ferrite content in the organization for strong plasticity regulation, then due to the limited maximum cooling capacity of the Stelmore air-cooling line, the improvement of the network carbide is limited. At the same time, the temperature difference between the windward and leeward sides of the wire rod is large when it is cooled by air, and bainite or even martensite structure is prone to appear locally, causing the increase of mechanical fluctuation of the wire rod, aggravating the risk of wire breakage and cold heading cracking. The time of the wire rod in the pearlite and troostite phase transformation temperature range is further shortened, the lamella spacing and organizational stress are further increased, and the plasticity improvement effect of the wire rod is limited. Summary of the invention

[0006] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a eutectoid carbon cold heading steel wire rod for 13.9 grade bolts and a manufacturing method thereof, which can combine the eutectoid carbon chemical composition design and the microstructure and performance regulation of the hot-rolled wire rod to achieve strength-plasticity matching, and can be used for the cold heading manufacturing of 13.9 grade bolts, which can reduce material costs and improve the yield rate.

[0007] The technical solution adopted by the present invention to solve its technical problem is:

[0008] A eutectoid carbon cold heading steel wire rod for 13.9 grade bolts, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.75%-0.79%, Si: 0.20%-0.40%, Mn: 0.45%-0.55%, P≤0.015%, S≤0.015%, the rest is Fe and unavoidable impurities, and the microstructure includes tempered pearlite accounting for 32%-39% by volume and tempered troostite accounting for 61%-68% by volume.

[0009] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:

[0010] (1) Carbon: The carbon element is the main strengthening element of the present invention. It is cheaper than other elements in steel. As an austenite-forming element, it can promote the formation of austenite, help to provide the matrix strength of the material through solid solution strengthening and precipitation strengthening, and determine the amount of carbides precipitated in the finished bolt after quenching and tempering heat treatment, thereby affecting the final hardness and strength of the bolt. However, it also increases the risk of decarburization and the risk of cementite being distributed in a network along the grain boundary. In addition, if the carbon content is too high, the temperature of the bainite phase region is higher, which is not conducive to microstructure control. Therefore, in order to facilitate microstructure control, ensure the cold deformation performance of cold heading steel wire rod, and meet the final performance level requirements of 13.9 grade fasteners without adding high alloy and micro alloy components, the mass percentage of carbon is controlled to be 0.75%~0.79%.

[0011] (2) Silicon: The Si element is often added to steel as a deoxidizer during the smelting process. It can dissolve in austenite to achieve a solid solution strengthening effect, thereby improving the hardness and strength of the steel. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization, and reduce the cold heading forming performance of the material. Therefore, the mass percentage of Si is controlled to be 0.20%~0.40%.

[0012] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. As an austenite-forming element, it can promote the formation of austenite and further improve the strength and hardenability of steel through precipitation strengthening and solid solution strengthening. However, while improving the strength of steel, excessive Mn content will aggravate the segregation during the solidification of the steel billet, resulting in poor uniformity of the steel, increasing the tendency of grain coarsening during the heating process of the material, and increasing the difficulty of controlling the cooling structure. In addition, excessive Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.45%~0.55%.

[0013] (4) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.

[0014] The cold heading steel wire rod adopts the eutectoid carbon chemical composition design, replaces the high alloy content and the addition of expensive micro-alloy components with the lower cost C element, and provides higher matrix strength through solid solution strengthening and microstructure regulation. Compared with the eutectoid wire rod structure of troostite + ferrite obtained after traditional controlled rolling and controlled cooling, the cold heading steel wire rod includes most of tempered troostite and a small part of tempered pearlite. The tempered troostite retains the troostite structure interlamellar spacing finer than the pearlite structure and has higher strength. The bainite structure has the characteristics of smaller distortion and better plasticity. Tempering is used to further reduce the dislocation density of the troostite structure to improve the plasticity of the wire rod and reduce draw hardening. The tempered pearlite retains the characteristics of larger interlamellar spacing and better plasticity than the troostite structure, and higher strength than the ferrite structure. The troostite is combined with a small amount of pearlite to provide better matrix plasticity before tempering. After tempering, the pearlite structure is transformed into tempered pearlite with smaller organizational stress and dislocation density, so that the plasticity of the final cold heading steel wire rod can be further improved.

[0015] Compared with the cold heading steel wire rod which obtains full bainite or a small amount of bainite complex phase structure after traditional controlled rolling and controlled cooling, the cold heading steel wire rod uses solid solution strengthening and refinement of the interlamellar spacing to obtain a strength that is not inferior to the existing 13.9 grade cold heading steel wire rod for bolts, and has significantly improved plasticity, thereby avoiding the brittleness of the wire rod caused by the bainite structure, and is not easy to break during the coiling, transportation and uncoiling of the wire rod, thereby improving the yield rate, drawing and cold heading performance of the cold heading steel wire rod, breaking the application limitation of the eutectoid carbon chemical composition in the field of high-strength grade bolt cold heading, and can effectively reduce costs and reduce raw material waste.

[0016] In a preferred embodiment, the interlamellar spacing of the tempered pearlite is 165-200 nm, which can further avoid the disadvantages of too high interlamellar spacing on matrix strength and drawing deformation ability.

[0017] In a preferred embodiment, the interlamellar spacing of the tempered troostite is 100-145 nm, which can further avoid the disadvantageous effect of too low interlamellar spacing on the plasticity of the matrix.

[0018] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which can further avoid the brittleness and crack sensitivity caused by the network carbides precipitated along the grain boundaries, and effectively alleviate the local cracking problem caused by this during the drawing and cold heading process.

[0019] In a preferred embodiment, the diameter of the cold heading steel wire rod is 18.0~28.0mm, the tensile strength is 1150~1200MPa, and the cross-sectional shrinkage rate is 43%~48%. It has higher tensile strength and significantly improved cross-sectional shrinkage rate than the existing cold heading steel wire rod. It can be used as a raw material to manufacture fasteners such as 13.9 grade bolts through spheroidizing annealing, drawing, cold heading and tempering processes.

[0020] A method for manufacturing a eutectoid carbon cold heading steel wire rod for 13.9 grade bolts, the manufacturing method comprising:

[0021] According to the chemical composition of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts as described above, the wire rod is produced by controlled rolling. After the wire rod is spun into a wire rod at a spinning temperature of ≥910°C, it is subjected to online molten salt strong isothermal treatment, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥35°C / s for strong isothermal phase transformation, promoting pearlite and bainite phase transformation and high temperature tempering, and finally subjected to hot air roller strong slow cooling to produce a cold heading steel wire rod having a microstructure including 32% to 39% by volume of tempered pearlite and 61% to 68% by volume of tempered bainite.

[0022] The above-mentioned manufacturing method adopts online molten salt strong isothermal treatment directly after spinning. Compared with the Stelmore air-cooling rapid cooling process, it can utilize the high-speed heat exchange characteristics of molten salt to make the molten salt and wire rod evenly and quickly exchange heat. On the one hand, the wire rod enters the pearlite phase temperature range more quickly from the austenitizing temperature after spinning, avoiding the wire rod from staying in the secondary cementite range of 750~820℃ and the tertiary cementite peak range of 700~800℃ for a long time, which can effectively reduce the level of network carbides and alleviate the grain coarsening caused by tertiary cementite precipitation, so that the grains are finer and the plasticity and toughness of the eutectoid carbon steel matrix are improved.

[0023] On the other hand, quickly skipping the phase transformation temperature range of ferrite and entering the pearlite phase region with a large degree of supercooling for strong isothermal treatment is beneficial to the transformation of austenite structure into troostite with finer interlamellar spacing. The austenite structure in the wire rod structure can be transformed into most of the troostite and a small part of the pearlite structure, regulating the strength and plasticity of the matrix structure. When the wire rod passes through the molten salt, the molten salt can cover the surface of the wire rod. Compared with Stelmor air cooling, there is no strong temperature difference problem between the windward side and the leeward side. When the alloy content is less and the hardenability of the wire rod is relatively low, It can prevent the wire rod from falling into the temperature range of the bainite phase and producing hard and brittle bainite. At the same time, compared with the slow cooling or delayed cooling by Stelmor insulation, it is not the continuous cooling by Stelmor insulation after cooling, but the continuous high-temperature isothermal treatment of the wire rod and the molten salt temperature. The use of online molten salt strong isothermal treatment can significantly extend the time of the wire rod in the pearlite phase region. After the tissue incubation, the wire rod is still in a high temperature state, which further promotes the high-temperature tempering of the pearlite and troostite tissues formed by the incubation, reduces the tissue stress and dislocation density, and significantly improves the plasticity of the wire rod.

[0024] After a long period of online molten salt strong isothermal treatment, the structure is fully transformed into tempered troostite and tempered pearlite, and the risk of residual austenite transforming into bainite under subsequent cooling is avoided. Finally, compared with insulation and slow cooling, hot air is used to further reduce the cooling rate of the wire rod after online molten salt strong isothermal treatment, prolong the high temperature state, promote further softening of the wire rod structure, and obtain the final structure and strength-plasticity matching of the cold heading steel wire rod. Compared with direct insulation and slow cooling after spinning, the above manufacturing method combines online molten salt strong isothermal treatment with superheated air roller strong slow cooling, and also has faster production efficiency.

[0025] In a preferred embodiment, during the controlled rolling, the heating temperature of the steel billet is controlled to be ≤1100°C and the furnace time is controlled to be ≤4.5h before rolling, which can promote the uniform diffusion of high carbon components and avoid the risks of burning and decarburization.

[0026] In a preferred embodiment, the controlled rolling adopts low-temperature controlled rolling, the initial rolling temperature is controlled to 1065~1085℃, the initial rolling reduction is 29%~39%, and a lower initial rolling temperature is used to prevent the aggravation of high-temperature decarburization, so that the depth of the decarburization layer is ≤0.45% of the diameter. It also avoids excessively low initial rolling temperature that limits the initial rolling reduction and aggravates the wear of the rolling mill. Under a larger initial rolling reduction, columnar crystals are destroyed to prepare for grain refinement.

[0027] In a preferred embodiment, the controlled rolling controls the final rolling temperature to be ≥935°C, the final rolling reduction to be 38%~46%, and the appropriate final rolling temperature is selected to improve the rolling efficiency. Combined with a larger final rolling reduction, the rolling within the austenite grain recrystallization temperature range can achieve the purpose of grain refinement and provide higher base surface structure strength.

[0028] In a preferred embodiment, the final rolling temperature is 935-980° C. Selecting a lower final rolling temperature can further avoid high-temperature decarburization and further coarsening of recrystallized grains during the rolling process.

[0029] In a preferred embodiment, the spinning temperature is 910-940°C. Selecting a lower spinning temperature can further avoid grain coarsening, austenitization to prepare for the deformation nuclei of sorbite and pearlite phases, and avoid the spinning temperature being too low, causing the rolling temperature to be too low, aggravating the wear of the rolling mill, affecting the rolling efficiency, precipitating network carbides or reducing the degree of supercooling in the spinning stage, which is not conducive to the nucleation of sorbite.

[0030] In a preferred embodiment, the online molten salt strong isothermal control molten salt temperature is 555-605°C, and the processing time is 510-650s. The lower the molten salt temperature, the more favorable it is for forming a higher proportion of troostite structure with finer interlamellar spacing, so that the strength of the wire rod increases and the plasticity decreases. However, if the molten salt temperature is too low, an excessively high proportion of troostite structure or even a small amount of bainite structure is formed, which is not conducive to the plasticity of the matrix. On the contrary, the higher the molten salt temperature, the more favorable it is for forming a higher proportion of pearlite structure with coarser interlamellar spacing. With a longer processing time, it is beneficial to promote high-temperature tempering of pearlite and troostite, so that the strength of the wire rod decreases. However, if the molten salt temperature is too high, a too low proportion of troostite or even a certain amount of ferrite will be formed. The grain coarsening will occur due to the precipitation of tertiary cementite due to the slow cooling rate, which is not conducive to the strength and plasticity of the wire rod. If the treatment time is too long, it will cause excessive loss of matrix strength. If the treatment time is too short, it will be difficult to temper and soften the pearlite and troostite structures, which will cause the plasticity of the wire rod to decrease and be easy to harden by drawing. Therefore, the molten salt temperature and treatment time can be further controlled, the pearlite and troostite content of the wire rod can be controlled, and the high-temperature tempering softening effect of the pearlite and troostite structures can be adjusted, thereby adjusting the matching of the strength and plasticity of the wire rod.

[0031] In a preferred embodiment, the online molten salt strong isothermal control molten salt circulation rate is 530~730t / h, and the molten salt temperature rise is ≤8°C. Since the wire rod quickly drops to the molten salt temperature after passing through the online molten salt, the spinning temperature is quite different from the molten salt temperature. A higher molten salt circulation rate is used to control the molten salt temperature rise to maintain a larger supercooling degree and wire rod cooling rate, thereby further improving the uniformity of microstructure phase change and high-temperature tempering.

[0032] In a preferred embodiment, the hot air roller strong slow cooling adopts a roller to transport the wire rod into the insulation cover, and controls the wire rod to be cooled to below 350°C at a cooling rate of 0.1~0.45°C / s with hot air above 300°C. Compared with extending the length of the salt bath tank in the online molten salt strong isothermal stage, the high temperature state of the wire rod out of the salt bath tank and the length of the roller for transporting it to the winding station can be utilized to make the production more economical. When the insulation cover is closed, compared with the existing Stelmor insulation process, the hot air in the insulation cover is used to maintain the high temperature atmosphere to further reduce the cooling rate of the wire rod, so that the wire rod after phase change tempering can be further tempered and softened at a continuous high temperature.

[0033] In a preferred embodiment, the hot air originates from the hot air on the online molten salt strong isothermal tank. Since the air temperature above the online molten salt isothermal salt bath tank is relatively high, it is transported to the insulation cover and used as hot air to control the cooling speed of the wire rod. The thermal energy of the hot air on the tank can be further recycled to reduce production energy consumption. After the wire rod is cooled to below 350°C, the wire rod is transported to the coil at a roller speed of 0.6~0.9m / s. After the wire rod is cooled to below 350°C, the tempering softening effect is weakened. The wire rod can be quickly offline by increasing the roller speed, thereby improving production efficiency.

[0034] Compared with the prior art, the beneficial effects of the present invention are at least:

[0035] (1) Aiming at the current situation that the main fasteners used are mainly 8.8 and 10.9 grades, as the strength grade is increased to 13.9 grade, the cost and yield rate of steel mills are greatly restricted, and the strength and plasticity of the products after controlled rolling and controlled cooling are difficult to be balanced, the present invention provides a 13.9 grade eutectoid carbon cold heading steel wire rod for bolts, which adopts the eutectoid carbon chemical composition design, does not add high alloy content and expensive microalloy components, forms a microstructure including most tempered troostite and a small part of tempered pearlite through solid solution strengthening and microstructure regulation, can achieve a tensile strength of 1150~1200MPa, a cross-sectional reduction rate of 43%~48%, and a network carbide level of 0, effectively reducing the brittleness, crack sensitivity and tensile hardening ability of the cold heading steel wire rod, achieving high strength and plasticity matching, and is used to manufacture 13.9 grade bolts and other fasteners, which can significantly reduce the material cost of steel mills and downstream users, improve the yield rate, and has good market application prospects.

[0036] (2) In view of the current situation that the Stelmor air cooling process after spinning has greatly limited the manufacturing and production efficiency of eutectoid carbon steel for cold heading steel wire rods for 13.9 grade bolts, the manufacturing method of the present invention is based on the chemical composition of eutectoid carbon, combined with online molten salt strong isothermal and roller strong slow cooling technology, and utilizes the high-speed heat exchange capacity of molten salt to control the wire rod to quickly enter the pearlite phase region with a large degree of supercooling for strong isothermal phase transformation, avoid the wire rod from staying in the secondary cementite range and the tertiary cementite peak range for a long time, control the pearlite and troostite content of the wire rod, and promote high-temperature tempering of the pearlite and troostite structure to soften the matrix, and finally soften the structure through hot air roller strong slow cooling, effectively reducing the stress and dislocation density of the structure, successfully manufacturing cold heading steel wire rod with higher production efficiency, and having good industrial adaptability and market application prospects.

[0037] (3) The manufacturing method of the present invention is combined with low-temperature controlled rolling to further prevent the aggravation of high-temperature decarburization and the further coarsening of recrystallized grains during the rolling process, thereby improving the overall grain refinement effect and avoiding the aggravation of rolling mill wear caused by too low temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0039] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;

[0040] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;

[0041] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION

[0042] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:

[0043] A preferred embodiment of the manufacturing method of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.79%, Si: 0.38%, Mn: 0.45%, P: 0.015%, S: 0.013%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature controlled rolling → wire laying → online molten salt strong isothermal → hot air roller strong slow cooling → coiling, specifically:

[0044] The low-temperature controlled rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high-carbon components and avoid the risks of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 28mm through a rolling line. Low-temperature controlled rolling is used to prevent the aggravation of high-temperature decarburization, so that the rolling within the recrystallization temperature range of the austenite grains can achieve the purpose of grain refinement. Specifically: the heating temperature of the steel billet is controlled to be 1095°C, the time in the furnace is 4.2h, the initial rolling temperature is 1080°C, the initial rolling reduction is 29%, the final rolling temperature is 960°C, the final rolling reduction is 38%, and the decarburization layer depth is ≤0.45% of the diameter.

[0045] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 925°C.

[0046] The online molten salt strong isothermal treatment adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by a roller and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 36°C / s for strong isothermal phase transformation, avoiding the wire rod to stay in the secondary cementite interval and the tertiary cementite peak interval for a long time, quickly skipping the ferrite phase transformation temperature interval, entering the pearlite phase region with a large degree of supercooling, controlling the pearlite and troostite content of the wire rod, avoiding the generation of hard and brittle bainite phase, and promoting high-temperature tempering of pearlite and troostite structures, reducing organizational stress and dislocation density, and softening the matrix. Specifically: the molten salt temperature is controlled to be 586°C, the processing time is 615s, the molten salt circulation volume is 600t / h, and the molten salt temperature rise is ≤8°C.

[0047] The hot air roller strong slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is transported into the insulation cover by the roller, and the hot air generated above the salt bath tank is transported into the insulation cover as hot air for strong slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.3m / s, and the wire rod is cooled to 348℃ at a cooling rate of 0.3℃ / s by hot air above 300℃, and then the wire rod is transported to the coil at a roller speed of 0.75m / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 310℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as shown in Figure 1 shown.

[0048] Comparative Example 1:

[0049] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → wire laying → Stelmor insulation and slow cooling → coiling, specifically: the heating temperature of the steel billet is controlled to be 1150°C, the time in the furnace is 4h, the initial rolling temperature is 1135°C, the final rolling temperature is 1000°C, the wire laying temperature is 980°C, the Stelmor insulation and slow cooling adopts closing all fans and insulation covers, and the wire rod is conveyed by rollers. The wire rod completes phase change at a cooling rate of 2.9°C / s in the cover, and the finished wire rod is obtained after coiling off the line.

[0050] Comparative Example 2:

[0051] A method for manufacturing a wire rod, which differs from that of Example 1 in that the method is manufactured according to a process flow of controlled rolling → wire laying → Stelmor rapid cooling → roller slow cooling → coiling, specifically: controlling the heating temperature of the steel billet to be 1050°C, the furnace time to be 5h, the initial rolling temperature to be 1030°C, the final rolling temperature to be 900°C, the wire laying temperature to be 880°C, the Stelmor rapid cooling adopts opening 1~7# fans at 75%, so that the wire rod is cooled to 650°C at a cooling rate of 5.5°C / s, the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1.4°C / s, and the finished wire rod is obtained after coiling off the line.

[0052] Comparative Example 3:

[0053] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling → roller slow cooling. Specifically: the Stelmor rapid cooling is performed by opening 1~5# fans at 95%, so that the wire rod is cooled to 625°C at a cooling rate of 9.5°C / s; the roller slow cooling is performed by closing all fans and insulation covers, so that the wire rod completes a phase change in the cover at a cooling rate of 0.9°C / s, and the finished wire rod is obtained after it comes off the line.

[0054] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:

[0055] Table 1. Comparison of wire rod structure and properties by different manufacturing methods

[0056]

[0057] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the troostite and ferrite structures obtained by high-temperature spinning and Stelmor insulation slow cooling, although the strength is higher, the cooling rate is too slow, and it will stay in the secondary cementite range and the tertiary cementite peak range for a long time, which increases the brittleness and crack sensitivity of the material. The present invention adopts the chemical composition of eutectic carbon, combines online molten salt strong isothermal and roller strong slow cooling technology, and utilizes the high-speed heat exchange capacity of molten salt to control the wire rod to quickly enter the pearlite phase region with a large degree of supercooling for strong isothermal phase transformation, thereby avoiding the wire rod from staying in the secondary cementite range and the tertiary cementite peak range for a long time, and effectively improving the problem of network carbides.

[0058] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with the low-temperature spinning and Stelmor rapid cooling and roller slow cooling process, the cooling rate of the wire rod with roller slow cooling is further reduced. Although the network carbide problem is improved to a certain extent, the level is still high, the incubation time of troostite is reduced, and a certain proportion of pearlite structure with a large interlamellar spacing is obtained, but the strength is greatly lost. However, due to the limited maximum cooling capacity of the Stelmor air-cooling line, after the troostite incubation, the wire rod is already in a low temperature state, and the dislocation density of the troostite is relatively high. Large, will produce greater drawing hardening, is not conducive to deep drawing and cold heading, the present invention uses online molten salt strong isothermal treatment, with a large degree of supercooling into the pearlite phase region for strong isothermal treatment, is beneficial to the transformation of austenite structure into troostite with finer interlamellar spacing, the austenite structure in the wire rod structure can be transformed into most of the troostite and a small part of the pearlite structure, can significantly extend the wire rod in the pearlite phase time, promote the incubated pearlite and troostite structure to be tempered at high temperature, reduce the organizational stress and dislocation density, significantly improve the wire rod plasticity.

[0059] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with further increasing the Stelmor rapid cooling rate and reducing the roller slow cooling wire rod cooling rate, bainite or even martensite structure is prone to local appearance, causing increased mechanical fluctuations and brittleness of the wire rod. After a long period of online molten salt strong isothermal treatment, the present invention fully transforms the structure into tempered troostite and tempered pearlite, avoiding the mixing of bainite structure in the structure and achieving strong plasticity matching. Embodiment 2:

[0060] A preferred embodiment of the manufacturing method of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.78%, Si: 0.2%, Mn: 0.49%, P: 0.012%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature controlled rolling → wire laying → online molten salt strong isothermal → hot air roller strong slow cooling → coiling, specifically:

[0061] The low temperature controlled rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to promote the uniform diffusion of high carbon components and avoid the risk of burning and decarburization. After heating to a high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 22mm through a rolling line. Low temperature controlled rolling is used to prevent the aggravation of high temperature decarburization, so that the rolling within the recrystallization temperature range of the austenite grains can achieve the purpose of grain refinement. Specifically: the heating temperature of the steel billet is controlled to be 1080°C, the time in the furnace is 4h, the initial rolling temperature is 1065°C, the initial rolling reduction is 36%, the final rolling temperature is 935°C, the final rolling reduction is 43%, and the decarburization layer depth is ≤0.45% of the diameter.

[0062] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the formation of a large undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 910°C.

[0063] The online molten salt strong isothermal treatment adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by a roller and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 35°C / s for strong isothermal phase transformation, avoiding the wire rod to stay in the secondary cementite interval and the tertiary cementite peak interval for a long time, quickly skipping the ferrite phase transformation temperature interval, entering the pearlite phase region with a large degree of supercooling, controlling the pearlite and troostite content of the wire rod, avoiding the generation of hard and brittle bainite phase, and promoting high-temperature tempering of pearlite and troostite structures, reducing organizational stress and dislocation density, and softening the matrix. Specifically: the molten salt temperature is controlled to be 605°C, the processing time is 650s, the molten salt circulation volume is 530t / h, and the molten salt temperature rise is ≤8°C.

[0064] The hot air roller strong slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is transported into the insulation cover by the roller, and the hot air generated above the salt bath tank is transported into the insulation cover as hot air for strong slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.35m / s, and the wire rod is cooled to 335℃ at a cooling rate of 0.45℃ / s by hot air above 300℃, and then the wire rod is transported to the coil at a roller speed of 0.6m / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 298℃. After packaging and storage, the cold heading steel wire rod product is obtained, and its metallographic structure diagram is as follows Figure 2 shown.

[0065] Comparative Example 4:

[0066] A method for manufacturing a wire rod, which differs from that of Example 2 in that the heating temperature of the steel billet is controlled to be 1075°C, the furnace time is 4.2h, the initial rolling temperature is 1055°C, the final rolling temperature is 930°C, the spinning temperature is 900°C, the wire rod is cooled at a cooling rate of 34°C / s to the pearlite phase region for a strong isothermal phase transformation, and the finished wire rod is obtained after being rolled off the line.

[0067] Comparative Example 5:

[0068] A method for manufacturing a wire rod, which differs from Example 2 in that the wire rod is cooled at a cooling rate of 33°C / s to a pearlite phase region for a strong isothermal phase transformation, the molten salt temperature is 630°C, and the finished wire rod is obtained after being rolled off the production line.

[0069] Comparative Example 6:

[0070] A method for manufacturing a wire rod, which differs from Example 2 in that the wire rod is cooled at a cooling rate of 37°C / s to a pearlite phase region for a strong isothermal phase transformation, the molten salt temperature is 550°C, the molten salt circulation rate is 630t / h, and the finished wire rod is obtained after being rolled off the line. Embodiment 3:

[0071] A preferred embodiment of the manufacturing method of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.77%, Si: 0.4%, Mn: 0.53%, P: 0.013%, S: 0.01%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature controlled rolling → wire laying → online molten salt strong isothermal → hot air roller strong slow cooling → coiling, specifically:

[0072] The low-temperature controlled rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high-carbon components and avoid the risk of burning and decarburization. After heating to a high-temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 25mm through a rolling line. Low-temperature controlled rolling is used to prevent the aggravation of high-temperature decarburization, so that the rolling within the recrystallization temperature range of the austenite grains can achieve the purpose of grain refinement. Specifically: the heating temperature of the steel billet is controlled to be 1100°C, the time in the furnace is 4.5h, the initial rolling temperature is 1085°C, the initial rolling reduction is 31%, the final rolling temperature is 980°C, the final rolling reduction is 40%, and the decarburization layer depth is ≤0.45% of the diameter.

[0073] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the formation of a larger undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 940°C.

[0074] The online molten salt strong isothermal treatment adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by a roller and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 38°C / s for strong isothermal phase transformation, avoiding the wire rod to stay in the secondary cementite interval and the tertiary cementite peak interval for a long time, quickly skipping the ferrite phase transformation temperature interval, entering the pearlite phase region with a large degree of supercooling, controlling the pearlite and troostite content of the wire rod, avoiding the generation of hard and brittle bainite phase, and promoting high-temperature tempering of pearlite and troostite structures, reducing organizational stress and dislocation density, and softening the matrix. Specifically: the molten salt temperature is controlled to be 572°C, the processing time is 552s, the molten salt circulation volume is 730t / h, and the molten salt temperature rise is ≤8°C.

[0075] The hot air roller strong slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is transported into the insulation cover by the roller, and the hot air generated above the salt bath tank is transported into the insulation cover as hot air for strong slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.25m / s, and the wire rod is cooled to 345℃ at a cooling rate of 0.24℃ / s by hot air above 300℃, and then the wire rod is transported to the coil at a roller speed of 0.85m / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 305℃. After packaging and storage, the finished cold heading steel wire rod is obtained, and its metallographic structure diagram is as shown in Figure 3 shown.

[0076] Comparative Example 7:

[0077] A method for manufacturing a wire rod, which differs from the manufacturing method of Example 3 in that the online molten salt strong isothermal treatment time is 700s, and the finished wire rod is obtained after the coil is rolled off the line.

[0078] Comparative Example 8:

[0079] A method for manufacturing a wire rod, which differs from the manufacturing method of Example 3 in that the online molten salt strong isothermal treatment time is 480s, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 4:

[0080] A preferred embodiment of the manufacturing method of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.75%, Si: 0.29%, Mn: 0.55%, P: 0.014%, S: 0.011%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature controlled rolling → wire laying → online molten salt strong isothermal → hot air roller strong slow cooling → coiling, specifically:

[0081] The low temperature controlled rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to promote uniform diffusion of high carbon components and avoid the risk of burning and decarburization. After heating to a high temperature steel billet with rollable plasticity, the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 18mm through a rolling line. Low temperature controlled rolling is used to prevent the aggravation of high temperature decarburization, so that the rolling within the recrystallization temperature range of the austenite grains can achieve the purpose of grain refinement. Specifically: the heating temperature of the steel billet is controlled to be 1090°C, the time in the furnace is 4.2h, the initial rolling temperature is 1075°C, the initial rolling reduction is 39%, the final rolling temperature is 945°C, the final rolling reduction is 46%, and the decarburization layer depth is ≤0.45% of the diameter.

[0082] The spinning process is used to convert the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. Through an appropriate spinning temperature, the wire rod is prevented from precipitating network carbides during the spinning stage, the tendency of grain growth is reduced, and conditions are created for the formation of a larger undercooling and sorbite nucleation. Specifically, the spinning temperature is controlled to be 915°C.

[0083] The online molten salt strong isothermal treatment adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by a roller and quickly cooled to the molten salt temperature, so that the wire rod is cooled to the pearlite phase region at a cooling rate of 37°C / s for strong isothermal phase transformation, avoiding the wire rod to stay in the secondary cementite range and the tertiary cementite peak range for a long time, quickly skipping the ferrite phase transformation temperature range, entering the pearlite phase region with a large degree of supercooling, controlling the pearlite and troostite content of the wire rod, avoiding the generation of hard and brittle bainite phase, and promoting high-temperature tempering of pearlite and troostite structures, reducing organizational stress and dislocation density, and softening the matrix. Specifically: the molten salt temperature is controlled to be 555°C, the processing time is 510s, the molten salt circulation volume is 640t / h, and the molten salt temperature rise is ≤8°C.

[0084] The hot air roller strong slow cooling process adopts the roller insulation cover to be closed, and the wire rod coming out of the salt bath tank is transported into the insulation cover by rollers. At the same time, the hot air generated above the salt bath tank is transported into the insulation cover as hot air for strong slow cooling treatment to promote further softening of the wire rod structure. Specifically: the initial roller speed is 0.2m / s, and the wire rod is cooled to 340℃ at a cooling rate of 0.1℃ / s with hot air above 300℃, and then the wire rod is transported to the coil at a roller speed of 0.9m / s; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the coiling temperature is 300℃. After packaging and warehousing, the finished cold heading steel wire rod is obtained.

[0085] Comparative Example 9:

[0086] A method for manufacturing wire rod, which differs from Example 4 in that the method is manufactured according to the process flow of low-temperature controlled rolling → wire spinning → online molten salt strong isothermal → roller slow cooling → coiling, the roller slow cooling adopts a heat preservation cover to be closed, no hot air is delivered, the initial roller speed is 0.2m / s, the wire rod is controlled to be cooled to 340℃ at a cooling rate of 1.2℃ / s, and then the wire rod is conveyed to the coiling at a roller speed of 0.6m / s; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished wire rod is obtained after the coiling is off the line.

[0087] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 9 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:

[0088] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods

[0089]

[0090] It can be seen from the results of Examples 1 to 4 that the present invention forms a microstructure including a majority of tempered troostite and a small portion of tempered pearlite through solid solution strengthening combined with microstructure regulation, and can achieve a tensile strength of 1150 to 1200 MPa, a cross-sectional shrinkage of 43 to 48%, and a network carbide grade of 0, which effectively reduces the brittleness, crack sensitivity and tensile hardening ability of the cold heading steel wire rod, achieves high strength and plasticity matching, and is used to manufacture fasteners such as 13.9-grade bolts, and has good market application prospects.

[0091] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the spinning temperature is too low, the supercooling degree is reduced, and it is not conducive to the nucleation of troostite; from the comparison results of Examples 1 to 4 and Comparative Example 5, it can be seen that the higher the molten salt temperature, the more favorable it is to form a pearlite structure with a higher proportion and coarser interlamellar spacing, and a longer treatment time is beneficial to promoting the high-temperature tempering of pearlite and troostite, but the molten salt temperature is too high, and a too low proportion of troostite structure is formed. Due to the slow cooling rate, the precipitation of tertiary cementite causes grain coarsening, which is not conducive to the strength and plasticity of the wire rod; from the comparison results of Example 2 and Comparative Example 6, it can be seen that the molten salt temperature is too low, and a too high proportion of troostite structure or even a small amount of bainite structure is formed, which is not conducive to the plasticity of the matrix.

[0092] From the comparison results of Examples 1 to 4 with Comparative Example 7, it can be seen that a longer treatment time is beneficial to promoting the high-temperature tempering of pearlite and troostite, but too long a treatment time will cause excessive loss of matrix strength; from the comparison results of Example 3 with Comparative Example 8, it can be seen that if the treatment time is too short, it is difficult to temper and soften the pearlite and troostite structures, which will cause the plasticity of the wire rod to decrease and be easy to harden by drawing. Therefore, the molten salt temperature and treatment time can be further controlled to control the pearlite and troostite content of the wire rod, and to regulate the high-temperature tempering and softening effect of the pearlite and troostite structures.

[0093] From the comparison results of Example 4 and Comparative Example 9, it can be seen that compared with the slow cooling on the roller table, the thermal energy of the hot air on the trough is further recovered and utilized to reduce production energy consumption. The hot air in the insulation cover is used to maintain a high-temperature atmosphere to further reduce the cooling rate of the wire rod, which can enable the wire rod after phase change tempering to be further tempered and softened at a continuous high temperature.

[0094] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on steelmaking raw materials. Any equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A eutectoid carbon cold heading steel wire rod for 13.9 grade bolts, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.75% to 0.79%, Si: 0.20% to 0.40%, Mn: 0.45% to 0.55%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities, and its microstructure includes tempered pearlite accounting for 32% to 39% by volume and tempered troostite accounting for 61% to 68% by volume; The manufacturing method comprises: producing a wire rod by controlled rolling according to the chemical composition of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts, after the wire rod is spun into a wire rod at a spinning temperature of ≥910°C, performing online molten salt strong isothermal treatment, cooling the wire rod to the pearlite phase region at a cooling rate of ≥35°C / s for strong isothermal phase transformation, promoting pearlite and bainite phase transformation and high-temperature tempering, and finally performing hot air roller strong slow cooling to produce a cold heading steel wire rod having a microstructure including tempered pearlite and tempered bainite, wherein the online molten salt strong isothermal treatment controls the molten salt temperature to be 555-605°C, the treatment time to be 510-650s, the hot air roller strong slow cooling uses a roller to convey the wire rod into a heat preservation cover, and controls the wire rod to be cooled to below 350°C at a cooling rate of 0.1-0.45°C / s with hot air above 300°C.

2. The eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 165-200 nm, the interlamellar spacing of the tempered troostite is 100-145 nm, and the network carbide level of the cold heading steel wire rod is level 0.

3. The eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 1 or 2, characterized in that: The diameter of the cold heading steel wire rod is 18.0-28.0 mm, the tensile strength is 1150-1200 MPa, and the cross-sectional shrinkage is 43%-48%.

4. A method for manufacturing eutectoid carbon cold heading steel wire rod for 13.9 grade bolts, characterized in that: The manufacturing method thereof comprises: According to the chemical composition controlled rolling production line of the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts as claimed in claim 1, after the wire rod is spun into wire rod at a spinning temperature of ≥910°C, it is subjected to online molten salt strong isothermal treatment, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥35°C / s for strong isothermal phase transformation, promoting pearlite and bainite phase transformation and high-temperature tempering, and finally subjected to hot air roller strong slow cooling to produce a cold heading steel wire rod having a microstructure including 32% to 39% tempered pearlite and 61% to 68% tempered bainite by volume; the online molten salt strong isothermal control molten salt temperature is 555 to 605°C, the processing time is 510 to 650s, the hot air roller strong slow cooling uses a roller to convey the wire rod into a heat preservation cover, and controls the wire rod to be cooled to below 350°C at a cooling rate of 0.1 to 0.45°C / s with hot air above 300°C.

5. The method for manufacturing the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 4, characterized in that: During the controlled rolling, the heating temperature of the steel billet is controlled to be ≤1100°C and the time in the furnace is controlled to be ≤4.5h before rolling.

6. The method for manufacturing the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 4, characterized in that: The controlled rolling adopts low temperature controlled rolling, controls the initial rolling temperature to be 1065-1085°C, the initial rolling reduction to be 29%-39%, the final rolling temperature to be ≥935°C, and the final rolling reduction to be 38%-46%.

7. The method for manufacturing the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 4, characterized in that: The online molten salt strong isothermal control molten salt circulation rate is 530~730t / h, and the molten salt temperature rise is ≤8℃.

8. The method for manufacturing the eutectoid carbon cold heading steel wire rod for 13.9 grade bolts according to claim 4, characterized in that: The hot air comes from the hot air on the online molten salt strong isothermal tank; after the wire rod is cooled to below 350°C, it is transported to the coil at a roller speed of 0.6~0.9m / s.

Citation Information

Patent Citations

  • Composite microalloyed high-strength steel forge piece with tensile strength of 700 MPa and production method thereof

    CN104032237A

  • Hot rolled wire rod for high-strength cut steel wires and production method of hot rolled wire rod