A welding method for low-strength matching welding joint of 785MPa grade high-strength steel

By using 735MPa grade welding wire and a low-strength matching welding method with specific welding process parameters, the problems of preheating before welding and postheating after welding in the welding of 785MPa grade high-strength steel were solved, achieving efficient, low-cost welding quality and safety.

CN118664034BActive Publication Date: 2024-11-29CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411170369.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

In the existing technology, welding of 785MPa high-strength steel requires strict preheating and postheating processes, which results in low welding efficiency, high cost and difficulty in ensuring welding quality, especially making it prone to welding cold cracks.

Method used

Low-strength matching welding is performed using 735MPa grade welding wire. By determining the joint type, groove type and size, and combining specific welding process parameters such as welding wire specifications, current, voltage, speed and gas flow rate, high-strength steel welding without post-heating can be achieved.

Benefits of technology

The welded joint has a strength no less than that of the steel plate, excellent low-temperature impact toughness, avoids the impact of post-heat treatment on performance, improves welding efficiency and reduces costs, while ensuring welding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118664034B_ABST
    Figure CN118664034B_ABST
Patent Text Reader

Abstract

The invention provides a welding method for a 785MPa-grade high-strength steel low-strength matching welding joint, comprising the following steps: S1, determining a joint form; S2, determining a welding groove form of a plate to be welded according to a thickness of the plate to be welded; S3, determining a groove size according to the groove form of the plate to be welded; S4, determining a weld size according to the groove size; S5, processing the plate to be welded into a groove according to the groove size; S6, preheating the plate to be welded to a temperature of 100-150°C; S7, welding, wherein the weld size is obtained by process parameters during welding; the process parameters during welding are: a welding wire specification of φ1.2mm, a welding current of 200-240A, a welding voltage of 24-28V, a welding speed of 30-40cm / min, a shielding gas of 95%Ar and 5%CO2, and a shielding gas flow rate of 18-25L / min. The present invention accurately obtains the weld size through the groove size, so that the internal stress distribution of the weld joint structure during welding is more uniform, no post-heat treatment is required, the welding production process is simplified, and the welding quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of welding technology, and in particular to a welding method for a 785MPa grade high-strength steel low-strength matching welding joint. Background Art

[0002] Welding is an essential and key process in the manufacturing process of steel structures, and for the welding of high-strength steel, the focus is on welding quality and welding efficiency. In terms of welding quality, the main thing is to avoid problems such as pores, inclusions, lack of fusion and welding cracks in the welded joints; in terms of welding efficiency, the main focus is on new welding processes such as high-energy beams and automation, as well as welding preheating and post-heating processes.

[0003] With the demand for large-scale and lightweight development of engineering structures, the application of high-strength steel welded structures is becoming more and more widespread. However, the problem of welding cracks in high-strength steel and the limited types of welding materials available for high-strength steel welding are bottlenecks that restrict the full performance of high-strength steel. As the strength of steel increases, the strength of supporting welding materials is also required to increase simultaneously. The increase in the strength of welding materials will lead to a significant decrease in the toughness of the weld metal and a significant increase in the sensitivity of welding cold cracks. Because the weld metal is a cast structure, it is an inherent property that the toughness of the weld metal decreases with the increase of weld strength. Especially after the weld metal strength exceeds 800MPa, the toughness of the weld metal is difficult to improve, and the toughness decreases more significantly with the increase of strength; with the increase of weld joint strength, the sensitivity of welding cold cracks increases, and welding cold cracks are very likely to occur, which brings great risks to engineering applications. In order to prevent the occurrence of welding cold cracks, the conventional methods currently used are preheating before welding and post-heating after welding. For example, the welding of 785MPa-grade high-strength steel in my country requires preheating of 100-150℃ before welding and post-heating of 200-250℃ for more than two hours immediately after welding. The welding preheating and post-heating process not only increases the welding cost, but also is a technical bottleneck that restricts the manufacturing progress and quality of high-strength steel structures.

[0004] In order to ensure the welding quality of high-strength steel welded joints and improve welding efficiency, the United States, Russia, Japan and other countries all use low-strength matching welding technology for high-strength steel welding, that is, low-strength welding materials are used for welding high-strength steel, and the joints are strengthened by certain weld seams to ensure equal strength. This welding method can not only keep the toughness of the welded joints at a high level, but also ensure the safety and reliability of the joints. At the same time, due to the low strength of the welding materials used, the sensitivity of welding cold cracks is reduced, and to a certain extent, high-strength steel can be welded without post-heating or even preheating. For example, Japan's NS110 steel welding adopts a technical route based on low-matching welding and combined with equal-strength matching welding. In the 1990s, Japan and the United States cooperated to study the low-matching welding technology of NS110 steel, HY-100 steel and HY-130 steel. Through a series of tests, especially large-scale explosion tests, the static strength, fatigue performance, stress corrosion resistance, explosion resistance and other performance of NS110 steel low-matching welded joints were fully evaluated. The results show that it is feasible to use low-matching welded joints with a strength of 15% lower. In 2006, Japan included low-matching welding materials for NS110 steel into the Defense Agency's specifications, including electrodes and gas shielded welding wires with a yield strength of 95 kg. Russia used 735MPa grade welding materials to weld 785MPa steel, achieving non-post-heat welding of this strength grade of steel. The use of low-strength matching welding technology for welding high-strength steel has been widely used abroad, but no specific design method for the size of the welding joint has been seen.

[0005] my country has also conducted a lot of research on low-match welding technology for high-strength steel. For example, Harbin Institute of Technology has carried out equal-load design of welded joints based on the fracture parameter K factor, and has applied for patents such as "Design method for butt joints with type I center cracks to achieve equal load (201010615818.6)", "Design method for welded joints to carry loads according to the bearing capacity of parent materials (201010615842.X)", "Derivation method and application of stress intensity factor of butt joints with type I center cracks (201010615638.8)", "Design method for butt joints with center cracks under tensile loads" and "Design method for butt joints with center cracks under tensile loads" and "Design method for butt joints with center cracks under tensile loads" and "Design method for butt joints with center cracks to achieve equal load (201010615818.6)". In the paper "Design Method for Equal Load and Application of K Factor (201110064677.8)", the equal load design idea of ​​welded joints based on fracture parameter K factor was proposed, and the method for determining the shape factor expression of geometric discontinuous structures with defects was given. At the same time, the design criteria for equal load joints based on fracture parameter K factor were given, and the corresponding equal load design system for welded joints was developed. The shape parameters of joints with different defects that meet the equal load requirements can be obtained. However, it is difficult to determine the boundary conditions when this method is actually used, and a high level of special technology is required. When welding 785MPa grade high-strength steel in my country, it is required to preheat 100-150℃ before welding, post-heat 200-250℃ after welding and keep warm for more than two hours. This harsh welding process must be strictly implemented, otherwise it is very easy to produce welding cold cracks. This welding process is not only not conducive to improving welding efficiency and controlling welding costs, but also not conducive to ensuring welding quality. Summary of the invention

[0006] In view of this, the present invention aims to propose a welding method for 785MPa grade high strength steel low strength matching welding joints. This method solves the problem that the prior art requires preheating to 100-150°C before welding, post-heating to 200-250°C after welding and heat preservation for more than 2 hours. This harsh welding process must be strictly implemented, otherwise welding cold cracks are very likely to occur. This welding process is not only not conducive to improving welding efficiency and controlling welding costs, but also not conducive to ensuring welding quality.

[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0008] A welding method for a 785MPa grade high strength steel low strength matching welding joint comprises the following steps:

[0009] S1. Determine the joint form;

[0010] S2. Determine the groove form according to the thickness of the plate to be welded;

[0011] S3. Determine the groove size according to the groove form of the plate to be welded;

[0012] S4. Determine the weld size according to the groove size of the plate to be welded;

[0013] S5. Process the plate to be welded into a groove according to the groove size;

[0014] S6. Preheat the plate to be welded to a temperature of 100-150°C;

[0015] S7. Welding, wherein the weld size is obtained by the process parameters during welding; the process parameters during welding are: welding wire specification is φ1.2mm, welding current is 200-240A, welding voltage is 24-28V, welding speed is 30-40cm / min, shielding gas is 95%Ar and 5%CO2, and shielding gas flow rate is 18-25L / min.

[0016] The welding joint of the present invention, after welding 785MPa high-strength steel with 735MPa-grade welding wire, can not only achieve a strength of the welding joint that is not lower than the steel plate, but also the welding joint has excellent low-temperature impact toughness (-50℃KV2), which can better ensure the safety and reliability of the welding joint; the weld size can be accurately obtained through the groove size, so that the internal stress distribution of the welding joint structure during welding is more uniform, and no post-heat treatment is required again, which simplifies the welding production process, while avoiding the influence of post-heat treatment on the performance of the welding joint, improving the welding quality, and greatly improving the welding efficiency of the structure and reducing the welding cost.

[0017] Furthermore, the welding wire is a 735MPa gas shielded welding wire, and the yield strength R P0.2 742~750MPa, tensile strength R m It is 851~855MPa, the elongation after break A is 19~20%, and the section shrinkage Z is 69%.

[0018] Furthermore, the yield strength R of the steel to be welded P0.2 830~844MPa, tensile strength R m It is 875~890MPa, the elongation after break A is 19~22%, and the cross-sectional shrinkage Z is 72~77%.

[0019] Furthermore, the joint form is one of butt joint and corner joint.

[0020] Furthermore, when the joint is butt joint, the thickness of the plate to be welded is d The thickness is 16 to 30 mm, and the groove form is a single-sided welding groove form.

[0021] Furthermore, when the joint is butt joint, the thickness of the plate to be welded is d The groove is 30 to 80 mm, and the groove is a double-sided welding groove.

[0022] Furthermore, when the joint is a fillet joint, the thickness of the plate to be welded dThe thickness is 16 to 24 mm, and the groove form is a single-sided welding groove form.

[0023] Furthermore, when the joint is a fillet joint, the thickness of the plate to be welded d The groove is 20 to 60 mm, and the groove form is a double-sided welding groove form.

[0024] Furthermore, the weld size includes one or more of weld excess height, weld width, weld foot width, and weld foot height.

[0025] Furthermore, the welding groove form of the plate to be welded is one of single-sided symmetrical groove butt joint, single-sided asymmetrical groove butt joint, double-sided symmetrical groove butt joint, double-sided asymmetrical groove butt joint, single-sided groove corner joint, and double-sided groove corner joint.

[0026] Furthermore, when single-sided symmetrical groove butt welding is adopted, the weld reinforcement is calculated according to the following formula (1), and the weld width is calculated according to the following formula (2):

[0027] h =0.106 d (1)

[0028] B =2( h / tg (180- i ) + ( d - p ) tg ( α 3 / 2)) +b+2c (2)

[0029] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 3 —Angle of the third groove, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, i ≥140°, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 3 =45~55°, b =0~3mm, c=2~8mm, d =16~30mm.

[0030] Furthermore, when single-sided asymmetric groove butt welding is adopted, the weld reinforcement is calculated according to the following formula (3), and the weld width is calculated according to the following formula (4):

[0031] h= 0.106 d (3)

[0032] B =2 h / tg (180- i )+( d - p )( tga 2 +tgα 1 )+ b + 2c (4)

[0033] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 1 — first groove angle, °; α 2 —Second groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, θ≥140°, p is determined according to the welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 1 =10~15°, α 2 =30~35°, b =0~3mm, c =2~8mm, d =16~30mm.

[0034] Furthermore, when double-sided symmetrical groove butt welding is adopted, the weld reinforcement is calculated according to the following formula (5), the weld width is calculated according to the following formula (6), and the third groove width at the lower end is calculated according to the following formula (7):

[0035] h= 0.106 d (5)

[0036] B =2 h / tg (180- i )+2( d - p - H ) tg ( α 3 / 2) +b+2c (6)

[0037] k 3 =( d - p - H ) tg ( α 3 / 2) (7)

[0038] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 3 —Angle of the third groove, °; k 3 —Width of the third groove at the lower end, mm; b —Assembly clearance, mm; c —Overlap, mm; H —Back groove depth, mm; preferably, i ≥140°, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤2mm, H = d / 2-4mm, α 3 =45~55°, b =0~3mm, c =2~8mm, d =30~80mm.

[0039] Furthermore, when double-sided asymmetric groove butt welding is adopted, the weld reinforcement is calculated according to the following formula (8), the weld width is calculated according to the following formula (9), the lower first groove width is calculated according to the following formula (10), and the lower second groove width is calculated according to the following formula (11):

[0040] h =0.106 d (8)

[0041] B =2 h / tg (180- i )+( δ-pH )( tga 2 + tga 1 ) +b+ 2 c (9)

[0042] k 1 =( d - p - H ) tg ( α 1 / 2) (10)

[0043] k 2 =( d - p - H ) tg ( α 2 / 2) (11)

[0044] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 1 — first groove angle, °; α 2 —Second groove angle, °; k 1 —Width of the first groove at the lower end, mm; k 2 —Width of the second groove at the lower end, mm; H —Back groove depth, mm ;b —Assembly clearance, mm; c —Overlap, mm; H —Back groove depth, mm; preferably, i ≥140°, p Determined by welding method, 6mm≤ p ≤δ / 2-4mm or p≤2mm, H = d / 2 - 4mm, α 1 =10~15°, α 2 =30~35°, b =0~3mm, c =2~8mm, δ= 30~80mm.

[0045] Furthermore, when single-sided groove fillet welding is used, the weld leg width is calculated according to the following formula (12), and the weld leg height is calculated according to the following formula (13):

[0046] K 1 =( d-p ) tga 4 + b + c (12)

[0047] K 2 = 0.25 d+ 2 (13)

[0048] In the formula, K 1 —Weld leg width, mm; K 2 —Weld leg height, mm; d —Steel plate thickness, mm; p —Welding groove root allowance, mm; α 4 —The fourth groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 4 =45~55°, b =0 ~ 3mm, c =2~8mm, δ= 16 ~ 24mm.

[0049] Furthermore, when double-sided groove fillet welding is used, the weld leg width is calculated according to the following formula (14), the weld leg height is calculated according to the following formula (15), and the fourth groove width isk 4 Calculate according to the following formula (16):

[0050] K 1 =( d - p - H ) tga 5 + b + c (14)

[0051] K 2 = 0.25 d +2 (15)

[0052] k 4 = ( d - p - H ) tg ( α 5 / 2) (16)

[0053] In the formula, K 1 —Weld leg width, mm; K 2 —Weld leg height, mm; d —Steel plate thickness, mm; p —Welding groove root allowance, mm; α 5 —Fifth groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; k 4 —The fourth groove width, mm; H —Back groove depth, mm; preferably ,p ≤ d / 2-4mm, more preferably, 6mm≤ p ≤ d / 2-4mm, α 5 =45~55°, H = d / 2 - 4mm, b =0 ~ 3mm, c =2~8mm, d =20 ~ 60mm.

[0054] Furthermore, when the thickness of the two plates to be welded is different during welding, the weld width B Calculated according to the thickness of the thinner side steel plate.

[0055] Furthermore, the thickness of the plate to be welded is 16 ~ 80mm.

[0056] Furthermore, the thickness of the plate to be welded is one of 16 mm, 32 mm, 58 mm, and 80 mm.

[0057] Compared with the prior art, the welding method of a 785MPa grade high-strength steel low-strength matching welding joint described in the present invention has the following advantages:

[0058] The welded joint of the present invention, after welding 785MPa high-strength steel with 735MPa grade welding wire, can not only achieve a strength of the welded joint that is not lower than that of the steel plate, but also has excellent low-temperature impact toughness at -50°C KV2, which can better ensure the safety and reliability of the welded joint;

[0059] The present invention can accurately obtain the weld size through the groove size, so that the internal stress distribution of the weld joint structure during welding is more uniform, and no post-heat treatment is required, which simplifies the welding production process and avoids the influence of post-heat treatment on the performance of the weld joint, thereby improving the welding quality, greatly improving the welding efficiency of the structure, and reducing the welding cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 It is a structural schematic diagram of the weld toe angle and overlap amount of the butt joint of the present invention;

[0061] Figure 2 It is a structural schematic diagram of the fillet joint weld toe angle and overlap amount of the present invention;

[0062] Figure 3 A diagram showing the groove form of a single-sided symmetrical groove butt joint of the present invention;

[0063] Figure 4 It is a weld formation dimension diagram of a single-sided symmetrical groove butt joint of the present invention;

[0064] Figure 5 A diagram showing the groove form of a single-sided asymmetric butt joint of the present invention;

[0065] Figure 6 It is a dimension diagram of the weld formation of a single-sided asymmetric butt joint of the present invention;

[0066] Figure 7 It is a double-sided symmetrical butt joint groove form diagram of the present invention;

[0067] Figure 8 It is a double-sided symmetrical butt joint weld formation dimension diagram of the present invention;

[0068] Figure 9 It is a double-sided asymmetric butt joint groove form diagram of the present invention;

[0069] Figure 10 It is a double-sided asymmetric butt joint weld formation dimension diagram of the present invention;

[0070] Figure 11 A diagram showing the welding groove form of a single-sided groove fillet joint of the present invention;

[0071] Figure 12 It is a single-sided groove fillet joint weld forming dimension drawing of the present invention;

[0072] Figure 13 A diagram showing the groove form of a double-sided grooved corner joint of the present invention;

[0073] Figure 14 It is a dimension drawing of the weld formation of the double-sided groove fillet joint of the present invention. DETAILED DESCRIPTION

[0074] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the description of the present invention, it should be noted that the directions or positional relationships indicated by the terms "upper", "lower", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention.

[0075] The present invention is aimed at high-strength steel with a yield strength of 785MPa, and adopts welding wire with a yield strength of 735MPa. The welding method is butt joint or fillet joint, and the welding groove and weld shape size are designed. The present invention can achieve the strength of the welded joint is not lower than that of the steel plate. At the same time, for the thick steel plate with a thickness of 80mm, the window-shaped restrained welding crack test without post-heat welding is carried out, and no welding cold cracks are found. The specific design scheme is as follows:

[0076] A welding method for a 785MPa grade high strength steel low strength matching welding joint comprises the following steps:

[0077] S1. Determine the joint type, which can be a butt joint or a corner joint, such as Figure 1 , Figure 2 As shown;

[0078] S2. Determine the groove form of the plate to be welded according to the thickness of the plate to be welded; in order to achieve the same weld metal on the front and back sides as much as possible, when the thickness of the butt joint steel plate is d ≤30mm, fillet joint web thickness d When the diameter is ≤24mm, it is designed as a single-sided welding groove, such as Figure 3~Figure 6 , Figure 11~Figure 12 As shown; when the butt joint steel plate thickness d ≥24mm, the web thickness of the fillet joint d When the diameter is ≥20mm, the design is double-sided welding groove, such as Figure 7~Figure 10 , Figure 13~Figure 14 As shown;

[0079] S3. Determine the groove size according to the groove form of the plate to be welded;

[0080] When single-sided or double-sided symmetrical groove butt welding or single-sided asymmetrical groove butt welding is adopted, the groove size includes the third groove angle. α 3 , the third groove angle is the upper end of the groove, α 3 45~55°; When double-sided asymmetric groove butt welding is used, the groove size includes the first groove angle α 1 , Second groove angle α 2 , the first groove angle and the second groove angle are both located at the upper end of the groove, and the first groove angle α 1 The second groove angle is 10-15°. α 2 Generally, it is 30-35°, and the groove angle can be appropriately increased or decreased according to the thickness of the steel plate, welding position and welding method.

[0081] When single-sided groove fillet welding is used, the groove size includes the fourth groove angle α 4 , α 4 It is 45~55°.

[0082] When double-sided groove fillet welding is used, the groove size includes the fifth groove angle. α 5 , α 5 It is 45~55°.

[0083] S4. Determine the weld size according to the groove size;

[0084] S41. Determine the root amount of the welding groove p ; When welding with arc welding or metal arc welding, the root p for d / 2-4mm, when using automatic submerged arc welding, the root amountp Pick d / 2-4mm and 6mm maximum value, such as Figure 1 , Figure 2 As shown;

[0085] S42, determine the depth of the reverse groove H ; If the welding groove of the selected plate to be welded is a double-sided welding groove, in order to make the front and back welds symmetrical after welding, the back groove depth H for d / 2-4mm. According to the trigonometric function relationship, when double-sided symmetrical groove butt welding is adopted, the width of the third groove at the lower end is k 3 =( d - p - H ) tg ( α 3 / 2); When double-sided asymmetric groove butt welding is adopted, the first groove width at the lower end k 1 =( d - p - H ) tg ( α 1 / 2) , Width of the second groove at the lower end k 2 =( d - p - H ) tg ( α 2 / 2);

[0086] S43. Determine the weld toe angle of the weld joint i ; To meet the fatigue performance requirements of the joint, the weld toe angle of the butt joint i Should be no less than 140°, preferably 140-160°; the weld toe angle of the fillet joint i It should be not less than 130°, preferably 130-160°. Figure 1 , Figure 2 As shown;

[0087] S44. Determine the overlap on both sides of the weld joint c ; Overlap c ≥The width of the coarse grain zone in the weld heat affected zone, preferably, the overlap c =2~8mm, specifically, the overlap of general arc welding and metal arc welding c Take 2mm, the overlap of automatic submerged arc welding c Take 8mm, such as Figure 1 , Figure 2 As shown;

[0088] S45. Use numerical simulation and test verification methods to determine the weld height of the butt joint while ensuring the strength, fatigue and explosion resistance of the welded joint. h Relationship with plate thickness δ, or fillet joint weld leg height K 2 and plate thickness d When high-strength steel with a yield strength of 785 MPa is welded with welding materials with a yield strength of 735 MPa, the weld reinforcement height of the butt joint is calculated. h =0.106 d , the lower weld leg height of the corner joint K 2 = 0.25 d +2mm;

[0089] S46, according to the joint form, steel plate thickness d、 Bevel angle α 、Weld toe angle i , Overlap c , Assembly clearance b , root amount p , Back groove depth H Etc., using trigonometric function relationships, the weld widths of different joint forms are calculated B , specifically:

[0090] When single-sided symmetrical groove butt welding is used, Figure 3 , Figure 4 As shown, the weld reinforcement is calculated according to the following formula (1) and the weld width is calculated according to the following formula (2):

[0091] h =0.106 d (1)

[0092] B =2( h / tg (180- i ) + ( d - p ) tg ( α 3 / 2)) +b+2c (2)

[0093] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i—weld toe angle, °; p —Welding groove root allowance, mm; α 3 —Angle of the third groove, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, i ≥140°, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 3 =45~55°, b =0~3mm, c =2~8mm, d =16~30mm.

[0094] When single-sided asymmetric groove butt welding is used, Figure 5 , Figure 6 As shown, the weld height is calculated according to the following formula (3), and the weld width is calculated according to the following formula (4):

[0095] h= 0.106 d (3)

[0096] B =2 h / tg (180- i )+( d - p )( tga 2 +tgα 1 )+ b + 2c (4)

[0097] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 1 — first groove angle, °; α 2 —Second groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, θ≥140°, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 1 =10~15°, α 2 =30~35°, b =0~3mm, c =2~8mm, d =16~30mm.

[0098] When double-sided symmetrical groove butt welding is used, Figure 7 , Figure 8 As shown, the weld reinforcement is calculated according to the following formula (5), the weld width is calculated according to the following formula (6), and the lower groove width is calculated according to the following formula (7):

[0099] h= 0.106 d (5)

[0100] B =2 h / tg (180- i )+2( d - p - H ) tg ( α 3 / 2) +b+2c (6)

[0101] k 3 =( d - p - H ) tg ( α 3 / 2) (7)

[0102] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B —Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 3 —Angle of the third groove, °; k 3 —Width of the third groove at the lower end, mm; b —Assembly clearance, mm; c —Overlap, mm; H —Back groove depth, mm; preferably, i≥140°, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤2mm, H = d / 2-4mm, α 3 =45~55°, b =0~3mm, c =2~8mm, d =30~80mm.

[0103] When double-sided asymmetric groove butt welding is used, Figure 9 , Figure 10 As shown, the weld reinforcement is calculated according to the following formula (8), the weld width is calculated according to the following formula (9), the lower first groove width is calculated according to the following formula (10), and the lower second groove width is calculated according to the following formula (11):

[0104] h =0.106 d (8)

[0105] B =2 h / tg (180- i )+( δ-pH )( tga 2 + tga 1 ) +b+ 2 c (9)

[0106] k 1 =( d - p - H ) tg ( α 1 / 2) (10)

[0107] k 2 =( d - p - H ) tg ( α 2 / 2) (11)

[0108] In the formula, h —weld excess height, mm; d —Steel plate thickness, mm; B—Weld width, mm; i —weld toe angle, °; p —Welding groove root allowance, mm; α 1 — first groove angle, °; α 2 —Second groove angle, °; k 1 —Width of the first groove at the lower end, mm; k 2 —Width of the second groove at the lower end, mm; b —Assembly clearance, mm; c —Overlap, mm; H —Back groove depth, mm; preferably, i ≥140°, p Determined by welding method, 6mm≤ p ≤δ / 2-4mm or p ≤2mm, H = d / 2 - 4mm, α 1 =10~15°, α 2 =30~35°, b =0~3mm, c =2~8mm, δ= 30~80mm.

[0109] When single-sided bevel fillet welding is used, Figure 11 , Figure 12 As shown, the weld leg width is calculated according to the following formula (12), and the weld leg height is calculated according to the following formula (13):

[0110] K 1 =( d-p ) tga 4 + b + c (12)

[0111] K 2 = 0.25 d+ 2 (13)

[0112] In the formula, K 1 —Weld leg width, mm; K 2 —Weld leg height, mm; d —Steel plate thickness, mm; p—Welding groove root allowance, mm; α 4 —The fourth groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; preferably, p Determined by welding method, 6mm≤ p ≤ d / 2-4mm or p ≤ d / 2-4mm, α 4 =45~55°, b =0 ~ 3mm, c =2~8mm, δ= 16 ~ 24mm.

[0113] When double-sided bevel fillet welding is used, Figure 13 , Figure 14 As shown, the weld leg width is given by the following formula (14), the weld leg height is given by the following formula (15), and the fourth groove width is k 4 Calculate according to the following formula (16):

[0114] K 1 =( d - p - H ) tga 5 + b + c (14)

[0115] K 2 = 0.25 d +2 (15)

[0116] k 4 = ( d - p - H ) tg ( α 5 / 2) (16)

[0117] In the formula, K 1 —Weld leg width, mm; K 2 —Weld leg height, mm; d —Steel plate thickness, mm;p —Welding groove root allowance, mm; α 5 —Fifth groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; k 4 —The fourth groove width, mm; H —Back groove depth, mm; preferably ,p ≤ d / 2-4mm, more preferably, 6mm≤ p ≤ d / 2-4mm, H = d / 2-4mm, α 5 =45~55°, b =0 ~ 3mm, c =2~8mm, d =20 ~ 60mm.

[0118] When the thickness of the plates to be welded on both sides of the butt joint groove is inconsistent, the weld width B Calculated according to the thickness of the thinner side steel plate.

[0119] S5. Processing the plate to be welded into a groove according to the groove size;

[0120] S6. Preheat the plate to be welded to a temperature of 100-150°C;

[0121] S7. Weld the plates to be welded, wherein the filling of the weld during welding is achieved by controlling the process parameters during welding; the process parameters during welding are: welding wire specification is φ1.2mm, welding current is 200-240A, welding voltage is 24-28V, welding speed is 30-40cm / min, shielding gas is 95%Ar and 5%CO2, and shielding gas flow rate is 18-25L / min.

[0122] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0123] Example 1

[0124] The welded joint is welded with 785MPa high-strength steel with a thickness of 16mm. The mechanical properties of the steel are shown in Table 1. The joint groove form is as follows Figure 3 The corresponding groove size and weld size are shown in Table 3. i 150°, overlap cThe thickness of the welded joint is 2mm, the welding wire specifications are shown in Table 2, and the welding process is shown in Table 4. The welded joint is preheated to 110°C before welding, and the steel plate is not post-heated after welding. The performance of the welded joint is shown in Table 5.

[0125] Example 2

[0126] The welded joint is welded with 785MPa high-strength steel with a thickness of 32mm. The mechanical properties of the steel are shown in Table 1. The joint groove form is as follows Figure 7 The corresponding groove size and weld size are shown in Table 3. i 150°, overlap c The welding wire specifications are shown in Table 2, and the welding process is shown in Table 4; the preheating is 130°C before welding, and the steel plate is not post-heated after welding. The performance of the welded joint is shown in Table 5.

[0127] Example 3

[0128] The welded joint is welded with 785MPa high-strength steel with a thickness of 58mm. The mechanical properties of the steel are shown in Table 1. The joint groove form is as follows Figure 7 The corresponding groove size and weld size are shown in Table 3. i 150°, overlap c The thickness of the welded joint is 2mm, the welding wire specifications are shown in Table 2, and the welding process is shown in Table 4. The welded joint is preheated to 150°C before welding, and the steel plate is not post-heated after welding. The performance of the welded joint is shown in Table 5.

[0129] Example 4

[0130] The welded joint is welded with 785MPa high-strength steel with a thickness of 80mm. The mechanical properties of the steel are shown in Table 1. The joint groove form is as follows Figure 7 The corresponding groove size and weld size are shown in Table 3. i 160°, overlap c The thickness of the welded joint is 4 mm, the welding wire specifications are shown in Table 2, and the welding process is shown in Table 4. The welded joint is preheated to 150°C before welding, and the steel plate is not post-heated after welding. The performance of the welded joint is shown in Table 5.

[0131] Table 1 Mechanical properties of the plates to be welded

[0132]

[0133] Note: R P0.2 refers to the yield strength; R m It refers to tensile strength; A refers to elongation after fracture, and Z refers to the reduction of area.

[0134] Table 2 Basic mechanical properties of deposited metal of test wire

[0135]

[0136] Table 3 Welding groove and weld formation dimensions

[0137]

[0138] Table 4 Welding process parameters

[0139]

[0140] Table 5 Basic mechanical properties of welded joints

[0141]

[0142] Test example

[0143] The mechanical properties of the welded joints of the test plates welded in Examples 1 to 4 were tested, and the test results are shown in Table 5. The results show that the strength of the welded joint is as strong as that of the steel plate, and the tensile properties are all the same as those of the parent material, indicating that the weld size used achieves the strength of the welded joint as strong as that of the steel plate, and the welded joint has excellent low-temperature impact toughness.

[0144] After the welding of the welded joints of Examples 1 to 4 was completed and placed for 48 hours, radiographic inspection was performed in accordance with GB / T 3323, and the specified Class I requirements were met; in accordance with CB 20776-2021 "Window-Shaped Constraint Welding Crack Test Method", under low temperature and high humidity ((-5-0)℃×(80-90)%RH) and high temperature and high humidity ((30-35)℃×(80-90)%RH) environmental conditions, preheating and no post-heating were performed to conduct window-shaped restraint welding crack resistance tests, specifically dissecting the welded test plates, and no welding cold cracks were found on the sections. This indicates that this welding method can achieve non-post-heating welding of 785MPa high-strength steel.

[0145] The 80mm thick 785MPa high-strength steel in Table 1 and the 735MPa grade gas shielded welding wire in Table 2 were used. According to CB20776-2021 "Window-shaped restraint welding crack test method", under low temperature and high humidity ((-5~0)℃×(80~90)%RH) and high temperature and high humidity ((30~35)℃×(80~90)%RH) environmental conditions, preheating (120~140)℃ without post-heating, the window-shaped restraint welding crack resistance test was carried out, and the welding process parameters are shown in Table 4. After the welding was completed and placed for 48 hours, the radiographic inspection was carried out according to GB / T 3323, and the requirements of level I were met. According to CB20776-2021, the welded test plate was dissected, and no welding cold cracks were found on the section. It shows that this welding method can achieve non-post-heating welding of 785MPa high-strength steel.

[0146] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A welding method for a 785MPa grade high strength steel low strength matching welded joint, characterized in that: The steps include: S1. Determine the joint form: the joint form is a butt joint or a corner joint; S2. Determine the groove form according to the thickness of the plate to be welded: The welding groove form of the plates to be welded is one of single-sided symmetrical groove butt joint, single-sided asymmetrical groove butt joint, double-sided symmetrical groove butt joint, double-sided asymmetrical groove butt joint, single-sided groove corner joint, and double-sided groove corner joint; When the joint form is butt joint, when the thickness of the plate to be welded is 16-30 mm, the groove form is a single-sided welding groove form, and when the thickness of the plate to be welded is 30-80 mm, the groove form is a double-sided welding groove form; When the joint form is fillet joint, when the thickness of the plate to be welded is 16-24mm, the groove form is a single-sided welding groove form, and when the thickness of the plate to be welded is 20-60mm, the groove form is a double-sided welding groove form; S3. Determine the groove size according to the groove form of the plate to be welded: When double-sided asymmetric groove butt welding is used, the groove size includes the first groove angle α 1 , the second groove angle α 2 , the first groove angle and the second groove angle are both located at the upper end of the groove, α 1 10~15°, α 2 30~35°; When single-sided symmetrical groove butt welding is used, the groove size includes the third groove angle α 3 , the third groove angle is located at the upper end of the groove, α 3 45~55°; S4. Determine the weld size according to the groove size of the plate to be welded: The weld size includes one or more of weld excess height, weld width, weld leg width, and weld leg height; When single-sided symmetrical groove butt welding is used, the weld reinforcement is calculated using the following formula (1) and the weld width is calculated using the following formula (2): h =0.106 δ (1) B =2( h / tg(180- θ )+( δ - p )tg ( α 3 / 2))+ b + 2c (2) In the formula, B —Weld width, mm; h —weld excess height, mm; θ —weld toe angle, °; δ —Steel plate thickness, mm; p —Welding groove root allowance, mm; α 3 —The third groove angle, °; b —Assembly clearance, mm; c —Overlap, mm; S5. Process the plate to be welded into a groove according to the groove size; S6. Preheat the plate to be welded to a temperature of 100-150°C; S7, welding, wherein the weld size is obtained by controlling the process parameters during welding; the process parameters during welding are: welding wire specification is φ1.2mm, welding current is 200-240A, welding voltage is 24-28V, welding speed is 30-40cm / min, shielding gas is 95%Ar and 5%CO2, and shielding gas flow rate is 18-25L / min; The welding wire is a 735MPa gas shielded welding wire, and the yield strength R P0.2 742~750MPa, tensile strength R m The steel is 851-855MPa, the elongation after fracture A is 19-20%, and the section shrinkage Z is 69%; The yield strength R of the plate to be welded P0.2 830~844MPa, tensile strength R m It is 875~890MPa, the elongation after break A is 19~22%, and the cross-sectional shrinkage Z is 72~77%.

2. The welding method according to claim 1, characterized in that: The thickness of the plate to be welded is one of 16 mm, 32 mm, 58 mm, and 80 mm.

Citation Information

Patent Citations

  • Design method capable of ensuring welding joint to be born according to bearing capability of parent metal

    CN102091893A

  • Designing method for realizing equal load-carrying of tension-loaded butt joint with central crack on welding line, and application of K factor

    CN102136018A

  • Butt joint design method for implementing equal load carrying of I-shaped center crack-containing butt joint

    CN102163243A

  • Method for deducing stress intensity factor of butt joint containing I-type center bursts and application

    CN102176212B

  • Welding process for high-strength type steel plate

    CN105108273A