A high-strength and high-toughness plastic packaging material and preparation method thereof
Through the multi-component synergistic formula of high-density polyethylene, metallocene polyethylene, linear low-density polyethylene and modified glass fiber, combined with the preparation method of modified glass fiber, the strength decrease of existing plastic packaging materials at extreme temperatures is solved. and the problem of brittleness, achieving high strength, toughness and good processing performance, suitable for high-demand packaging in industries such as food and medical care.
Patent Information
- Application Number
- CN202411172140.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing plastic packaging materials have decreased strength and are prone to brittle at extreme temperatures, and the demand for high strength and toughness in food and medical industries is difficult to meet, and there are problems of fracture, perforation and wear.
Using multi-component collaborative formulas of high-density polyethylene, metallocene polyethylene, linear low-density polyethylene and modified glass fiber, combined with the preparation method of modified glass fiber, grafting through carboxylation, acid chloride, and polyethylene glycol and thiol grafting and other steps to form high-strength and high-toughness plastic packaging material with excellent strength and toughness.
It achieves high strength, toughness and good processing properties of the material, reduces breakage, perforation and wear during packaging, transportation and use, has good barrier properties and chemical resistance, and can better protect the packaging contents.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of packaging materials, and in particular to a high-strength and high-toughness plastic packaging material and a preparation method thereof. Background Art
[0002] In modern industry, packaging materials play an important role in protecting products, extending product shelf life, and facilitating transportation and storage. With the advancement of technology and consumers' increasing demands for product quality, the performance requirements for packaging materials are also constantly increasing. Currently, the commonly used packaging materials on the market include paper materials, metal materials, glass materials and plastic materials, among which plastic packaging materials are widely used due to their excellent comprehensive performance.
[0003] Plastic packaging materials have the advantages of light weight, water resistance, chemical corrosion resistance, and easy processing and molding, and have become important materials in daily life and industrial production. Commonly used plastic packaging materials include polyethylene (PE), polypropylene (PP), polyester (PET), etc.
[0004] In the field of modern packaging materials, plastic materials have become the mainstream choice due to their significant advantages. Polyethylene (PE), polypropylene (PP) and polyester (PET) are the three most commonly used plastic packaging materials, and each material plays an important role in its respective application field due to its unique chemical structure and properties.
[0005] Polyethylene (PE) is a thermoplastic resin with good flexibility, excellent chemical stability and electrical insulation properties. It is mainly used to make plastic bags, plastic films, containers and bottle caps. Its high-density polyethylene (HDPE) form is known for its toughness and impact resistance, and is ideal for making rigid containers. Low-density polyethylene (LDPE) is often used in transparent film products due to its transparency and flexibility.
[0006] Polypropylene (PP) is a semi-crystalline material with good heat resistance, chemical resistance and high strength. It is harder than polyethylene and is an excellent material for manufacturing injection molded parts, films for packaging food, bottle caps and fiber industries. The high melting point of polypropylene makes it suitable for packaging materials for high-temperature retort bagged foods, and its light weight also helps reduce transportation costs.
[0007] Polyester (PET) has a dominant position in the carbonated beverage and bottled water markets due to its excellent transparency and gas barrier properties. PET's high strength and excellent dimensional stability make it a preferred material for bottles and food containers. In addition, PET is also a renewable plastic with mature recycling technology, and is widely used in the production of fibers and new packaging materials.
[0008] Although these materials have been widely used in many fields, each material still has its shortcomings in application. For example, the strength of polyethylene decreases at extreme temperatures, polypropylene tends to become brittle in low temperature environments, and although polyester has excellent barrier properties, its processing technology is complex and the cost is high.
[0009] Chinese patent document CN113817255A discloses a soft plastic packaging material and its preparation method. The raw materials include, by weight: 30-40 parts of polycarbonate, 60-70 parts of linear low-density polyethylene, 50-70 parts of polypropylene, 4-6 parts of phthalic acid, 4-10 parts of silicon dioxide, 2-4 parts of plasticizer, 2-4 parts of graphene, 15-20 parts of glass fiber, 4-6 parts of styrene-acrylonitrile copolymer, 4-6 parts of zirconium dioxide, and 1-3 parts of fire retardant.
[0010] Although these materials can meet basic needs in many applications, in some specific fields, such as food and medical industries, higher requirements are placed on the strength and toughness of packaging materials to solve the problems of breakage, perforation and wear that may occur during packaging, transportation and use. Summary of the invention
[0011] In order to address the deficiencies in the prior art, the purpose of the present invention is to provide a high-strength and high-toughness plastic packaging material and a preparation method thereof. The multi-component synergistic formula not only has excellent strength and toughness, but also maintains good processing performance and use performance, and can effectively reduce the problems of breakage, perforation and wear during packaging, transportation and use. In addition, it also has good barrier properties and chemical resistance, and can better protect the contents of the package.
[0012] In order to achieve the above object, the present invention adopts the following technical solution:
[0013] A high-strength and high-toughness plastic packaging material is made of the following components, measured by weight: 50-70 parts of high-density polyethylene, 10-30 parts of metallocene polyethylene, 5-15 parts of linear low-density polyethylene, 5-12 parts of modified glass fiber, and 1-3 parts of calcium stearate.
[0014] Preferably, the density of the high-density polyethylene is 0.949-0.955 g / cm 3 , melt flow rate is 0.6~1.0g / 10min;
[0015] Preferably, the metallocene polyethylene has a density of 0.924-0.929 g / cm 3 , melt flow rate is 1.3~1.8g / 10min;
[0016] Preferably, the linear low-density polyethylene has a density of 0.918-0.922 g / cm3 , melt flow rate is 1.7~2.3g / 10min;
[0017] Preferably, the method for preparing the modified glass fiber comprises the following steps:
[0018] Carboxylation and acyl chloride: First, 3-[3-carboxyallylamide]propyltriethoxysilane reacts with the silanol groups on the surface of the glass fiber to form a monolayer on the fiber surface, introducing carboxyl groups and double bonds. Subsequently, thionyl chloride (SOCl2) reacts with the surface carboxyl groups to undergo nucleophilic substitution, converting the carboxyl groups into more active acyl chloride groups. This process introduces active groups on the surface of the glass fiber, laying the foundation for subsequent modification.
[0019] (1) adding glass fiber and 3-[3-carboxyallylamide]propyltriethoxysilane to anhydrous ethanol, stirring and mixing, filtering the product, washing with alcohol, and drying to obtain carboxylated glass fiber; adding the carboxylated glass fiber to thionyl chloride, reflux reaction, filtering the product, washing with dichloromethane, and drying to obtain acyl chloride glass fiber;
[0020] Polyethylene glycol (PEG) grafting: The acyl chloride group on the surface of the acyl chloride glass fiber undergoes an esterification reaction with the terminal hydroxyl group of PEG. Triethylamine acts as a base to neutralize the HCl produced by the reaction and promote the reaction. Through this step, PEG is grafted to the surface of the glass fiber through an ester bond.
[0021] (2) Add polyethylene glycol and triethylamine to anhydrous dichloromethane, stir evenly, then add chlorinated glass fiber, stir to react, filter the product, wash with dichloromethane and deionized water in sequence, and dry to obtain an intermediate;
[0022] Octadecanethiol grafting: Finally, under the initiation of azobisisobutyronitrile (AIBN), octadecanethiol undergoes a free radical addition reaction with the double bonds remaining on the surface of the glass fiber. AIBN decomposes under heating conditions to produce free radicals, which initiate the reaction. This step allows octadecanethiol to be grafted onto the surface of the glass fiber through a thioether bond, further modifying the surface properties of the fiber.
[0023] (3) adding the intermediate and octadecyl mercaptan to tetrahydrofuran, continuously introducing nitrogen, adding azobisisobutyronitrile, and subjecting to reflux reaction, filtering the product, washing it with tetrahydrofuran and ethanol in sequence, and vacuum drying it to obtain the modified glass fiber.
[0024] Preferably, in step (1), the glass fiber has a diameter of 100-1000 nm and a length of 1-1000 μm.
[0025] Preferably, in step (1), the amount ratio of glass fiber to 3-[3-carboxyallylamide]propyltriethoxysilane is 10 g:3-6 g; and the stirring and mixing condition is stirring and mixing at room temperature for 4-6 hours.
[0026] Preferably, in step (1), the ratio of carboxylated glass fiber to thionyl chloride is 10 g: 50-100 mL; and the reflux reaction conditions are 70-80° C. for 3-5 h.
[0027] Preferably, in step (2), the usage ratio of polyethylene glycol, triethylamine and chlorinated glass fiber is 20 g: 1-5 mL: 10 g.
[0028] Preferably, in step (2), the stirring reaction condition is stirring the reaction at room temperature for 18 to 24 hours.
[0029] Preferably, in step (3), the usage ratio of the intermediate, octadecyl mercaptan and azobisisobutyronitrile is 10 g: 8-12 g: 0.1-1 g.
[0030] Preferably, in step (3), the reflux reaction conditions are reflux reaction at 60-70° C. for 18-24 h.
[0031] The present invention also claims a method for preparing the high-strength and high-toughness plastic packaging material, comprising the following steps:
[0032] High-density polyethylene, metallocene polyethylene and linear low-density polyethylene are mixed in a high-speed mixer for 3 to 5 minutes, and then modified glass fiber and calcium stearate are added, and the mixture is mixed for 5 to 10 minutes. The mixture is placed in a film blowing machine and blown at 160 to 190° C. to obtain the high-strength and high-toughness plastic packaging material.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1) The present invention proposes a high-strength and high-toughness plastic packaging material, which successfully combines the advantages of each component and overcomes the limitations of a single material by rationally proportioning high-density polyethylene, metallocene polyethylene, linear low-density polyethylene, modified glass fiber and calcium stearate. High-density polyethylene provides excellent rigidity, strength and chemical resistance; metallocene polyethylene has a narrow molecular weight distribution and uniform short chain branches, giving the material good toughness and processing performance; linear low-density polyethylene provides excellent tensile strength and impact resistance. Modified glass fiber, as a reinforcing filler, significantly improves the mechanical strength and thermal stability of the material. Calcium stearate, as a lubricant and dispersant, improves the fluidity and dispersibility of the material, and also has a certain toughening effect. This multi-component synergistic formula not only has excellent strength and toughness, but also maintains good processing performance and use performance. It can effectively reduce the problems of breakage, perforation and wear during packaging, transportation and use. In addition, it has good barrier properties and chemical resistance, can better protect the contents of the package and extend the shelf life of the product.
[0035] 2) The present invention provides a method for preparing modified glass fiber. First, carboxyl groups and double bonds are simultaneously introduced on the surface of glass fiber by using a silane coupling agent; then, the carboxyl groups are converted into acyl chloride groups, which react with polyethylene glycol to form densely arranged polyethylene glycol chains on the fiber surface; finally, thiol-ene click chemistry is used to react octadecyl mercaptan with the double bonds remaining on the fiber surface to introduce long-chain alkyl groups. This series of modification processes can improve the interfacial compatibility between glass fiber and polymer matrix, while giving the fiber surface multifunctional properties.
[0036] 3) The present invention provides a modified glass fiber, which forms a unique "molecular brush" structure on the surface of the glass fiber through a multi-step modification process, including polyethylene glycol segments and long-chain alkyl groups with good compatibility with the polymer matrix. This structure significantly improves the interfacial bonding force between the glass fiber and the polymer matrix and enhances the stress transfer efficiency. Polyethylene glycol grafting increases the surface potential value of the glass fiber and improves the dispersibility and stability of the glass fiber. At the same time, the polyethylene glycol chain interpenetrates with the molecular chain of the polymer material to achieve a stable embedding of the glass fiber. The long-chain alkyl group not only enhances the association with the glass fiber, but also forms a hanging chain in the matrix of the packaging material, further improving the mechanical properties and toughness of the material. Polyethylene glycol and long-chain alkyl groups can entangle with the matrix chain to synergistically improve the mechanical properties, mechanical properties and toughness of the packaging film. This multiple action mechanism enables the final packaging material to maintain good mechanical properties and chemical resistance in various complex environments. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0038] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.
[0039] Polyethylene glycol: CAS number: 25322-68-3, molecular weight: 2000, provided by Jinan Lingwei Chemical Co., Ltd.
[0040] A method for preparing a high-strength and high-toughness plastic packaging material comprises the following steps:
[0041] (1) Add 10 g of glass fiber and 3-6 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 4-6 hours, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 50-100 mL of thionyl chloride, reflux at 70-80° C. for 3-5 hours, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0042] (2) Add 20 g of polyethylene glycol and 1-5 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 18-24 h, filter the product, wash it three times with dichloromethane and deionized water, and dry it to obtain an intermediate;
[0043] (3) Add 10 g of the intermediate and 8-12 g of octadecanethiol to 100 mL of tetrahydrofuran, continue to introduce nitrogen, add 0.1-1 g of azobisisobutyronitrile, and reflux at 60-70° C. for 18-24 h. Filter the product, wash it with tetrahydrofuran and ethanol three times in sequence, and dry it in vacuum to obtain the modified glass fiber.
[0044] (4) 50-70 parts of high-density polyethylene, 10-30 parts of metallocene polyethylene, and 5-15 parts of linear low-density polyethylene are mixed in a high-speed mixer for 3-5 minutes, and then 5-12 parts of modified glass fiber and 1-3 parts of calcium stearate are added, and the mixture is mixed for 5-10 minutes. The mixture is placed in a film blowing machine and blown at 160-190° C. to obtain the high-strength and high-toughness plastic packaging material.
[0045] The present invention will be further described below through specific embodiments.
[0046] Example 1
[0047] A method for preparing a high-strength and high-toughness plastic packaging material comprises the following steps:
[0048] (1) Add 10 g of glass fiber and 6 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 6 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 80° C. for 3 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0049] (2) Add 20 g of polyethylene glycol and 5 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 24 h, filter the product, wash it three times with dichloromethane and deionized water, and dry it to obtain an intermediate;
[0050] (3) 10 g of the intermediate and 12 g of octadecyl mercaptan were added to 100 mL of tetrahydrofuran, nitrogen was continuously introduced, 1 g of azobisisobutyronitrile was added, and the mixture was refluxed at 70° C. for 18 h. The product was filtered, washed with tetrahydrofuran and ethanol three times in sequence, and dried in vacuo to obtain the modified glass fiber.
[0051] (4) 70 g of high-density polyethylene, 30 g of metallocene polyethylene, and 15 g of linear low-density polyethylene were mixed in a high-speed mixer for 5 min, and then 12 g of modified glass fiber and 3 g of calcium stearate were added. The mixture was mixed for another 10 min, and then placed in a film blowing machine for film blowing at 190° C. to obtain the high-strength and high-toughness plastic packaging material.
[0052] Example 2
[0053] A method for preparing a high-strength and high-toughness plastic packaging material comprises the following steps:
[0054] (1) Add 10 g of glass fiber and 5 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 5 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 78° C. for 4 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0055] (2) Add 20 g of polyethylene glycol and 4 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 22 h, filter the product, wash it with dichloromethane and deionized water three times in sequence, and dry it to obtain an intermediate;
[0056] (3) 10 g of the intermediate and 10 g of octadecyl mercaptan were added to 100 mL of tetrahydrofuran, nitrogen was continuously introduced, 0.6 g of azobisisobutyronitrile was added, and the mixture was refluxed at 68° C. for 22 h. The product was filtered, washed with tetrahydrofuran and ethanol three times in sequence, and dried in vacuum to obtain the modified glass fiber.
[0057] (4) 65 g of high-density polyethylene, 25 g of metallocene polyethylene, and 12 g of linear low-density polyethylene were mixed in a high-speed mixer for 4 min, and then 10 g of modified glass fiber and 2 g of calcium stearate were added. The mixture was mixed for another 8 min, and then placed in a film blowing machine for film blowing at 180° C. to obtain the high-strength and high-toughness plastic packaging material.
[0058] Example 3
[0059] A method for preparing a high-strength and high-toughness plastic packaging material comprises the following steps:
[0060] (1) Add 10 g of glass fiber and 4 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 5 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 74° C. for 4 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0061] (2) Add 20 g of polyethylene glycol and 3 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 20 h, filter the product, wash it with dichloromethane and deionized water three times in sequence, and dry it to obtain an intermediate;
[0062] (3) 10 g of the intermediate and 10 g of octadecyl mercaptan were added to 100 mL of tetrahydrofuran, nitrogen was continuously introduced, 0.4 g of azobisisobutyronitrile was added, and the mixture was refluxed at 64° C. for 20 h. The product was filtered, washed with tetrahydrofuran and ethanol three times in sequence, and dried in vacuum to obtain the modified glass fiber.
[0063] (4) 55 g of high-density polyethylene, 20 g of metallocene polyethylene, and 10 g of linear low-density polyethylene were mixed in a high-speed mixer for 4 min, and then 8 g of modified glass fiber and 2 g of calcium stearate were added. The mixture was mixed for another 8 min, and then placed in a film blowing machine for film blowing at 170° C. to obtain the high-strength and high-toughness plastic packaging material.
[0064] Example 4
[0065] A method for preparing a high-strength and high-toughness plastic packaging material comprises the following steps:
[0066] (1) Add 10 g of glass fiber and 3 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 4 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 70° C. for 5 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0067] (2) Add 20 g of polyethylene glycol and 1 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 18 h, filter the product, wash it three times with dichloromethane and deionized water, and dry it to obtain an intermediate;
[0068] (3) 10 g of the intermediate and 8 g of octadecyl mercaptan were added to 100 mL of tetrahydrofuran, nitrogen was continuously introduced, 0.1 g of azobisisobutyronitrile was added, and the mixture was refluxed at 60° C. for 24 h. The product was filtered, washed with tetrahydrofuran and ethanol three times in sequence, and dried in vacuo to obtain the modified glass fiber.
[0069] (4) 50 g of high-density polyethylene, 10 g of metallocene polyethylene, and 5 g of linear low-density polyethylene were mixed in a high-speed mixer for 3 min, and then 5 g of modified glass fiber and 1 g of calcium stearate were added. The mixture was mixed for 5 min, and the mixture was placed in a film blowing machine and blown at 160° C. to obtain the high-strength and high-toughness plastic packaging material.
[0070] Comparative Example 1
[0071] A method for preparing a plastic packaging material comprises the following steps:
[0072] (1) Add 10 g of glass fiber and 6 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 6 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 80° C. for 3 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0073] (2) Add 20 g of polyethylene glycol and 5 mL of triethylamine to 100 mL of anhydrous dichloromethane, stir evenly, then add 10 g of chlorinated glass fiber, stir and react at room temperature for 24 h, filter the product, wash it three times with dichloromethane and deionized water, and dry it to obtain an intermediate;
[0074] (3) 70 g of high-density polyethylene, 30 g of metallocene polyethylene, and 15 g of linear low-density polyethylene were mixed in a high-speed mixer for 5 min, and then 12 g of the intermediate and 3 g of calcium stearate were added. The mixture was mixed for another 10 min, and the mixture was placed in a film blowing machine and blown at 190° C. to obtain the plastic packaging material.
[0075] Comparative Example 2
[0076] A method for preparing a plastic packaging material comprises the following steps:
[0077] (1) Add 10 g of glass fiber and 6 g of 3-[3-carboxyallylamide]propyltriethoxysilane to 100 mL of anhydrous ethanol, stir and mix at room temperature for 6 h, filter the product, wash with alcohol, and dry to obtain carboxylated glass fiber; add 10 g of carboxylated glass fiber to 100 mL of thionyl chloride, reflux at 80° C. for 3 h, filter the product, wash with dichloromethane, and dry to obtain acyl chloride glass fiber;
[0078] (2) 70 g of high-density polyethylene, 30 g of metallocene polyethylene, and 15 g of linear low-density polyethylene were mixed in a high-speed mixer for 5 min, and then 12 g of acyl chloride glass fiber and 3 g of calcium stearate were added. The mixture was mixed for 10 min, and the mixture was placed in a film blowing machine for film blowing at 190° C. to obtain the plastic packaging material.
[0079] The packaging materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 were tested for transparency, tensile properties, puncture resistance, and tear resistance.
[0080] Transparency was tested by SDR850 high-precision transmittance tester at a visible light wavelength of 550nm. Tensile properties were tested in accordance with the test method of GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets". The film sample was 10mm wide and 180mm long. It was tested by XLM (PC) intelligent electronic tensile testing machine. The initial distance between the fixtures was 100mm and the tensile speed was 5mm / min. Each sample was tested 5 times in the transverse direction (TD) and longitudinal direction (MD), and the average tensile strength in the two directions was calculated. The puncture resistance performance refers to GB / T 10004-2008 "Plastic composite film for packaging, dry composite bag, extrusion composite" was tested, and the force required for puncturing the packaging material under the conditions of pillow diameter 1mm and pushing speed 50mm / min was measured as the puncture resistance; the tear strength test was carried out with reference to GB / T16578.1-2008 "Determination of tear resistance of plastic film and sheeting Part 1: Trouser tear method". Specific data are shown in Table 1.
[0081] Table 1 Packaging material performance test results
[0082]
[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A high-strength and high-toughness plastic packaging material, characterized in that: The invention is made of the following components by weight: 50-70 parts of high-density polyethylene, 10-30 parts of metallocene polyethylene, 5-15 parts of linear low-density polyethylene, 5-12 parts of modified glass fiber, and 1-3 parts of calcium stearate; The preparation method of the modified glass fiber comprises the following steps: (1) adding glass fiber and 3-[3-carboxyallylamide]propyltriethoxysilane to anhydrous ethanol, stirring and mixing, filtering the product, washing with alcohol, and drying to obtain carboxylated glass fiber; adding the carboxylated glass fiber to thionyl chloride, reflux reaction, filtering the product, washing with dichloromethane, and drying to obtain acyl chloride glass fiber; (2) Add polyethylene glycol and triethylamine to anhydrous dichloromethane, stir evenly, then add chlorinated glass fiber, stir to react, filter the product, wash with dichloromethane and deionized water in sequence, and dry to obtain an intermediate; (3) adding the intermediate and octadecyl mercaptan to tetrahydrofuran, continuously introducing nitrogen, adding azobisisobutyronitrile, reflux reaction, filtering the product, washing with tetrahydrofuran and ethanol in sequence, and vacuum drying to obtain the modified glass fiber; In step (3), the reflux reaction conditions are reflux reaction at 60-70° C. for 18-24 h.
2. The packaging material according to claim 1, characterized in that: In step (1), the diameter of the glass fiber is 100-1000 nm, and the length is 1-1000 μm.
3. The packaging material according to claim 1, characterized in that: In step (1), the ratio of glass fiber to 3-[3-carboxyallylamide]propyltriethoxysilane is 10 g:3-6 g; and the stirring and mixing condition is stirring and mixing at room temperature for 4-6 hours.
4. The packaging material according to claim 1, characterized in that: In step (1), the amount ratio of carboxylated glass fiber to thionyl chloride is 10 g: 50-100 mL; and the reflux reaction conditions are reflux reaction at 70-80° C. for 3-5 h.
5. The packaging material according to claim 1, characterized in that: In step (2), the usage ratio of polyethylene glycol, triethylamine and chlorinated glass fiber is 20 g:1~5 mL:10 g.
6. The packaging material according to claim 1, characterized in that: In step (2), the stirring reaction condition is stirring the reaction at room temperature for 18 to 24 hours.
7. The packaging material according to claim 1, characterized in that: In step (3), the usage ratio of the intermediate, octadecyl mercaptan and azobisisobutyronitrile is 10 g: 8-12 g: 0.1-1 g.
8. A method for preparing the high-strength and high-toughness plastic packaging material according to any one of claims 1 to 7, characterized in that: The steps include: High-density polyethylene, metallocene polyethylene and linear low-density polyethylene are mixed in a high-speed mixer for 3 to 5 minutes, and then modified glass fiber and calcium stearate are added, and the mixture is mixed for 5 to 10 minutes. The mixture is placed in a film blowing machine and blown at 160 to 190° C. to obtain the high-strength and high-toughness plastic packaging material.