A blended anti-drip polymer material and preparation method thereof

By using porous materials that controllable release of organic functional molecules as flame retardants in polymer materials, the problem of melting droplets during combustion of polymer materials is solved, which improves the anti-droplet performance and maintains the processability and mechanical properties of the material.

CN118667307BActive Publication Date: 2024-11-22DONGHUA UNIV +3
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411163548.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing polymer materials are prone to produce melt droplets when burning, resulting in fire safety hazards. The existing anti-droplet technology has problems with harsh reaction conditions and affecting the regularity and mechanical properties of polymers.

Method used

Using porous materials that controllable release of organic functional molecules as flame retardants, melt blend with polymer matrix, and anchor the organic functional molecules into the porous materials through chemical bonding, release them at high temperature to form a cross-linking reaction, enhancing melt viscosity To achieve anti-droplet effect.

Benefits of technology

It achieves the improvement of anti-droplet performance without melting droplets at high temperatures, while maintaining the processability and mechanical properties of the material. It is suitable for blending with polymer materials such as polyester and polyamide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118667307B_ABST
    Figure CN118667307B_ABST
Patent Text Reader

Abstract

The invention discloses a blended anti-melting drop polymer material and a preparation method thereof. The product is obtained by melt blending a polymer matrix and a flame retardant. The flame retardant is an organically modified porous material. The porous material is a porous material that can controllably release organic functional molecules. The material includes an inorganic porous modified powder and an organic functional molecule. The inorganic porous modified powder is an inorganic porous powder with a hydroxyl functional group. The organic functional molecules are all fixed on the inner surface of the pores of the inorganic porous modified powder. During preparation, the inorganic porous powder is treated to obtain an inorganic porous modified powder, and then an organic functional molecule solution is added to obtain a porous material that can controllably release organic functional molecules. Then, a coupling modifier is added to obtain a flame retardant, and finally the polymer matrix and the flame retardant are melt blended to obtain the product. The preparation method of the invention is simple. During preparation, the organic functional molecules are firmly anchored inside the pores of the porous material by chemical bonding technology, and the obtained product has an excellent flame retardant and anti-melting drop effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a blended anti-drip polymer material and a preparation method thereof. Background Art

[0002] Polymer materials are widely used in production and life due to their excellent performance, but their flammability and the problem of secondary combustion caused by a large number of droplets in addition to their own combustion make them a serious fire safety hazard. Therefore, how to improve the anti-droplet behavior of polymer materials has always been a key research direction of flame retardant materials, and it is also a difficult direction.

[0003] In order to solve the above problems, the prior art achieves the purpose of anti-dripping by means of blending and copolymerization.

[0004] The prior art introduces anti-drip groups into polymer molecular chains by copolymerization to achieve the purpose of anti-drip, such as document 1 "The high-temperature self-crosslinking contribution of azobenzene groups to the flame retardance and anti-dripping of copolyesters [J]. Journal of Materials Chemistry, A. Materials for energy and sustainability, 2013, 1 (32): 9264-9272.", document 2 "New application for aromatic Schiff base: High efficiency flame-retardant and anti-dripping action for polyesters [J]. Chemical Engineering Journal, 336: 622-632.", document 3 "A novel flame-retardant-free copolyester: cross-linking towards self extinguishing and non-dripping [J]. Journal of Materials Chemistry, 2012, 22 (37): 19849-19857.》, Patent Application CN202310790926.4. However, this method has several problems: (1) The reaction conditions are harsh and usually need to be carried out under high temperature and high pressure. The current common polymerization equipment cannot meet its production requirements and the production line needs to be replaced as a whole, which is unrealistic for industrial production; (2) After the anti-melting group is introduced into the polymer chain, the regularity of the polymer molecules is greatly destroyed, thereby affecting the crystallization performance of the polymer and seriously affecting the subsequent processing and molding. The mechanical properties of the products are often poor.

[0005] The method of blending and adding to achieve the purpose of anti-dripping does not require harsh reaction conditions and will not affect the regularity and crystallization properties of the polymer molecules. However, this method is often difficult to achieve the purpose of anti-dripping. In order to achieve flame retardant properties, flame retardants are added in excess in the prior art. When the amount of flame retardant added is too large, the mechanical properties of the polymer material will be much lower than that without adding anti-dripping components, and cannot meet the needs of most application scenarios. For example, patent application CN202311127587.8 discloses a method for preparing a flame-retardant and drip-inhibiting polyester fiber, wherein the polyester fiber contains polyester, flame-retardant polyester masterbatch, and drip-inhibiting agent, and the added mass ratio is 65~75:15~25:2~20. After co-spinning, the flame-retardant fiber is obtained, and the mass proportion of the flame-retardant masterbatch and the drip-inhibiting agent is 17~45%; for example, in document 4 "Synthesis, Characterization and Properties of Phosphorus-Containing Flame-Retardant Polymer PDPPP [D]. Sichuan University, 2004.", the flame retardant has a good flame retardant effect only after the addition amount of the flame retardant in the polymer reaches 8%, and document 5 "Synthesis and characterization of cyclic bisphenol A (phenylenephosphonate) oligomer and its flame retardancy application [J]. PolymerDegradation & Stability, 2015, 122: 161-168.》 reported a kind of oligomer flame retardant CPBA. When the mass addition amount of CPBA in polyester PBT reaches 25%, the oxygen index of PBT can be increased from 20.2% to 28.6%.

[0006] For example, patent application CN202311843594.8 discloses a halogen-free high temperature flame retardant polymer material and its preparation method, wherein the preparation method is to first prepare modified short basalt fiber and modified polypropylene, then melt and mix the modified short basalt fiber, modified polypropylene and potassium persulfate, extrude them, and then hot press and cool them to obtain the halogen-free high temperature flame retardant polymer material. However, the amount of flame retardant added in the preparation method is high, even reaching 10-20%. Although anti-melting droplet resistance is achieved, the mechanical properties of the obtained halogen-free high temperature flame retardant polymer material will be greatly reduced due to excessive addition of flame retardant.

[0007] In addition, for organic small molecule flame retardants, their blending and addition into the polymer matrix will affect the melt processability of the polymer material. At the same time, the organic small molecules will also migrate, affecting the overall performance of the material. Therefore, the organic functionalized molecules cannot be simply added directly into the polymer matrix for blending and processing.

[0008] Therefore, it is of great significance to study a blended anti-drip polymer material and a preparation method thereof to solve the above-mentioned problems existing in the prior art. Summary of the invention

[0009] The purpose of the present invention is to solve the problems existing in the prior art and to provide a blended anti-drip polymer material and a preparation method thereof.

[0010] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0011] A blended anti-melt dripping polymer material is obtained by melt blending a polymer matrix and a flame retardant, wherein the flame retardant is an organically modified porous material, and the porous material is a porous material capable of controllably releasing organic functional molecules;

[0012] The porous material capable of controlling the release of organic functional molecules comprises an inorganic porous modified powder and organic functional molecules, wherein the inorganic porous modified powder is an inorganic porous powder having a silane coupling agent chemically bonded inside the pores, and the organic functional molecules are all fixed on the inner surface of the pores of the inorganic porous modified powder;

[0013] The organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0014] ;

[0015] Wherein, R is an ester bond, an amide bond, an imide bond, , or , It indicates a carbon chain with 3 to 5 carbon atoms;

[0016] The polymer matrix is ​​polyester or polyamide;

[0017] Organic modification of porous materials refers to modification of porous materials by using a coupling modifier, wherein the coupling modifier is γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, vinyltriethoxysilane or trimethoxy[3-(methylamino)propyl]silane.

[0018] As the preferred technical solution:

[0019] In the blended anti-drip polymer material as described above, the amount of the flame retardant added relative to the polymer matrix is ​​1-5wt%.

[0020] As described above, the blended anti-drip polymer material has a UL-94 flame retardant grade of V-0 and has no drips when burned; the complex viscosity of the blended anti-drip polymer material at 290°C is 78~89 Pa•s, and the complex viscosity at 370°C is 180~288 Pa•s.

[0021] In the above-mentioned blended anti-drip polymer material, the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0022] or ;

[0023] In the formula, -R´- is -CH=CH-, -C≡C-, -CH=N- or -N=N-; at least one of -R1 to -R6 is an active functional group, and the rest are -H, and the active functional group is -NH2, -COOH or -OH.

[0024] A method for preparing a blended anti-drip polymer material as described in any one of the above items comprises the following steps:

[0025] (1) dispersing an inorganic porous powder in a mixed solvent of ethanol and water, and ultrasonically stirring at room temperature to obtain a dispersed system; the inorganic porous powder is silicon dioxide, titanium dioxide, aluminum oxide or zirconium oxide with a particle size of 2-3 μm and a pore size of 50-100 nm;

[0026] (2) filtering the dispersed system obtained in step (1), and vacuum drying the filtered wet product at 30-40°C for 8-16 hours, controlling the water content to 1-3%, to obtain an inorganic porous powder containing trace water. At this time, this part of the trace water is present in the pores of the porous powder;

[0027] (3) Adding an inorganic porous powder containing trace amounts of water and a silane coupling agent into a high-speed mixer, first mixing at room temperature at a speed of 3000 r / min for 1 to 2 h, then reducing the speed to 1000 r / min, heating to 80 to 100°C under a slightly negative pressure state, and reacting for 3 to 5 h until no water is discharged; the silane coupling agent is γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, vinyltriethoxysilane or trimethoxy[3-(methylamino)propyl]silane; the slightly negative pressure state refers to a state where the vacuum degree is -0.01 to -0.02 MPa;

[0028] (4) adding the powder obtained in step (3) into ethanol (the mass volume ratio of powder to ethanol is 20-30 g:100 ml), stirring for 0.5-1 h, filtering, and washing the filter cake with ethanol for 3-5 times. The washed filter cake is vacuum dried at 80-100° C. for 10-12 h to obtain an inorganic porous modified powder;

[0029] (5) adding the inorganic porous modified powder to an organic functional molecule solution (obtained by dissolving the organic functional molecules in a solvent, the solvent being ethanol, butanol, dimethylformamide, toluene, dimethyl sulfoxide or N-methylpyrrolidone), reacting under catalyst conditions, and filtering, washing and drying in sequence after the reaction is completed to obtain a porous material capable of controllably releasing the organic functional molecules;

[0030] (6) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer, and mixing the materials at a temperature of 60 to 80 °C and a speed of 3000 r / min for 1 to 2 h to obtain an organically modified porous material, i.e., a flame retardant;

[0031] (7) Melt-blending the polymer matrix with the flame retardant obtained in step (6) to obtain a blended anti-drip polymer material.

[0032] As the preferred technical solution:

[0033] In the method for preparing a blended anti-drip polymer material as described above, the mass concentration of the inorganic porous powder in the dispersion system of step (1) is 30-50%.

[0034] In the method for preparing a blended anti-drip polymer material as described above, in step (3), the mass ratio of the inorganic porous powder containing trace amounts of water to the silane coupling agent is 1:0.4-0.8.

[0035] The method for preparing a blended anti-drip polymer material as described above, wherein the mass concentration of the organic functional molecule solution in step (5) is 10-20%, the mass volume ratio of the inorganic porous modified powder to the organic functional molecule solution is 5-10 g:100 ml, the catalyst is one or two of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 1,3-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 4-dimethylaminopyridine, N-hydroxysuccinimide, p-toluenesulfonic acid, N,N'-carbonyldiimidazole, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 1-hydroxybenzotriazole, the reaction temperature is room temperature to 160°C, the reaction pressure is from normal pressure to 0.3 MPa, and the reaction time is 2 to 12 h.

[0036] In the method for preparing a blended anti-drip polymer material as described above, in step (6), the mass ratio of the porous material capable of controllably releasing organic functional molecules to the coupling modifier is 1:0.02-0.03.

[0037] In the method for preparing a blended anti-drip polymer material as described above, the temperature of melt blending in step (7) is 240-300°C.

[0038] Principle of the invention:

[0039] First, a micro-water environment is formed inside the pores of the inorganic porous powder through low-temperature drying. This micro-water environment provides the necessary conditions for the subsequent chemical reaction. Then, through high-speed stirring, the silane coupling agent is evenly dispersed inside and on the surface of the pores, forming a physical coating layer of the silane coupling agent inside and on the surface of the pores. The temperature is controlled to allow the coupling agent inside the pores to react chemically with the micro-water in the pores. The silane coupling agent after the reaction inside the pores is chemically bonded to the inner surface of the inorganic porous powder, and the reaction process is controlled under micro-negative pressure conditions. The small molecules generated in the reaction are discharged from the reaction system; the silane coupling agent on the surface of the powder after the reaction is eluted in an ethanol solution, the reaction conditions are controlled, and the organic functionalized molecules are chemically bonded with the silane coupling agent inside the inorganic porous powder through chemical reactions (esterification reaction, amidation reaction, addition reaction, Schiff base reaction, etc.) in an appropriate reaction system, at which time the organic functional molecules are anchored inside the inorganic porous powder; finally, an organic coating layer is formed on the surface of the inorganic porous powder through physical coating, so that the flame retardant of the present invention is obtained.

[0040] The design feature of the flame retardant of the present invention is that the organic functional molecules are firmly anchored inside the pores of the porous material through chemical bonding technology. This unique design enables the material to accurately release organic functional molecules that can trigger cross-linking reactions at high temperatures or when burning under specific temperature conditions. These released organic functional molecules undergo cross-linking reactions to form a three-dimensional network structure, thereby significantly enhancing the viscosity of the melt at high temperatures, effectively reducing the fluidity of the melt, and thus achieving an anti-drip effect.

[0041] Specifically, at processing temperatures (usually no more than 300°C), the porous hybrid material remains stable, does not release organic functional molecules, and does not undergo cross-linking reactions, thereby ensuring that the material's processability is not affected. In particular, the material is suitable for melt blending with polymer materials such as polyester and polyamide, and the chemical bonds anchoring the organic functional molecules (such as ester bonds, amide bonds, imine bonds, etc.) can exist stably at processing temperatures without causing any adverse effects on the polymer matrix.

[0042] However, when the temperature exceeds 300°C, such as when it encounters combustion or high temperature, the chemical bonds anchoring the organic functional molecules begin to break, and the organic functional molecules are released from the pores of the porous material and evenly dispersed in the polymer matrix. In the temperature range of 350~450°C, these released organic functional molecules undergo cross-linking reactions to form a solid three-dimensional network structure, which significantly increases the viscosity of the melt at high temperatures and effectively prevents the formation of droplets, thereby achieving the material's anti-droplet performance at high temperatures.

[0043] Beneficial effects:

[0044] (1) The present invention forms a chemical bond between the organic functionalized molecules and the silane coupling agent inside the inorganic porous powder, anchoring the organic functional molecules inside the inorganic porous powder, so that the material can accurately release the organic functional molecules that can trigger a cross-linking reaction at high temperature or when burning under specific temperature conditions, and the released organic functional molecules undergo a cross-linking reaction to form a three-dimensional network structure, thereby significantly enhancing the viscosity of the melt at high temperature and effectively reducing the fluidity of the melt, thereby achieving an anti-dripping effect, thereby improving the anti-dripping performance of the material at high temperature.

[0045] (2) The present invention uses porous materials to provide a place and active sites for the introduction of organic functional molecules, which can solve the influence of small molecular organic matter on the processing of polymer matrix. At the same time, the large pore surface area can achieve a high loading amount of organic molecules.

[0046] (3) The preparation process and preparation conditions of the present invention are simple, and the prepared polymer material has high anti-melting droplet performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a schematic diagram of the blended anti-drip polymer composite material in Example 1;

[0048] Figure 2 It is a complex viscosity diagram of the blended anti-drip polymer material prepared by compounding pure PET and PET+anti-drip flame retardant of Example 5 at different temperatures. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0050] The test methods involved in the performance indicators of the present invention are as follows:

[0051] UL-94 flame retardant grade: tested using a vertical burning tester in accordance with GB / T 2408-2008.

[0052] Complex viscosity: Tested using a rotational rheometer.

[0053] Tensile strength of polymer slices and blended anti-drip polymer materials: polymer slices and blended anti-drip polymer materials were tested in accordance with the standard GB / T 1040.2-2006.

[0054] The inorganic porous powder of the present invention is an inorganic porous powder with hydroxyl functional groups.

[0055] Example 1

[0056] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0057] (1) Preparation of raw materials:

[0058] Inorganic porous powder: silica with an average particle size of 2 μm and an average pore size of 50 nm;

[0059] Ethanol;

[0060] water;

[0061] Silane coupling agent: γ-aminopropyltriethoxysilane;

[0062] Organic functional molecule solution: The solvent is ethanol, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0063] ;

[0064] Catalyst: N, N'-diisopropylcarbodiimide;

[0065] Coupling modifier: γ-aminopropyltriethoxysilane;

[0066] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG600, tensile breaking strength: 52.6MPa;

[0067] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 30%;

[0068] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 30° C. for 16 h, controlling the water content to 1%, to obtain an inorganic porous powder containing trace amounts of water;

[0069] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer in a mass ratio of 1:0.4, first mixed at room temperature at a speed of 3000 r / min for 1 h, then the speed is reduced to 1000 r / min, the temperature is raised to 80 °C under a slightly negative pressure state, and the reaction is carried out for 5 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.01 MPa;

[0070] (5) adding the powder obtained in step (4) into ethanol at a mass volume ratio of 20 g:100 ml, stirring for 0.5 h and filtering, and washing the filter cake with ethanol three times. The washed filter cake was vacuum dried at 80 ° C for 12 h to obtain an inorganic porous modified powder;

[0071] (6) Adding the inorganic porous modified powder to a 10% mass concentration organic functional molecule solution at a mass volume ratio of 5 g:100 ml, reacting at a temperature of 120 ° C and a pressure of 0.3 MPa for 2 h under catalyst conditions, and filtering, washing, and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0072] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.02, and mixing the materials at a temperature of 60°C and a speed of 3000 r / min for 2 h to obtain an organically modified porous material, i.e., a flame retardant;

[0073] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0074] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5, and the amount of the flame retardant added relative to the polymer matrix is ​​2 wt%.

[0075] like Figure 1 As shown, the organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0076] ;

[0077] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength of the blended anti-drip polymer material is 53.8MPa, the complex viscosity at 290°C is 82Pa•s, and the complex viscosity at 370°C is 183Pa•s.

[0078] Comparative Example 1

[0079] A method for preparing a blended anti-drip polymer material is basically the same as Example 1, except that the operation of step (5) is omitted, that is, the inorganic porous modified powder in step (6) is replaced by the powder obtained in step (4).

[0080] The organic functional molecules in the final blended anti-drip polymer material are not combined with the surface of the inorganic porous powder, but are free in the reaction system; the UL-94 flame retardant grade of the blended anti-drip polymer material is V-1, and there are more droplets in the burning state; the tensile strength of the blended anti-drip polymer material is 47.9MPa, the complex viscosity at 290°C is 43Pa•s, and the complex viscosity at 370°C is 35Pa•s.

[0081] By comparing Comparative Example 1 with Example 1, it can be found that the UL-94 flame retardant grade and complex viscosity of Comparative Example 1 are significantly reduced. Comparative Example 1 has a certain anti-dripping effect, but it is much worse than the effect of Example 1. This is because after omitting the operation of step (5), there are more silane coupling agents adsorbed by physical interaction on the surface of the inorganic porous powder. This part of the silane coupling agent reacts in step (6) to obtain anti-dripping molecules (this part of the silane coupling agent is physically adsorbed with the inorganic porous powder and cannot be fixed, but exists freely in the form of small molecules, so it is called anti-dripping molecules). It is still adsorbed on the powder surface by physical action, affecting the grafting of anti-dripping molecules at the reaction sites in the powder pores. In addition, the physical interaction between the anti-dripping molecules and the powder surface is weak. During the blending process, these physical binding effects are destroyed. These small molecules originally adsorbed on the powder surface are free in the polymer material, resulting in a decrease in the viscosity of the polymer melt in the molten state, and there is no phenomenon that the anti-dripping molecules are concentratedly released after 330°C, which greatly increases the viscosity of the melt at high temperature. In addition, although the complex viscosity at 370°C in Comparative Example 1 is 35 Pa•s, it is also somewhat higher than that of pure PET (9 Pa•s), but this is only a partial cross-linking between free anti-drip molecules, which has a limited effect on the increase in melt viscosity and cannot achieve the purpose of anti-drip.

[0082] Comparative Example 2

[0083] A method for preparing a blended anti-melting droplet polymer material is basically the same as that in Example 1, except that: the water content of the powder in step (3) is controlled to be 5%, thereby obtaining an inorganic porous powder with a relatively high water content. At this water content, water not only remains in the pores of the porous powder, but also a relatively high amount of water remains on the surface of the powder. In step (4), the coupling agent can not only react in the pores of the powder, but can also be grafted on the surface of the porous powder through chemical bonds. In step (5), the coupling agent physically coated on the surface of the powder can be eluted, but the coupling agent grafted on the surface of the powder through chemical bonds is still coated on the surface of the powder. Since the surface of the powder is chemically coated by the coupling agent at this time, the organic functional molecules described in step (6) are blocked due to the steric hindrance effect of the coupling agent chemically coated on the surface, and cannot enter the pores, but can only react with the coupling agent on the surface of the powder, thereby obtaining a surface-coated modified porous powder, rather than a porous powder with controllable release of organic functional molecules as in Example 1.

[0084] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-1, and there are more droplets in the burning state; the tensile strength of the blended anti-drip polymer material is 38.4MPa, the complex viscosity at 290°C is 133Pa•s, and the complex viscosity at 370°C is 138Pa•s.

[0085] By comparing Comparative Example 2 with Example 1, it can be found that the UL-94 flame retardant grade and complex viscosity of Comparative Example 2 are significantly reduced. Comparative Example 2 has a certain anti-dripping effect, but it is much worse than the effect of Example 1, and the complex viscosity of the melt at the processing temperature (290°C) is 51 Pa•s higher than that of Example 1, while the complex viscosity at 370°C is not significantly improved, which indicates that the processability of the resin processing process in Comparative Example 2 is deteriorated, and the anti-dripping property is not improved. This is because the organic functional molecules are only grafted on the surface of the powder, and the excess functional groups exposed on the surface will further react with the polymer molecules at the processing temperature, affecting the processability. At the same time, there is no process of concentrated release of organic functional molecules at high temperature, and there will be no phenomenon of greatly increased viscosity of the melt at high temperature.

[0086] Example 2

[0087] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0088] (1) Preparation of raw materials:

[0089] Inorganic porous powder: titanium dioxide with an average particle size of 2.5 μm and an average pore size of 50 nm;

[0090] Ethanol;

[0091] water;

[0092] Silane coupling agent: γ-(2,3-epoxypropoxy)propyltrimethoxysilane;

[0093] Organic functional molecule solution: The solvent is butanol, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0094] ;

[0095] Catalyst: p-toluenesulfonic acid;

[0096] Coupling modifier: γ-(2,3-epoxypropoxy)propyltrimethoxysilane;

[0097] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG600, tensile breaking strength: 52.6MPa;

[0098] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 30%;

[0099] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 35°C for 12 hours, controlling the water content to 2%, to obtain an inorganic porous powder containing trace amounts of water;

[0100] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer at a mass ratio of 1:0.6, and the mixture is first mixed at a speed of 3000 r / min at room temperature for 1.25 h, and then the speed is reduced to 1000 r / min, and the temperature is raised to 90 °C under a slightly negative pressure state, and the mixture is reacted for 4 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.01 MPa;

[0101] (5) adding the powder obtained in step (4) to ethanol at a mass volume ratio of 25 g:100 ml, stirring for 0.75 h, filtering, and washing the filter cake with ethanol for 4 times. The washed filter cake was vacuum dried at 85° C. for 11.5 h to obtain an inorganic porous modified powder;

[0102] (6) adding the inorganic porous modified powder to a 16% mass concentration organic functional molecule solution at a mass volume ratio of 8 g:100 ml, reacting at 30 °C and normal pressure for 8 h under catalyst conditions, and filtering, washing and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0103] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.022, and mixing at a temperature of 70°C and a speed of 3000 r / min for 1 h to obtain an organically modified porous material, i.e., a flame retardant;

[0104] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0105] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5; and the amount of the flame retardant added relative to the polymer matrix is ​​1 wt%.

[0106] The organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0107] ;

[0108] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength of the blended anti-drip polymer material is 55.3MPa, the complex viscosity at 290°C is 78Pa•s, and the complex viscosity at 370°C is 236Pa•s.

[0109] Example 3

[0110] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0111] (1) Preparation of raw materials:

[0112] Inorganic porous powder: alumina with an average particle size of 2 μm and an average pore size of 80 nm;

[0113] Ethanol;

[0114] water;

[0115] Silane coupling agent: γ-(2,3-epoxypropoxy)propyltrimethoxysilane;

[0116] Organic functional molecule solution: The solvent is dimethylformamide, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0117] ;

[0118] Catalyst: 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride;

[0119] Coupling modifier: γ-(2,3-epoxypropoxy)propyltrimethoxysilane;

[0120] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG720, tensile breaking strength: 55.8MPa;

[0121] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 30%;

[0122] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 40° C. for 8 h, controlling the water content to 2.80%, to obtain an inorganic porous powder containing trace amounts of water;

[0123] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer at a mass ratio of 1:0.8, and the mixture is first mixed at a speed of 3000 r / min at room temperature for 1.5 h, and then the speed is reduced to 1000 r / min, and the temperature is raised to 100 °C under a slightly negative pressure state, and the mixture is reacted for 3 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.02 MPa;

[0124] (5) adding the powder obtained in step (4) to ethanol at a mass volume ratio of 30 g:100 ml, stirring for 1 hour, filtering, and washing the filter cake with ethanol 5 times. The washed filter cake is vacuum dried at 90° C. for 11 hours to obtain an inorganic porous powder with a hydroxyl functional group, i.e., an inorganic porous modified powder;

[0125] (6) adding the inorganic porous modified powder to a 20% mass concentration organic functional molecule solution at a mass volume ratio of 10 g:100 ml, reacting at 50 °C and normal pressure for 12 h under catalyst conditions, and filtering, washing and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0126] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.025, and mixing the materials at a temperature of 80°C and a speed of 3000 r / min for 1.5 h to obtain an organically modified porous material, i.e., a flame retardant;

[0127] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0128] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5; and the amount of the flame retardant added relative to the polymer matrix is ​​1 wt%.

[0129] The organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0130] ;

[0131] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength at break of the blended anti-drip polymer material is 58.1MPa, the complex viscosity at 290°C is 86Pa•s, and the complex viscosity at 370°C is 192Pa•s.

[0132] Example 4

[0133] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0134] (1) Preparation of raw materials:

[0135] Inorganic porous powder: zirconium oxide with an average particle size of 2.5 μm and an average pore size of 80 nm;

[0136] Ethanol;

[0137] water;

[0138] Silane coupling agent: N-(β-aminoethyl)-γ-aminopropyltriethoxysilane;

[0139] Organic functional molecule solution: The solvent is toluene, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0140] ;

[0141] Catalyst: a mixture of 4-dimethylaminopyridine and 1,3-dicyclohexylcarbodiimide in a mass ratio of 1:1;

[0142] Coupling modifier: N-(β-aminoethyl)-γ-aminopropyltriethoxysilane;

[0143] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG720, tensile breaking strength: 55.8MPa;

[0144] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 30%;

[0145] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 32° C. for 15 h, controlling the water content to 1.50%, to obtain an inorganic porous powder containing trace amounts of water;

[0146] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer in a mass ratio of 1:0.5, first mixed at room temperature at a speed of 3000 r / min for 1.75 h, then the speed is reduced to 1000 r / min, the temperature is raised to 85 °C under a slightly negative pressure state, and the reaction is carried out for 4.5 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.02 MPa;

[0147] (5) adding the powder obtained in step (4) to ethanol at a mass volume ratio of 20 g:100 ml, stirring for 0.5 h and filtering, and washing the filter cake with ethanol three times. The washed filter cake was vacuum dried at 95° C. for 10.5 h to obtain an inorganic porous modified powder;

[0148] (6) Adding the inorganic porous modified powder to an organic functional molecule solution with a mass volume ratio of 10 g:100 ml, reacting at a temperature of 160 ° C and a pressure of 0.3 MPa for 6 hours under catalyst conditions, and filtering, washing and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0149] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.03, and mixing the materials at a temperature of 65°C and a speed of 3000 r / min for 1.75 h to obtain an organically modified porous material, i.e., a flame retardant;

[0150] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0151] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5; and the amount of the flame retardant added relative to the polymer matrix is ​​5wt%.

[0152] The organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0153] ;

[0154] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength of the blended anti-drip polymer material is 56.3MPa, the complex viscosity at 290°C is 84Pa•s, and the complex viscosity at 370°C is 288Pa•s.

[0155] Example 5

[0156] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0157] (1) Preparation of raw materials:

[0158] Inorganic porous powder: silica with an average particle size of 2.5 μm and an average pore size of 100 nm;

[0159] Ethanol;

[0160] water;

[0161] Silane coupling agent: γ-aminopropyltrimethoxysilane;

[0162] Organic functional molecule solution: The solvent is dimethyl sulfoxide, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0163] ;

[0164] Catalyst: a mixture of N,N'-carbonyldiimidazole and 1-hydroxybenzotriazole in a mass ratio of 1:0.5;

[0165] Coupling modifier: γ-aminopropyltrimethoxysilane;

[0166] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG720, tensile breaking strength: 55.8MPa;

[0167] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 40%;

[0168] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 36°C for 11 hours, controlling the water content to 2%, to obtain an inorganic porous powder containing trace amounts of water;

[0169] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer at a mass ratio of 1:0.6, and the mixture is first mixed at a speed of 3000 r / min at room temperature for 2 h, and then the speed is reduced to 1000 r / min, and the temperature is raised to 95 °C under a slightly negative pressure state, and the mixture is reacted for 3.5 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.015 MPa;

[0170] (5) adding the powder obtained in step (4) to ethanol at a mass volume ratio of 30 g:100 ml, stirring for 0.75 h, filtering, and washing the filter cake with ethanol for 4 times. The washed filter cake was vacuum dried at 97 ° C for 10.25 h to obtain an inorganic porous modified powder;

[0171] (6) adding the inorganic porous modified powder to a 20% mass concentration organic functional molecule solution at a mass volume ratio of 8 g:100 ml, reacting at a temperature of 110 ° C and a pressure of 0.2 MPa for 8 h under catalyst conditions, and filtering, washing, and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0172] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.02, and mixing the materials at a temperature of 72°C and a speed of 3000 r / min for 1.4 h to obtain an organically modified porous material, i.e., a flame retardant;

[0173] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0174] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5; and the amount of the flame retardant added relative to the polymer matrix is ​​3wt%.

[0175] The organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0176] ;

[0177] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength of the blended anti-drip polymer material is 57.2MPa, the complex viscosity at 290°C is 89Pa•s, and the complex viscosity at 370°C is 180Pa•s.

[0178] The magnitude of the complex viscosity reflects the flowability of the melt under dynamic conditions. The larger the value, the greater the viscosity of the melt under this state, and the worse its fluidity. Figure 2 As shown, for pure PET or PET composite resin without anti-dripping function, as the temperature increases, the fluidity of the melt becomes better and the complex viscosity value becomes smaller; when the flame retardant (anti-dripping flame retardant) of the present invention is compounded with PET, when the temperature reaches above 330°C, the viscosity of the melt increases with the increase of temperature, so that the fluidity of the melt at this temperature becomes worse, thereby achieving no dripping in the combustion state.

[0179] Table 1

[0180]

[0181] Example 6

[0182] A method for preparing a blended anti-drip polymer material, the specific steps are as follows:

[0183] (1) Preparation of raw materials:

[0184] Inorganic porous powder: titanium dioxide with an average particle size of 3 μm and an average pore size of 100 nm;

[0185] Ethanol;

[0186] water;

[0187] Silane coupling agent: trimethoxy[3-(methylamino)propyl]silane;

[0188] Organic functional molecule solution: The solvent is N-methylpyrrolidone, and the organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows:

[0189] ;

[0190] Catalyst: 1-ethyl-(3-dimethylaminopropyl)carbodiimide;

[0191] Coupling modifier: trimethoxy[3-(methylamino)propyl]silane;

[0192] Polymer matrix: polyester, manufacturer: Sinopec, brand: FG600, tensile breaking strength: 52.6MPa;

[0193] (2) dispersing the inorganic porous powder in a mixed solvent of ethanol and water in a volume ratio of 4:1, and ultrasonically stirring at room temperature to obtain a dispersion system; the mass concentration of the inorganic porous powder in the dispersion system is 50%;

[0194] (3) filtering the dispersed system obtained in step (2), and vacuum drying the filtered wet product at 38°C for 9 hours, controlling the water content to 3%, to obtain an inorganic porous powder containing trace amounts of water;

[0195] (4) Inorganic porous powder containing trace amounts of water and silane coupling agent are added to a high-speed mixer at a mass ratio of 1:0.8, and the mixture is first mixed at a speed of 3000 r / min at room temperature for 2 h, and then the speed is reduced to 1000 r / min, and the temperature is raised to 98 °C under a slightly negative pressure state, and the mixture is reacted for 3.25 h until no water is discharged; the slightly negative pressure state refers to a state where the vacuum degree is -0.02 MPa;

[0196] (5) adding the powder obtained in step (4) into ethanol at a mass volume ratio of 20 g:100 ml, stirring for 1 hour and filtering, and washing the filter cake with ethanol for 5 times. The washed filter cake was vacuum dried at 100° C. for 10 hours to obtain an inorganic porous modified powder;

[0197] (6) Adding the inorganic porous modified powder to a 15% mass concentration organic functional molecule solution at a mass volume ratio of 5 g:100 ml, reacting at a temperature of 120 °C and a pressure of 0.2 MPa for 4 h under catalyst conditions, and filtering, washing, and drying in sequence after the reaction to obtain a porous material capable of controllably releasing organic functional molecules;

[0198] (7) adding the porous material capable of controlling the release of organic functional molecules and the coupling modifier into a high-speed mixer at a mass ratio of 1:0.025, and mixing the materials at a temperature of 75°C and a speed of 3000 r / min for 1.25 h to obtain an organically modified porous material, i.e., a flame retardant;

[0199] (8) melt-blending the polymer matrix and the flame retardant obtained in step (7) in a twin-screw extruder to obtain a blended anti-drip polymer material;

[0200] The temperatures of the zones of the twin-screw extruder are: 240°C in zone 1, 250°C in zone 2, 265°C in zone 3, 265°C in zone 4, and 260°C in zone 5; and the amount of the flame retardant added relative to the polymer matrix is ​​2 wt%.

[0201] The organic functional molecules in the final blended anti-drip polymer material are all fixed on the inner surface of the pores of the inorganic porous modified powder; the organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below;

[0202] ;

[0203] The UL-94 flame retardant grade of the blended anti-drip polymer material is V-0, and there are no drips in the burning state; the tensile strength at break of the blended anti-drip polymer material is 55.0MPa, the complex viscosity at 290°C is 85Pa•s, and the complex viscosity at 370°C is 192Pa•s.

Claims

1. A blended anti-drip polymer material, obtained by melt blending a polymer matrix and a flame retardant, characterized in that: The flame retardant is an organically modified porous material, and the porous material is a porous material capable of controllably releasing organic functional molecules; The porous material capable of controlling the release of organic functional molecules comprises an inorganic porous modified powder and organic functional molecules, wherein the inorganic porous modified powder is an inorganic porous powder having a silane coupling agent chemically bonded inside the pores, and the organic functional molecules are all fixed on the inner surface of the pores of the inorganic porous modified powder; The organic functional molecules are connected to the inner surface of the pores of the inorganic porous modified powder through the molecular structure shown below; Wherein, R is an ester bond, an amide bond, an imide bond, It indicates a carbon chain with 3 to 5 carbon atoms; The polymer matrix is ​​polyester or polyamide; Organic modification of porous materials refers to modification of porous materials with a coupling modifier, wherein the coupling modifier is γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, vinyltriethoxysilane or trimethoxy[3-(methylamino)propyl]silane; The preparation method of the blended anti-drip polymer material comprises the following steps: (1) dispersing the inorganic porous powder in a mixed solvent of ethanol and water, and ultrasonically stirring at room temperature to obtain a dispersed system; The inorganic porous powder is silicon dioxide, titanium dioxide, aluminum oxide or zirconium oxide with a particle size of 2 to 3 μm and a pore size of 50 to 100 nm; (2) filtering the dispersed system obtained in step (1), and vacuum drying the filtered wet product at 30-40° C. to control the water content to 1-3%, thereby obtaining an inorganic porous powder containing trace amounts of water; (3) adding an inorganic porous powder containing a trace amount of water and a silane coupling agent into a high-speed mixer, first mixing at room temperature at a speed of 3000 r / min for 1 to 2 hours, then reducing the speed to 1000 r / min, heating to 80 to 100° C. under a slightly negative pressure, and reacting until no water is discharged; the silane coupling agent is γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, vinyltriethoxysilane or trimethoxy[3-(methylamino)propyl]silane; The slightly negative pressure state refers to the state where the vacuum degree is -0.01~-0.02MPa; (4) adding the powder obtained in step (3) to ethanol, stirring for 0.5 to 1 hour, filtering, and washing the filter cake with ethanol for 3 to 5 times. The washed filter cake is vacuum dried at 80 to 100° C. for 10 to 12 hours to obtain an inorganic porous modified powder; (5) adding the inorganic porous modified powder to the organic functional molecule solution, reacting under catalyst conditions, and filtering, washing, and drying in sequence after the reaction is completed to obtain a porous material capable of controllably releasing the organic functional molecules; (6) adding the porous material capable of controllably releasing organic functional molecules and the coupling modifier into a high-speed mixer, and mixing the materials at a temperature of 60 to 80° C. and a speed of 3000 r / min for 1 to 2 hours to obtain a flame retardant; (7) Melt-blending the polymer matrix with the flame retardant obtained in step (6) to obtain a blended anti-drip polymer material.

2. A blended anti-drip polymer material according to claim 1, characterized in that: The flame retardant is added in an amount of 1 to 5 wt % relative to the polymer matrix.

3. A blended anti-drip polymer material according to claim 2, characterized in that: UL-94 flame retardant grade is V- Level 0, and there is no droplet in the burning state; the complex viscosity of the blended anti-droplet polymer material at 290°C is 78-89 Pa·s, and the complex viscosity at 370°C is 180-288 Pa·s.

4. The blended anti-drip polymer material according to claim 1, characterized in that: The organic functional molecule is an unsaturated conjugated cross-linkable molecule containing a benzene ring, and the structural formula is as follows: In the formula, -R′- is -CH=CH-, -C≡C-, -CH=N- or -N=N-; at least one of -R1 to -R6 is an active functional group, and the rest are -H, and the active functional group is -NH2, -COOH or -OH.

5. The blended anti-drip polymer material according to claim 1, characterized in that: The mass concentration of the inorganic porous powder in the dispersion system of step (1) is 30-50%.

6. The blended anti-drip polymer material according to claim 1, characterized in that: In step (3), the mass ratio of the inorganic porous powder containing trace amounts of water to the silane coupling agent is 1:0.4-0.

8.

7. The blended anti-drip polymer material according to claim 1, characterized in that: In step (5), the mass concentration of the organic functional molecule solution is 10-20%, the mass volume ratio of the inorganic porous modified powder to the organic functional molecule solution is 5-10g:100ml, the catalyst is one or two of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, 1,3-dicyclohexylcarbodiimide, N,N'-diisopropylcarbodiimide, 4-dimethylaminopyridine, N-hydroxysuccinimide, p-toluenesulfonic acid, N,N'-carbonyldiimidazole, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 1-hydroxybenzotriazole, the reaction temperature is room temperature to 160°C, the reaction pressure is from normal pressure to 0.3MPa, and the reaction time is 2 to 12h.

8. The blended anti-drip polymer material according to claim 1, characterized in that: In step (6), the mass ratio of the porous material capable of controllably releasing organic functional molecules to the coupling modifier is 1:0.02-0.

03.

9. The blended anti-drip polymer material according to claim 1, characterized in that: The temperature of melt blending in step (7) is 240-300°C.

Citation Information

Patent Citations

  • Molten-drop-resistant modified polyester fiber fabric

    CN116590807A

  • Preparation method of flame-retardant molten-drop-inhibiting polyester fiber

    CN117210956A

  • Halogen-free high-temperature-resistant flame-retardant high polymer material and preparation method thereof

    CN117487103A

  • Porous inorganic material with insecticidal and mothproof function and preparation method thereof

    CN102210302A

  • Efficient modified PP (Propene Polymer) composite materials for loading composite flame retardant through porous aluminum oxide and production method thereof

    CN104844930A