A method for preparing composite fiber toughened refractory material
By using the cladding and hyperbranching modification technology of polycrystalline alumina fibers in refractory materials, the fracture toughness and thermal stress distribution of refractory materials are solved, the thermal shock resistance and stability are improved, and the fiber performance is avoided. .
Patent Information
- Application Number
- CN202411170118.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-26
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of refractory materials, and in particular to a method for preparing a composite fiber toughened refractory material. Background Art
[0002] Refractory materials are a type of material that can maintain stable performance under high temperature conditions and can withstand special environments such as wear resistance, corrosion resistance, and chemical erosion resistance. In the traditional sense, refractory materials refer to inorganic refractory materials with a refractory temperature of not less than 1500°C. They are a type of basic material serving high-temperature technology and are widely used in construction, metallurgy, petrochemicals, aerospace and other fields.
[0003] Among them, inorganic refractories are mainly composed of materials such as alumina, silicate, calcium oxide, and silicon carbide. Specifically, from the perspective of raw material composition, the types of refractories include: siliceous (silicon oxide) refractories, aluminum silicate refractories, corundum refractories, magnesium refractories, magnesium calcium refractories, aluminum magnesium refractories, magnesium silicon refractories, carbon composite refractories, zirconium refractories, special refractories, etc. From the perspective of manufacturing methods, refractories can be divided into natural ore refractories and artificial refractories. From the perspective of material properties, refractories can be divided into block refractory products and amorphous refractories. From the perspective of heat treatment methods, refractories can be divided into unfired products, fired products, and molten cast products. From the perspective of refractoriness, refractories can be divided into ordinary refractories, advanced refractories, and special refractories. From the perspective of acidity and alkalinity, refractories can be divided into acidic refractories, neutral refractories, and alkaline refractories. In terms of density, refractory materials can be divided into lightweight refractory materials and heavy refractory materials.
[0004] Existing block refractory products have poor fracture toughness and the problem that fracture toughness limits the improvement of their thermal shock resistance. The existing technology uses fiber toughening to improve the above technical defects. Although it can improve the fracture toughness of refractory materials to a certain extent, the distribution uniformity of toughening fibers in the refractory matrix is not good, and the bonding performance with the refractory matrix is not ideal, resulting in uneven distribution of thermal stress such as thermal stress concentration in high-temperature environments. The overall stability of refractory materials in high-temperature and rapid temperature change environments is poor, and the thermal shock resistance needs to be further improved. The overall effective service life of refractory materials needs to be further improved.
[0005] Furthermore, after adding toughening fibers to the refractory materials, there are defects such as fiber recrystallization and excessive crystal growth in a high-temperature environment, which directly lead to a decrease in the performance of the toughening fibers in the refractory materials, and then cause the refractory materials to have unstable physical properties and poor overall stability. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides a preparation method of a composite fiber-reinforced refractory material, which can effectively improve the fracture toughness of the refractory material, improve the distribution uniformity of the composite fiber in the refractory material matrix, improve the bonding performance between the composite fiber and the refractory material matrix, effectively avoid thermal stress distribution defects such as thermal stress concentration of the refractory material in a high-temperature environment, improve the thermal stress distribution of the refractory material in a high-temperature environment, and further improve the overall stability and thermal shock resistance of the refractory material in a high-temperature and rapidly changing temperature environment; and effectively avoid the problem of reduced fiber performance in a high-temperature environment, and improve the physical properties of the refractory material.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a composite fiber toughened refractory material comprises the following steps: preparing primary composite fibers, preparing secondary composite fibers, surface pre-modification, hyperbranching modification, and mixed material sintering.
[0009] The method for preparing the primary composite fiber is as follows: adding glucose into deionized water, stirring and heating to 45-55° C., maintaining the temperature and stirring to dissolve, and obtaining a glucose solution with a mass concentration of 14-17wt%; then, under stirring conditions, using hydrochloric acid with a mass concentration of 32-36wt% to adjust the pH of the glucose solution to 1.5-2 to obtain a glucose treatment solution; immersing the polycrystalline alumina fiber in 80-85 times the weight of the glucose treatment solution, and ultrasonically treating for 20-30 minutes. After that, transfer it into an autoclave, seal the autoclave, evacuate the autoclave to a vacuum degree of 0.08-0.09MPa, let it stand for 1-2h, break the vacuum to normal pressure, control the autoclave to heat up to 190-200℃ at a heating rate of 2-2.5℃ / min, keep it warm for 4-5h, cool it to room temperature, separate the solid, wash the solid with 6-7 times its weight of deionized water, transfer it into a constant temperature drying oven, dry it at 85-90℃ to constant weight, and obtain a primary composite fiber.
[0010] In the preparation of the primary composite fiber, the alumina content of the polycrystalline alumina fiber is 86-90wt%, the fiber diameter is 3-4μm, and the fiber length is 55-70mm.
[0011] The method for preparing the secondary composite fiber comprises the following steps: uniformly mixing anhydrous ethanol and hydrogen peroxide (mass concentration 23-24wt%) at a weight ratio of 14-15:100, adding zirconium oxychloride octahydrate by stirring, and continuing to stir for 30-40 minutes; continuing to add acetylacetone and stirring for 10-20 minutes to obtain a sol treatment solution; adding the primary composite fiber into the sol treatment solution with a weight of 55-60 times, immersing for 30-50 minutes, separating out solids, transferring the solids into a constant temperature drying oven, drying at 80-85°C to constant weight, transferring the solids into a calcining furnace, heating to 800-820°C at a heating rate of 3-4°C / min in an argon atmosphere, calcining at the temperature for 2-3 hours, and cooling to room temperature to obtain the secondary composite fiber.
[0012] In the preparation of the secondary composite fiber, in the sol treatment liquid, the molar ratio of hydrogen peroxide, zirconium oxychloride octahydrate, and acetylacetone is 5.8-6.1:1:0.3-0.35.
[0013] The surface pre-modification method comprises the following steps: putting the secondary composite fiber into an ethanol solution (volume concentration of 80-85%), stirring for 10-20 minutes, heating to 42-48°C with stirring, and keeping the temperature; dripping γ-glycidyloxypropyltriethoxysilane with stirring, and after the dripping is completed, continuing to keep the temperature and stirring for 4-5 hours, separating the solid matter, washing the solid matter with 4-5 times the weight of deionized water, transferring the solid matter into a constant temperature drying oven, and drying the solid matter at 85-90°C to a constant weight to obtain the pre-modified fiber.
[0014] In the surface pre-modification, the weight ratio of the secondary composite fiber, the ethanol solution and γ-glycidyloxypropyltriethoxysilane is 12.5-13:200:3.5-4.
[0015] The hyperbranched modification method comprises the following steps: putting the pre-modified fiber into anhydrous ethanol, stirring for 10-20 minutes, heating to 55-60° C. with stirring, and dripping a hyperbranched modification liquid under the condition of heat preservation, reflux and stirring; after the hyperbranched modification liquid is dripped, the heat preservation, reflux and stirring are continued for 2-3 hours, solid matter is separated, and the solid matter is washed with 6-7 times the weight of deionized water, and then transferred to a constant temperature drying oven, and dried at 85-90° C. to constant weight to obtain a hyperbranched modified fiber.
[0016] In the hyperbranched modification, the weight ratio of the pre-modified fiber, anhydrous ethanol, and hyperbranched modification liquid is 29-30:300:16-16.5.
[0017] The preparation method of the hyperbranched modified liquid comprises the following steps: adding triethylenetetramine into 1.2-1.3 times of the weight of anhydrous ethanol, cooling to 0-2°C, keeping warm and stirring for 10-20 minutes, and then dropping methyl acrylate ethanol solution with stirring, and controlling the dropping rate to 0.8-1.2 mL / min. After the methyl acrylate ethanol solution is dropped, keeping warm and reacting for 2.5-3 hours to obtain a reaction liquid; transferring the reaction liquid into an evaporating kettle with reflux, keeping warm at 60-65°C for 60-80 minutes in a vacuum environment of 0.02-0.03 MPa, and then keeping warm at 120-125°C for 2-2.5 hours to obtain the hyperbranched modified liquid.
[0018] In the preparation of the hyperbranched modified liquid, the mass concentration of methyl acrylate in the ethanol solution of methyl acrylate is 40-42wt%;
[0019] The molar ratio of methyl acrylate to triethylenetetramine is 1:1.02-1.05.
[0020] The mixed material sintering method comprises the following steps: putting aluminum oxide powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol into a ball mill, and ball-milling and mixing for 2-3 hours to obtain a ball-milled product; drying the ball-milled product, uniformly mixing it with hyperbranched modified fibers, and then dry-pressing the product under a pressure of 15-18 MPa to obtain a green body; transferring the green body into a sintering furnace, sintering at 1300-1350° C. for 2-3 hours, and cooling the green body to room temperature to obtain a composite fiber-reinforced refractory material.
[0021] In the mixed material sintering, the weight ratio of alumina powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol is 68-70:28-31:7-8:7-8:3-3.5:2-2.5:58-62;
[0022] The weight ratio of alumina powder to hyperbranched modified fiber is 68-70:12-13.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The preparation method of the composite fiber toughened refractory material of the present invention adopts polycrystalline alumina fiber as the basic raw material fiber. In the step of preparing the primary composite fiber, a glucose treatment liquid is combined with the polycrystalline alumina fiber. After a hydrothermal reaction, a uniform carbon coating layer is formed on the outer surface of the polycrystalline alumina fiber to prepare the primary composite fiber. The high temperature resistance and thermal stability of the composite fiber are improved, which is beneficial to the structural stability of the composite fiber in the refractory material under high temperature conditions. The carbon coating layer of the composite fiber is used to optimize the heat conduction path of the refractory material, optimize the thermal stress distribution of the refractory material, avoid the thermal stress concentration defect of the refractory material caused by temperature change, and improve the toughness of the refractory material while improving the overall stability of the refractory material; then In the secondary composite fiber step, after using zirconium oxychloride octahydrate to prepare the sol treatment liquid, the primary composite fiber is combined with the sol treatment liquid, and the zirconium oxychloride is hydrolyzed to further form a uniform zirconium dioxide coating layer on the outer surface of the primary composite fiber to obtain the secondary composite fiber, thereby further improving the high temperature resistance of the composite fiber, effectively reducing the thermal stress of the refractory product due to temperature changes, improving the thermal shock resistance of the refractory material, and simultaneously improving the physical properties of the refractory material. When the fine cracks generated in a high temperature or rapid temperature change environment approach or reach the fiber surface, the interface damping effect of the composite fiber deflects and branches the fine cracks, thereby ensuring the toughening and strengthening effect of the composite fiber on the refractory material; then in the surface pre-modification step, The surface of the secondary composite fiber is pre-modified with γ-glycidyloxypropyltriethoxysilane to obtain a pre-modified fiber, which increases the reaction sites between the fiber and the subsequent amino-terminated hyperbranched polymer and improves the binding performance between the fiber and the amino-terminated hyperbranched polymer; then, in the hyperbranched modification step, the pre-modified fiber is hyperbranched modified with a hyperbranched modification liquid prepared by a specific method to obtain a hyperbranched modified fiber, and the amino groups of the amino-terminated hyperbranched polymer react and bond with the surface active groups of the fiber, thereby effectively improving the binding performance between the fiber and the refractory matrix, improving the uniformity of the fiber distribution in the refractory matrix, further optimizing the toughness, strength and other properties of the refractory, and improving the overall stability of the refractory; then, during the mixed material burning, the pre-modified fiber is subjected to hyperbranching modification, and the ... In the concluding step, the hyperbranched modified fibers are combined with raw materials such as aluminum oxide and silicon oxide to prepare composite fiber-reinforced refractory materials, which can effectively improve the fracture toughness of the refractory materials while improving the distribution uniformity of the composite fibers in the refractory matrix, improve the bonding performance of the composite fibers and the refractory matrix, effectively avoid thermal stress distribution defects such as thermal stress concentration of the refractory materials in high temperature environments, improve the thermal stress distribution of the refractory materials in high temperature environments, and further improve the overall stability and thermal shock resistance of the refractory materials in high temperature or rapidly changing temperature environments; and effectively avoid the problems of unstable physical properties and poor overall stability of the refractory materials due to defects such as recrystallization and excessive crystal growth of the composite fibers in the refractory materials in high temperature environments.
[0025] (2) The preparation method of the composite fiber toughened refractory material of the present invention, the prepared composite fiber toughened refractory material has a refractoriness of 1884-1891°C, an apparent porosity of 4.4-4.5%, and a room temperature fracture toughness of 2.13-2.17 MPa·m 1 / 2 The compressive strength at room temperature is 158.8-160.4MPa, the flexural strength at room temperature is 27.5-27.9MPa, and the interface bonding strength between the composite fiber and the refractory material is 31.2-31.8MPa.
[0026] (3) The preparation method of the composite fiber toughened refractory material of the present invention, the high temperature (1650°C) fracture toughness of the prepared composite fiber toughened refractory material is 1.84-1.90 MPa·m 1 / 2 The high temperature (1350℃) compressive strength is 154.6-155.1MPa, the high temperature (1500℃) flexural strength is 23.7-24.5MPa, and the heating permanent line change is 0.36-0.38%.
[0027] (4) The preparation method of the composite fiber toughened refractory material of the present invention comprises heating the composite fiber toughened refractory material to 1300°C at a heating rate of 20°C / min, keeping the temperature for 30 minutes, and then cooling it to room temperature by air cooling; after the aforementioned 20 times of rapid heating and air cooling, no deformation, cracks, or bubbling occurs, and the room temperature fracture toughness of the composite fiber toughened refractory material is 1.93-2.00 MPa·m 1 / 2 , high temperature (1650℃) fracture toughness is 1.65-1.72MPa·m 1 / 2 The high temperature (1350℃) compressive strength is 140.5-141.3MPa, and the high temperature (1500℃) flexural strength is 21.4-22.15MPa. DETAILED DESCRIPTION
[0028] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0029] Example 1
[0030] A method for preparing a composite fiber toughened refractory material, specifically comprising:
[0031] 1. Preparation of primary composite fiber
[0032] Glucose was added into deionized water, heated to 45°C with stirring, and dissolved by stirring to obtain a glucose solution with a mass concentration of 14wt%; then, under stirring, the pH of the glucose solution was adjusted to 1.5 with hydrochloric acid with a mass concentration of 32wt% to obtain a glucose-treated solution; polycrystalline alumina fiber was immersed in 80 times the weight of the glucose-treated solution, ultrasonically treated for 20 minutes, and then transferred to an autoclave, the autoclave was sealed, and evacuated to a vacuum degree of 0.08MPa in the autoclave, and after standing for 1 hour, the vacuum was broken to normal pressure, and the autoclave was controlled to heat up to 190°C at a heating rate of 2°C / min, and after keeping warm for 4 hours, it was cooled to room temperature, and the solid matter was separated, and the solid matter was washed with 6 times the weight of deionized water, and then transferred to a constant temperature drying oven, and dried at 85°C to constant weight to obtain a primary composite fiber.
[0033] Among them, the alumina content of the polycrystalline alumina fiber is 87.5wt%, the fiber diameter is 3.5μm, and the fiber length is 65mm.
[0034] 2. Preparation of secondary composite fibers
[0035] After evenly mixing anhydrous ethanol and hydrogen peroxide (mass concentration 23wt%) at a weight ratio of 14:100, zirconium oxychloride octahydrate was added with stirring and the stirring was continued for 30 minutes; acetylacetone was added and stirred for 10 minutes to obtain a sol treatment solution; the primary composite fiber was added into 55 times the weight of the sol treatment solution, immersed for 30 minutes, and the solid matter was separated. The solid matter was transferred to a constant temperature drying oven, dried at 80°C to constant weight, and then transferred to a calcining furnace. In an argon atmosphere, the temperature was increased to 800°C at a heating rate of 3°C / min, and the temperature was kept for calcination for 2 hours, and then cooled to room temperature to obtain a secondary composite fiber.
[0036] Among them, in the sol treatment liquid, the molar ratio of hydrogen peroxide, zirconium oxychloride octahydrate and acetylacetone is 5.8:1:0.3.
[0037] 3. Surface pre-modification
[0038] The secondary composite fiber was put into an ethanol solution (volume concentration of 80%), stirred for 10 minutes, then heated to 42°C with stirring and kept warm; γ-glycidyloxypropyltriethoxysilane was added dropwise with stirring, and after the addition was completed, the stirring was continued for 4 hours to separate the solid matter, and the solid matter was washed with 4 times the weight of deionized water, and then transferred to a constant temperature drying oven and dried at 85°C to constant weight to obtain the pre-modified fiber.
[0039] The weight ratio of the secondary composite fiber, the ethanol solution and γ-glycidyloxypropyltriethoxysilane is 12.5:200:3.5.
[0040] 4. Hyperbranched modification
[0041] The pre-modified fiber was put into anhydrous ethanol, stirred for 10 minutes, then heated to 55°C with stirring, and the hyperbranched modification liquid was dropped into the mixture under the stirring condition of heat preservation and reflux. After the hyperbranched modification liquid was added, the mixture was kept warm and refluxed for 2 hours to separate the solid matter. The solid matter was washed with 6 times the weight of deionized water, and then transferred to a constant temperature drying oven and dried at 85°C to constant weight to obtain the hyperbranched modified fiber.
[0042] The weight ratio of the pre-modified fiber, anhydrous ethanol and hyperbranched modified liquid is 29:300:16.
[0043] The preparation method of the hyperbranched modified liquid is as follows: adding triethylenetetramine to 1.2 times the weight of anhydrous ethanol, cooling to 0°C, keeping warm and stirring for 10 minutes, and then dropping an ethanol solution of methyl acrylate with stirring, and controlling the dropping rate to 0.8mL / min. After the dropwise addition of the ethanol solution of methyl acrylate is completed, keeping warm and reacting for 2.5 hours to obtain a reaction liquid; transferring the reaction liquid to an evaporating kettle with reflux, keeping warm at 60°C for 60 minutes in a vacuum environment of 0.02MPa, and then keeping warm at 120°C for 2 hours to obtain a hyperbranched modified liquid.
[0044] Wherein, in the ethanol solution of methyl acrylate, the mass concentration of methyl acrylate is 40wt%.
[0045] The molar ratio of methyl acrylate to triethylenetetramine is 1:1.02.
[0046] 5. Mixing and sintering
[0047] Alumina powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol are put into a ball mill, and ball-milled for 2 hours to obtain a ball-milled product; the ball-milled product is dried, mixed evenly with hyperbranched modified fibers, and then dry-pressed under a pressure of 15 MPa to obtain a green body; the green body is transferred into a sintering furnace, sintered at 1300°C for 2 hours, and cooled to room temperature to obtain a composite fiber-reinforced refractory material.
[0048] Among them, the weight ratio of aluminum oxide powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol is 68:28:7:7:3:2:58.
[0049] The weight ratio of alumina powder to hyperbranched modified fibers is 68:12.
[0050] Example 2
[0051] A method for preparing a composite fiber toughened refractory material, specifically comprising:
[0052] 1. Preparation of primary composite fiber
[0053] Glucose was added into deionized water, heated to 50°C with stirring, and dissolved by stirring at this temperature to obtain a glucose solution with a mass concentration of 16wt%; then, under stirring conditions, the pH of the glucose solution was adjusted to 1.8 with hydrochloric acid with a mass concentration of 35wt% to obtain a glucose-treated solution; polycrystalline alumina fiber was immersed in 82 times the weight of the glucose-treated solution, ultrasonically treated for 25 minutes, and then transferred to an autoclave, the autoclave was sealed, and evacuated to a vacuum degree of 0.085MPa in the autoclave, and after standing for 1.5 hours, the vacuum was broken to normal pressure, and the autoclave was controlled to heat up to 195°C at a heating rate of 2.2°C / min, and after keeping warm for 4.5 hours, it was cooled to room temperature, the solid matter was separated, and the solid matter was washed with 6.5 times the weight of deionized water, and then transferred to a constant temperature drying oven, and dried at 88°C to constant weight to obtain a primary composite fiber.
[0054] Among them, the alumina content of the polycrystalline alumina fiber is 87.5wt%, the fiber diameter is 3.5μm, and the fiber length is 65mm.
[0055] 2. Preparation of secondary composite fibers
[0056] After mixing anhydrous ethanol and hydrogen peroxide (mass concentration 23.5wt%) evenly at a weight ratio of 14.5:100, zirconium oxychloride octahydrate was added with stirring and stirring was continued for 35 minutes; acetylacetone was continued to be added and stirred for 15 minutes to obtain a sol treatment solution; the primary composite fiber was added into 58 times the weight of the sol treatment solution, immersed for 40 minutes, and the solid was separated. The solid was transferred to a constant temperature drying oven, dried at 82°C to constant weight, and then transferred to a calcining furnace. In an argon atmosphere, the temperature was increased to 810°C at a heating rate of 3.5°C / min, and the temperature was kept for calcination for 2.5 hours, and then cooled to room temperature to obtain a secondary composite fiber.
[0057] Among them, in the sol treatment liquid, the molar ratio of hydrogen peroxide, zirconium oxychloride octahydrate, and acetylacetone is 6:1:0.32.
[0058] 3. Surface pre-modification
[0059] The secondary composite fiber was put into an ethanol solution (volume concentration of 82%), stirred for 15 minutes, then heated to 45°C with stirring and kept warm; γ-glycidyloxypropyltriethoxysilane was added dropwise with stirring, and after the addition was completed, the stirring was continued for 4.5 hours of keeping warm, and the solid matter was separated. After the solid matter was washed with 4.5 times the weight of deionized water, it was transferred to a constant temperature drying oven and dried at 88°C to constant weight to obtain the pre-modified fiber.
[0060] The weight ratio of the secondary composite fiber, the ethanol solution and γ-glycidyloxypropyltriethoxysilane is 12.8:200:3.7.
[0061] 4. Hyperbranched modification
[0062] The pre-modified fiber was put into anhydrous ethanol, stirred for 15 minutes, then heated to 57°C with stirring, and the hyperbranched modification liquid was dropped into the mixture under the condition of heat preservation and reflux stirring. After the hyperbranched modification liquid was added, the mixture was kept warm and refluxed for 2.5 hours, and the solid was separated. The solid was washed with 6.5 times the weight of deionized water, and then transferred to a constant temperature drying oven and dried at 88°C to constant weight to obtain a hyperbranched modified fiber.
[0063] The weight ratio of the pre-modified fiber, anhydrous ethanol and hyperbranched modified liquid is 29.5:300:16.2.
[0064] The preparation method of the hyperbranched modified liquid is as follows: adding triethylenetetramine to 1.25 times the weight of anhydrous ethanol, cooling to 1°C, keeping warm and stirring for 15 minutes, and then dropping an ethanol solution of methyl acrylate with stirring, and controlling the dropping rate to 0.9 mL / min. After the dropwise addition of the ethanol solution of methyl acrylate is completed, keeping warm and reacting for 2.8 hours to obtain a reaction liquid; transferring the reaction liquid to an evaporating kettle with reflux, keeping warm at 62°C for 70 minutes in a vacuum environment of 0.025 MPa, and then keeping warm at 122°C for 2.3 hours to obtain a hyperbranched modified liquid.
[0065] Wherein, in the ethanol solution of methyl acrylate, the mass concentration of methyl acrylate is 41wt%.
[0066] The molar ratio of methyl acrylate to triethylenetetramine is 1:1.03.
[0067] 5. Mixing and sintering
[0068] Alumina powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol are put into a ball mill, and ball-milled for 2.5 hours to obtain a ball-milled product; the ball-milled product is dried, mixed evenly with hyperbranched modified fibers, and then dry-pressed under a pressure of 17 MPa to obtain a green body; the green body is transferred into a sintering furnace, sintered at 1330°C for 2.5 hours, and cooled to room temperature to obtain a composite fiber-reinforced refractory material.
[0069] Among them, the weight ratio of aluminum oxide powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol is 69:30:7.5:7.5:3.3:2.2:60.
[0070] The weight ratio of alumina powder to hyperbranched modified fibers is 69:12.5.
[0071] Example 3
[0072] A method for preparing a composite fiber toughened refractory material, specifically comprising:
[0073] 1. Preparation of primary composite fiber
[0074] Glucose was added into deionized water, heated to 55°C with stirring, and dissolved by stirring at this temperature to obtain a glucose solution with a mass concentration of 17wt%; then, under stirring, the pH of the glucose solution was adjusted to 2 with hydrochloric acid with a mass concentration of 36wt% to obtain a glucose-treated solution; polycrystalline alumina fiber was immersed in 85 times the weight of the glucose-treated solution, ultrasonically treated for 30 minutes, and then transferred into an autoclave, which was sealed and evacuated to a vacuum degree of 0.09MPa in the autoclave. After standing for 2 hours, the vacuum was broken to normal pressure, and the autoclave was controlled to heat up to 200°C at a heating rate of 2.5°C / min, and after being kept warm for 5 hours, it was cooled to room temperature, the solid matter was separated, and the solid matter was washed with 7 times the weight of deionized water, and then transferred into a constant temperature drying oven, and dried at 90°C to constant weight to obtain a primary composite fiber.
[0075] Among them, the alumina content of the polycrystalline alumina fiber is 87.5wt%, the fiber diameter is 3.5μm, and the fiber length is 65mm.
[0076] 2. Preparation of secondary composite fibers
[0077] After mixing anhydrous ethanol and hydrogen peroxide (mass concentration 24wt%) in a weight ratio of 15:100, zirconium oxychloride octahydrate was added with stirring and stirring was continued for 40 minutes; acetylacetone was added and stirred for 20 minutes to obtain a sol treatment solution; the primary composite fiber was added into 60 times the weight of the sol treatment solution, immersed for 50 minutes, and the solid was separated. The solid was transferred to a constant temperature drying oven, dried at 85°C to constant weight, and then transferred to a calcining furnace. In an argon atmosphere, the temperature was increased to 820°C at a heating rate of 4°C / min, and the temperature was kept for calcination for 3 hours, and then cooled to room temperature to obtain a secondary composite fiber.
[0078] Among them, in the sol treatment liquid, the molar ratio of hydrogen peroxide, zirconium oxychloride octahydrate, and acetylacetone is 6.1:1:0.35.
[0079] 3. Surface pre-modification
[0080] The secondary composite fiber was put into an ethanol solution (volume concentration of 85%), stirred for 20 minutes, then heated to 48°C with stirring and kept warm; γ-glycidyloxypropyltriethoxysilane was added dropwise with stirring, and after the addition was completed, the stirring was continued for 5 hours to separate the solid matter, and the solid matter was washed with 5 times the weight of deionized water, and then transferred to a constant temperature drying oven and dried at 90°C to constant weight to obtain the pre-modified fiber.
[0081] The weight ratio of the secondary composite fiber, the ethanol solution and γ-glycidyloxypropyltriethoxysilane is 13:200:4.
[0082] 4. Hyperbranched modification
[0083] The pre-modified fiber was put into anhydrous ethanol, stirred for 20 minutes, then heated to 60°C with stirring, and the hyperbranched modification liquid was dropped into the mixture under the stirring condition of heat preservation and reflux. After the hyperbranched modification liquid was added, the mixture was kept warm and refluxed for 3 hours to separate the solid matter. The solid matter was washed with 7 times the weight of deionized water, and then transferred to a constant temperature drying oven and dried at 90°C to constant weight to obtain the hyperbranched modified fiber.
[0084] The weight ratio of the pre-modified fiber, anhydrous ethanol and hyperbranched modified liquid is 30:300:16.5.
[0085] The preparation method of the hyperbranched modified liquid is as follows: adding triethylenetetramine to 1.3 times the weight of anhydrous ethanol, cooling to 2°C, keeping warm and stirring for 20 minutes, and then dropping an ethanol solution of methyl acrylate with stirring, and controlling the dropping rate to be 1.2mL / min. After the dropwise addition of the ethanol solution of methyl acrylate is completed, keeping warm and reacting for 3 hours to obtain a reaction liquid; transferring the reaction liquid to an evaporating kettle with reflux, keeping warm at 65°C for 80 minutes in a vacuum environment of 0.03MPa, and then keeping warm at 125°C for 2.5 hours to obtain a hyperbranched modified liquid.
[0086] Wherein, in the ethanol solution of methyl acrylate, the mass concentration of methyl acrylate is 42wt%.
[0087] The molar ratio of methyl acrylate to triethylenetetramine is 1:1.05.
[0088] 5. Mixing and sintering
[0089] Alumina powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol are put into a ball mill, and ball-milled for 3 hours to obtain a ball-milled product; the ball-milled product is dried, mixed evenly with hyperbranched modified fibers, and then dry-pressed under a pressure of 18 MPa to obtain a green body; the green body is transferred into a sintering furnace, sintered at 1350°C for 3 hours, and cooled to room temperature to obtain a composite fiber-reinforced refractory material.
[0090] Among them, the weight ratio of aluminum oxide powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and anhydrous ethanol is 70:31:8:8:3.5:2.5:62.
[0091] The weight ratio of alumina powder to hyperbranched modified fibers is 70:13.
[0092] Comparative Example 1
[0093] The technical solution of Example 2 is adopted, but the differences are: 1) the preparation of the primary composite fiber is omitted, and the polycrystalline alumina fiber is directly used in the step of preparing the secondary composite fiber; 2) the hyperbranching modification step is omitted.
[0094] Comparative Example 2
[0095] The technical solution of Example 2 is adopted, but the differences are: 1) the preparation of secondary composite fibers is omitted, and primary composite fibers are used for subsequent processing; 2) the surface pre-modification step is omitted.
[0096] The preparation methods of Examples 1-3 and Comparative Examples 1-2 were used to test the refractoriness, apparent porosity, fracture toughness at room temperature, fracture toughness at high temperature (1650°C), compressive strength at room temperature, compressive strength at high temperature (1350°C), flexural strength at room temperature, flexural strength at high temperature (1500°C), permanent line change upon heating, and interface bonding strength between the composite fiber and the refractory material of the prepared composite fiber-toughened refractory material.
[0097] Among them, the refractoriness detection method refers to GB / T 7322-2017 "Refractoriness Test Method for Refractory Materials".
[0098] The detection of apparent porosity refers to GB / T 2997-2015 "Test method for bulk density, apparent porosity and true porosity of dense shaped refractory products".
[0099] The single-edge notched beam method (SENB method) was used to test the room-temperature fracture toughness and high-temperature (1650°C) fracture toughness.
[0100] The test of room temperature compressive strength refers to GB / T 5072-2023 "Test method for room temperature compressive strength of refractory materials".
[0101] The test of high temperature compressive strength refers to GB / T 34218-2017 "Test method for high temperature compressive strength of refractory materials", and the test temperature is set to 1350℃.
[0102] The test of room temperature flexural strength refers to GB / T 3001-2017 "Test method for room temperature flexural strength of refractory materials".
[0103] The test of high temperature flexural strength refers to GB / T 3002-2017 "Test method for high temperature flexural strength of refractory materials", and the test temperature is set to 1500℃.
[0104] The detection of permanent linear changes upon heating refers to the length measuring instrument method of GB / T 5988-2022 "Test method for permanent linear changes upon heating of refractory materials", and the test temperature is set to 1300°C.
[0105] The interfacial bonding strength between the composite fiber and the refractory material is tested. The interfacial bonding strength between the composite fiber (i.e., hyperbranched modified fiber) and the refractory matrix is tested. Specifically, an Instron 3343 universal testing machine is used to conduct a single fiber pull-out test at room temperature, and a 10N mechanical sensor is set. The load measurement accuracy is ±0.5%, and the loading rate is set to 0.01 mm / s; each group is tested 10 times and the average value is taken. Among them, the calculation method of the interfacial bonding strength is: the maximum load of the composite fiber pulling out the refractory matrix / (single fiber diameter×single fiber length×π).
[0106] The specific results are shown in the following table:
[0107]
[0108] Further, the composite fiber toughened refractory materials were made into rectangular samples of 115mm×65mm×65mm using the preparation methods of Examples 1-3 and Comparative Examples 1-2. Each sample was placed in a high-temperature resistance furnace, and the heating rate was controlled to be 20℃ / min. The temperature was raised to 1300℃. After keeping the temperature for 30 minutes, the sample was taken out and the sample was blown to room temperature with compressed air at room temperature with a pressure of 0.1MPa. After repeating the aforementioned rapid heating and air cooling process 20 times, each sample was observed for deformation, cracks, and bubbling. The room-temperature fracture toughness, high-temperature (1650℃) fracture toughness, high-temperature (1350℃) compressive strength, and high-temperature (1500℃) flexural strength of each sample were tested. The specific results are shown in the following table:
[0109]
[0110] It can be seen that the preparation method of the composite fiber toughened refractory material of the present invention adopts polycrystalline alumina fiber as the basic raw material fiber. In the step of preparing the primary composite fiber, a glucose treatment liquid is combined with the polycrystalline alumina fiber. After the hydrothermal reaction, a uniform carbon coating layer is formed on the outer surface of the polycrystalline alumina fiber to prepare the primary composite fiber, which can improve the high temperature resistance and thermal stability of the composite fiber, and is beneficial to the structural stability of the composite fiber in the refractory material under high temperature conditions. The carbon coating layer of the composite fiber optimizes the heat conduction path of the refractory material, optimizes the thermal stress distribution of the refractory material, avoids the thermal stress concentration defect of the refractory material caused by temperature change, and improves the overall stability of the refractory material while improving the toughness of the refractory material. Then in the secondary composite fiber step, after preparing the sol treatment liquid with zirconium oxychloride octahydrate, the primary composite fiber is combined with the sol treatment liquid, and the zirconium oxychloride is hydrolyzed to further form a uniform zirconium dioxide coating layer on the outer surface of the primary composite fiber to obtain the secondary composite fiber, thereby further improving the high temperature resistance of the composite fiber, effectively reducing the thermal stress of the refractory product due to temperature changes, improving the thermal shock resistance of the refractory material, and simultaneously improving the physical properties of the refractory material. When the fine cracks generated in a high temperature or rapid temperature change environment approach or reach the fiber surface, the interface damping effect of the composite fiber deflects and branches the fine cracks, thereby ensuring the toughening and strengthening effect of the composite fiber on the refractory material; then in the surface pre-modification step, The surface of the secondary composite fiber is pre-modified by using γ-glycidyloxypropyltriethoxysilane to obtain pre-modified fiber, the reaction sites between the fiber and the subsequent amino-terminated hyperbranched polymer are increased, and the bonding performance between the fiber and the amino-terminated hyperbranched polymer is improved; then in the hyperbranched modification step, the pre-modified fiber is hyperbranched modified by using a hyperbranched modification liquid prepared by a specific method to obtain a hyperbranched modified fiber, and the amino groups of the amino-terminated hyperbranched polymer are reacted and bonded with the surface active groups of the fiber, so as to effectively improve the bonding performance between the fiber and the refractory matrix, improve the uniformity of the distribution of the fiber in the refractory matrix, further optimize the toughness, strength and other properties of the refractory, and improve the overall stability of the refractory; then in the mixed material burning In the concluding step, the hyperbranched modified fibers are combined with raw materials such as aluminum oxide and silicon oxide to prepare composite fiber-reinforced refractory materials, which can effectively improve the fracture toughness of the refractory materials while improving the distribution uniformity of the composite fibers in the refractory matrix, improve the bonding performance of the composite fibers and the refractory matrix, effectively avoid thermal stress distribution defects such as thermal stress concentration of the refractory materials in high temperature environments, improve the thermal stress distribution of the refractory materials in high temperature environments, and further improve the overall stability and thermal shock resistance of the refractory materials in high temperature or rapidly changing temperature environments; and effectively avoid the problem of unstable physical properties and poor overall stability of the refractory materials due to defects such as recrystallization and excessive crystal growth of the composite fibers in the refractory materials in high temperature environments.
[0111] It can be seen from Comparative Example 1 that after omitting the steps of preparing a composite fiber and hyperbranched modification, it is impossible to achieve thermal stress optimization of the refractory material through the carbon coating layer, and it is impossible to effectively avoid the thermal stress concentration defects of the refractory material caused by temperature changes. The fracture toughness and physical properties of the refractory material are reduced to a certain extent, and the interface bonding strength between the composite fiber and the refractory material is significantly reduced; at the same time, the overall stability of the refractory material is reduced, and the fracture toughness, compressive strength and flexural strength under high temperature and rapid temperature change conditions are significantly reduced, and deformation, cracks and bubbling phenomena occur.
[0112] It can be seen from Comparative Example 2 that after omitting the steps of preparing secondary composite fibers and pre-modification of the surface, the high temperature resistance of the composite fibers cannot be further improved, the thermal stress distribution of the refractory material cannot be further optimized, and the physical properties and thermal shock resistance of the refractory material are reduced to a certain extent; at the same time, in the subsequent hyperbranched modification step, the binding performance of the fiber and the amino-terminated hyperbranched polymer is reduced, the hyperbranched modification effect is poor, the binding performance of the composite fiber and the refractory matrix is reduced, and the fracture toughness, physical properties and overall stability of the refractory material cannot be further improved, which is specifically manifested in that the fracture toughness, compressive strength, flexural strength of the refractory material, and the interface bonding strength between the composite fiber and the refractory material are all reduced to a certain extent; at the same time, the overall stability of the refractory material is reduced, and the fracture toughness, compressive strength, and flexural strength under high temperature and rapid temperature change conditions are all significantly reduced, and deformation, cracks, and bubbling phenomena occur.
[0113] Unless otherwise specified, all percentages used in the present invention are by mass.
[0114] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite fiber toughened refractory material, characterized in that: The method comprises the following steps: preparing primary composite fiber, preparing secondary composite fiber, surface pre-modification, hyperbranching modification, and mixed material sintering; The method for preparing the primary composite fiber comprises: dipping the polycrystalline alumina fiber into the glucose treatment solution, transferring the polycrystalline alumina fiber into an autoclave after being evenly dispersed, sealing the autoclave, allowing the autoclave to stand in a vacuum environment, restoring the pressure to normal, heating the autoclave to 190-200° C., keeping the temperature for 4-5 hours, cooling the autoclave to room temperature, separating the solid matter, washing the solid matter, and drying the solid matter to obtain the primary composite fiber; The method for preparing the secondary composite fiber comprises: mixing anhydrous ethanol and hydrogen peroxide evenly, then adding zirconium oxychloride octahydrate and acetylacetone in sequence, mixing evenly, and obtaining a sol treatment solution; adding the primary composite fiber into the sol treatment solution, immersing, separating out solid matter, drying the solid matter at 80-85° C. to a constant weight, heating the solid matter to 800-820° C. in an argon atmosphere, and calcining the mixture at the same temperature to obtain the secondary composite fiber; The surface pre-modification method comprises the following steps: putting the secondary composite fiber into an ethanol solution, dispersing the fiber uniformly, heating the fiber to 42-48° C., and keeping the temperature; dripping γ-glycidyloxypropyltriethoxysilane with stirring, and after the dripping is completed, continuing to keep the temperature and stirring, separating the solid matter, washing the solid matter, and drying the solid matter to obtain the pre-modified fiber; The hyperbranched modification method comprises the following steps: putting the pre-modified fiber into anhydrous ethanol, uniformly dispersing the fiber, stirring and heating the fiber to 55-60° C., and dripping a hyperbranched modification liquid under the condition of heat preservation, reflux and stirring; after the hyperbranched modification liquid is dripped, the fiber is kept warm, refluxed and stirred, and solids are separated; the solids are washed and dried to obtain hyperbranched modified fibers; The preparation method of the hyperbranched modified liquid comprises the following steps: adding triethylenetetramine to anhydrous ethanol, cooling to 0-2°C, keeping the temperature constant and stirring, and dropping an ethanol solution of methyl acrylate; after the dropwise addition is completed, keeping the temperature constant for reaction for 2.5-3h to obtain a reaction liquid; keeping the reaction liquid in a vacuum environment of 0.02-0.03MPa for 60-65°C and then keeping the temperature constant at 120-125°C to obtain a hyperbranched modified liquid; The mixed material sintering method comprises the following steps: uniformly mixing alumina powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and hyperbranched modified fibers, and then dry-pressing the mixture to obtain a green body; and sintering the green body at 1300-1350° C. to obtain a composite fiber-reinforced refractory material.
2. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the primary composite fiber, the glucose concentration in the glucose treatment solution is 14-17wt%; the pH of the glucose treatment solution is 1.5-2; The weight ratio of the polycrystalline alumina fiber to the glucose treatment solution is 1:80-85; The alumina content of the polycrystalline alumina fiber is 86-90wt%, the fiber diameter is 3-4μm, and the fiber length is 55-70mm.
3. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the composite fiber, the standing time in the vacuum environment is 1-2 hours, and the vacuum degree is 0.08-0.09 MPa; The heating rate to 190-200°C is 2-2.5°C / min.
4. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the secondary composite fiber, the mass concentration of hydrogen peroxide is 23-24wt%; The weight ratio of anhydrous ethanol to hydrogen peroxide is 14-15:100; In the sol treatment liquid, the molar ratio of hydrogen peroxide, zirconium oxychloride octahydrate and acetylacetone is 5.8-6.1:1:0.3-0.
35.
5. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the secondary composite fiber, the weight ratio of the primary composite fiber to the sol treatment liquid is 1:55-60; The heating rate to 800-820°C is 3-4°C / min; The calcination time at 800-820℃ is 2-3h.
6. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the surface pre-modification, the volume concentration of the ethanol solution is 80-85%; The heat preservation and stirring time after the addition of γ-glycidyloxypropyltriethoxysilane is completed is 4-5 hours; The weight ratio of the secondary composite fiber, the ethanol solution and the gamma-glycidyloxypropyltriethoxysilane is 12.5-13:200:3.5-4.
7. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the hyperbranched modification, the heat preservation and reflux stirring time after the hyperbranched modification liquid is added is 2-3 hours; The weight ratio of the pre-modified fiber, anhydrous ethanol and hyperbranched modified liquid is 29-30:300:16-16.
5.
8. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the hyperbranched modified liquid, the weight ratio of triethylenetetramine to anhydrous ethanol is 1:1.2-1.3; The drop rate of the ethanol solution of methyl acrylate is 0.8-1.2 mL / min; The insulation time at 60-65℃ is 60-80min, and the insulation time at 120-125℃ is 2-2.5h.
9. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: In the preparation of the hyperbranched modified liquid, the concentration of methyl acrylate in the ethanol solution of methyl acrylate is 40-42wt%; The molar ratio of methyl acrylate to triethylenetetramine is 1:1.02-1.
05.
10. The method for preparing a composite fiber-reinforced refractory material according to claim 1, characterized in that: During the mixed material sintering, the dry pressing pressure is 15-18 MPa; The sintering time at 1300-1350℃ is 2-3h; The weight ratio of aluminum oxide powder, silicon oxide powder, calcium oxide, magnesium oxide, titanium oxide, carboxymethyl cellulose and hyperbranched modified fiber is 68-70:28-31:7-8:7-8:3-3.5:2-2.5:12-13.
Citation Information
Patent Citations
Modified fiber refractory material and preparation method thereof
CN104961477A
High-toughness ceramic composite material and preparing method thereof
CN106587981A
Method for preparing fiber reinforced multiphase ceramic matrix composite material
CN108395266A
Preparation process of low-thermal-expansion composite material
CN113372107A
Coating reinforcing material for ceramic composites
DE19743723A1