A method for preparing porous ceramics with controllable pore size and porosity
By combining nano-carbon fibers and alumina aerogel fibers, using silane coupling agents and asphalt, the problems of inappropriate pore size and insufficient strength of porous ceramic materials are solved, and the controllability of pore size and porosity is achieved, and the ceramics are improved. Mechanical properties and sintering effect.
Patent Information
- Application Number
- CN202411186413.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
During the filtration process, existing porous ceramic materials have low capture efficiency, easy blockage, and insufficient strength, which makes them difficult to meet the actual application needs.
Nanocarbon fiber and alumina aerogel fiber are combined, and a uniform and refined matrix structure is formed through multiple mechanical grinding and wet grinding. Hydrogen bonding is formed by using silane coupling agent and polyvinyl alcohol, and asphalt and alkaline magnesium carbonate are added. To optimize the mechanical properties of the ceramics, and to control pore size and porosity through phased heating and spray drying tower granulation.
It improves the internal strength and mechanical properties of the ceramic, realizes controllable pore size and porosity, enhances the flexural strength and sintering effect of the ceramic, and reduces costs.
Smart Images

Figure CN118684516B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alumina ceramics, and in particular to a method for preparing porous ceramics with controllable pore size and porosity. Background Art
[0002] Porous ceramic materials are widely used in chemical, environmental protection, biological, energy, food and medicine fields due to their low density, large specific surface area, low thermal conductivity, good permeability, high temperature resistance, corrosion resistance, wear resistance and other characteristics. They can be used as materials for filtration separation, heat insulation, sound absorption, bioceramics, catalyst carriers, etc. At present, the methods for preparing porous ceramics include adding pore-forming agents, chemical foaming, extrusion molding and sol-gel method. The prepared porous ceramics have good functionality, but their strength drops sharply due to the increase in porosity.
[0003] In actual application, especially in the filtration direction, the pore size of the ceramic plays a decisive role in the filtration direction. If the pore size is too large, the capture and filtration efficiency will be reduced, making it difficult to achieve the purpose of interception; if the pore size is too small, it is easy to cause blockage and reduce the filtration efficiency. When the ceramic body is full of filtered material, it needs to be regenerated, which greatly increases the cost. Therefore, in practical applications, it is necessary to prepare porous ceramic matrix materials with appropriate pore sizes according to actual conditions. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing porous ceramics with controllable pore size and porosity, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing porous ceramics with controllable pore size and porosity, comprising the following preparation steps:
[0006] (1) Nanocarbon fibers and anhydrous ethanol are ultrasonically treated at 20 kHz for 20 minutes, and aluminum sec-butoxide, deionized water at 60° C., and ethyl acetoacetate are added, and stirred at 60-80 rpm for 10-30 minutes to obtain aluminum sol; the content of the nanocarbon fibers in the aluminum sol is 1-10 wt%;
[0007] (2) Aluminum sol and polyvinyl alcohol aqueous solution were mixed in a mass ratio of 9:1, stirred at 85°C and 100 rpm for 30 min, cooled to room temperature while stirring, and continued to stir at room temperature for 24 h to obtain a spinning solution, which was spun into an ethanol-liquid nitrogen bath at -100~-30°C, and the fiber was taken out and then frozen at -65°C and a pressure of 4 Pa for 24 h, and high-temperature resistant alumina aerogel fibers with a length of 0.1~0.5 mm were sheared;
[0008] (3) 65-75 parts by weight of aluminum oxide, 1-5 parts by weight of calcined bauxite, 5-10 parts by weight of asphalt, 10-15 parts by weight of silicon carbide, 18-28 parts by weight of a sintering aid, and 0.9-1.4 parts by weight of magnesium fluoride are mixed, zirconium oxide grinding balls are added at a ball-to-material ratio of 5:1, the ball milling speed is 100-250 rpm, the ball milling time is 3-6 hours, 5-15 wt% of the total mass of a silane coupling agent is added, the ball-to-material ratio is maintained at 5:1, and the mixture is ball-milled at 300 rpm for 20 minutes and at 600 rpm for 40 minutes to obtain a ceramic raw material; the borax and basic magnesium carbonate in the sintering aid are mixed at a boron:magnesium molar ratio of 1.5:1;
[0009] (4) Take 55-74 parts by weight of ceramic raw materials, add them into a ball mill according to a mass ratio of 1:1:1 with deionized water and zirconium oxide grinding balls, the ball mill speed is 100-250r / min, the ball mill time is 3-6h, and then pour it into a low-speed stirring tank, add 20-40 parts by weight of pore-forming agent, 5-10 parts by weight of binder, and 8-20 parts by weight of high-temperature resistant alumina aerogel fiber, stir at 100-300rpm for 1-3h, send the material into a spray drying tower for granulation, the air inlet temperature in the drying tower is 200-300℃, and the air outlet temperature is 100-150℃, the collected powder is sieved through an 80-mesh sieve, filled into a mold, and then put into a cold isostatic press, the isostatic pressing pressure is 80-200MPa, and a green body is obtained;
[0010] (5) The green body is sintered in an atmospheric furnace, first heated to 200-300°C, kept warm for 30 minutes, then heated to 600°C, kept warm for 5-10 hours, then heated to 800-1000°C, kept warm for 1 hour, and finally heated to 1300-1500°C, kept warm for 1-3 hours to obtain porous ceramics with controllable pore size and porosity.
[0011] Furthermore, the particle size of the nano-carbon fiber in step (1) is 50-100 nm.
[0012] Furthermore, in step (1), the molar ratio of aluminum sec-butoxide, anhydrous ethanol, deionized water, and ethyl acetoacetate is 1:4-16:1.2-2:0.01-0.1.
[0013] Furthermore, the concentration of the polyvinyl alcohol aqueous solution in step (2) is 15 mg / mL.
[0014] Furthermore, in step (2), the volume ratio of ethanol to liquid nitrogen in the ethanol-liquid nitrogen bath is 1-6:1-5.
[0015] Furthermore, the spinning conditions in step (2) are as follows: the discharge speed of the spinning solution is 1-5 m / min, and the size of the spinning needle is 10-200 μm.
[0016] Furthermore, the asphalt in step (3) is coal tar, which is a material produced during the coking process of coal and has a softening point in the range of 60-120°C.
[0017] Furthermore, the silane coupling agent in step (3) is a mixture of KH-540 and 3-aminopropyltriethoxysilane in a mass ratio of 1:1.
[0018] Furthermore, the pore-forming agent in step (4) is spherical graphite carbon powder with a particle size of 15-50 μm.
[0019] Furthermore, the adhesive in step (4) is polyvinyl alcohol.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0021] (1) The present invention first preliminarily mixes alumina, calcined bauxite, asphalt, and sintering aids and mechanically grinds them to break and refine the particles, so that a uniform and refined matrix structure can be formed in the subsequent sintering process; then, a coupling agent is added and a secondary grinding is performed, and the above substances are modified by a silane coupling agent so that they can form hydrogen bonds with the polyvinyl alcohol binder, thereby building molecular bridges between the powders, greatly improving the bonding effect, thereby improving the internal strength of the ceramic and optimizing the mechanical properties of the ceramic; then, high-temperature resistant alumina aerogel fibers, polyvinyl alcohol, porogens, and solvents are added, and a third wet grinding is performed to obtain a ceramic slurry. The high-temperature resistance of the alumina aerogel allows the fibrous structure to be maintained in the subsequent high-temperature sintering process, thereby playing a long-term skeleton role and improving the strength of the ceramic;
[0022] (2) The present invention uses borax and basic magnesium carbonate as sintering aids for ceramics, which can react with the alumina base material in the ceramics to form a liquid phase, greatly improving the diffusion capacity of ions, accelerating the reaction process, promoting the formation of crystal nuclei and the growth process of crystals, so that the ceramics can be fully sintered at a relatively low temperature, and at the same time, they are well embedded in the surface layer of the aerogel, thereby enhancing the bonding strength and improving the mechanical properties of the ceramics. At the same time, the present invention adopts a staged heating treatment to prepare the ceramics, and controls the amount of borax and basic magnesium carbonate, so that part of the borax and basic magnesium carbonate first generate magnesium borate whiskers in situ, thereby enhancing the internal strength of the ceramics. In addition, the gas released by the thermal decomposition of basic magnesium carbonate forms a certain initial pore inside the ceramics;
[0023] (3) The present invention adds asphalt. During the staged sintering process, the asphalt is preferentially melted into a liquid state to bond the aerogel fibers. The asphalt is adsorbed and supported by the aerogel to prevent the molten asphalt from gathering at the bottom of the ceramic due to gravity and affecting subsequent treatment. Then, as the temperature rises, whiskers are generated inside the ceramic. The asphalt bonds to the surrounding whiskers. As the temperature further rises, the asphalt is gradually carbonized to form carbon fixed points, which then bridge the aerogel fibers and whiskers to form a micro-skeleton inside the ceramic. The internal structure has strong support. In addition, during the sintering process of the ceramic, the volatile components of the asphalt escape, thereby regulating the porosity of the ceramic. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0025] Figure 1 It is the microscopic morphology of the porous ceramic of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Example 1; (1) Aluminum sec-butoxide, deionized water at 60°C and ethyl acetoacetate were added to nano-carbon fibers with a particle size of 80 nm and anhydrous ethanol at 20 kHz for 20 min, and the mixture was stirred at 70 rpm for 20 min to obtain aluminum sol; the content of the nano-carbon fibers in the aluminum sol was 8 wt %; the molar ratio of the aluminum sec-butoxide, anhydrous ethanol, deionized water and ethyl acetoacetate was 1:10:1.8:0.06;
[0028] (2) Aluminum sol and polyvinyl alcohol aqueous solution with a concentration of 15 mg / mL were mixed in a mass ratio of 9:1, stirred at 85°C and 100 rpm for 30 min, cooled to room temperature while stirring, and continued to stir at room temperature for 24 h to obtain a spinning solution, which was spun into an ethanol-liquid nitrogen bath at -65°C. The volume ratio of ethanol to liquid nitrogen in the ethanol-liquid nitrogen bath was 6:5, the discharge speed of the spinning solution was 3 m / min, the spinning needle size was 100 μm, the fiber was taken out, and then frozen at -65°C and a pressure of 4 Pa for 24 h, and high-temperature resistant alumina aerogel fibers with a length of 0.3 mm were obtained by shearing;
[0029] (3) 70 parts by weight of aluminum oxide, 3 parts by weight of calcined bauxite, 7 parts by weight of asphalt, 12 parts by weight of silicon carbide, 23 parts by weight of a sintering aid, and 1.1 parts by weight of magnesium fluoride are mixed, zirconium oxide grinding balls are added at a ball-to-material ratio of 5:1, the ball milling speed is 200 rpm, the ball milling time is 4.5 hours, 10 wt% of the total mass of a silane coupling agent is added, the ball-to-material ratio is maintained at 5:1, and the ball milling is performed at 300 rpm for 20 minutes and at 600 rpm for 40 minutes to obtain a ceramic raw material; the silane coupling agent is KH-540 and 3-aminopropyltriethoxysilane mixed at a mass ratio of 1:1; the borax and basic magnesium carbonate in the sintering aid are mixed at a boron:magnesium molar ratio of 1.5:1;
[0030] (4) Take 60 parts by weight of ceramic raw materials, add them into a ball mill with deionized water and zirconium oxide grinding balls in a mass ratio of 1:1:1, the ball mill speed is 200 r / min, the ball milling time is 4.5 h, and then pour it into a low-speed stirring tank, add 20 parts by weight of 15 μm spherical graphite carbon powder, 7 parts by weight of polyvinyl alcohol, and 14 parts by weight of high-temperature resistant alumina aerogel fiber, stir at 200 rpm for 2 h, send the material into a spray drying tower for granulation, the air inlet temperature in the drying tower is 300 ° C, and the air outlet temperature is 150 ° C. After the collected powder is sieved through an 80-mesh sieve, it is filled into a mold and then put into a cold isostatic press with an isostatic pressing pressure of 140 MPa to obtain a green body;
[0031] (5) The green body is sintered in an atmospheric furnace by first heating the temperature to 250°C and keeping it at that temperature for 30 minutes, then heating the temperature to 600°C and keeping it at that temperature for 7 hours, then heating the temperature to 900°C and keeping it at that temperature for 1 hour, and finally heating the temperature to 1400°C and keeping it at that temperature for 2 hours to obtain porous ceramics with controllable pore size and porosity.
[0032] Example 2: The only difference between Example 2 and Example 1 is that the particle size of the spherical graphite carbon powder is 50 μm, and the remaining steps are the same as Example 1.
[0033] Example 3; The only difference between Example 3 and Example 1 is that the mass fraction of spherical graphite carbon powder is 27.5, and the remaining steps are the same as Example 1.
[0034] Example 4; The only difference between Example 4 and Example 1 is that the mass fraction of the spherical graphite carbon powder is 27.5 and the particle size is 50μm, and the remaining steps are the same as Example 1.
[0035] Example 5; The only difference between Example 5 and Example 1 is that the mass fraction of spherical graphite carbon powder is 35, and the remaining steps are the same as Example 1.
[0036] Example 6: The only difference between Example 6 and Example 1 is that the mass fraction of the spherical graphite carbon powder is 35 and the particle size is 50μm, and the remaining steps are the same as Example 1.
[0037] Comparative Example 1: The only difference between Comparative Example 1 and Example 1 is that no aerogel fiber is added, and the remaining steps are the same as Example 1.
[0038] Comparative Example 2: The only difference between Comparative Example 2 and Example 1 is that borax is not added, and the remaining steps are the same as Example 1.
[0039] Comparative Example 3: The difference between Comparative Example 3 and Example 1 is that basic magnesium carbonate is not added, and the remaining steps are the same as Example 1.
[0040] Comparative Example 4: The only difference between Comparative Example 4 and Example 1 is that no asphalt is added, and the remaining steps are the same as Example 1.
[0041] Comparative Example 5: The difference between Comparative Example 5 and Example 1 is only the difference in step (5). Step (5) is changed to: sintering the green body in an atmospheric furnace and keeping it at 1400°C for 7h to obtain a porous ceramic with controllable pore size and porosity.
[0042] Comparative Example 6: The difference between Comparative Example 6 and Example 1 is that step (3) is different. Step (3) is changed to: 70 parts by mass of aluminum oxide, 3 parts by mass of calcined bauxite, 7 parts by mass of asphalt, 12 parts by mass of silicon carbide, 23 parts by mass of sintering aid, and 1.1 parts by mass of magnesium fluoride are mixed, and zirconium oxide grinding balls are added at a ball-to-material ratio of 5:1. The ball milling speed is 200 rpm and the ball milling time is 4.5 h to obtain a ceramic raw material; the borax and basic magnesium carbonate in the sintering aid are mixed at a boron:magnesium molar ratio of 1.5:1. The remaining steps are the same as in Example 1.
[0043] Comparative Example 7; The difference between Comparative Example 7 and Example 1 is that there is no step (3), and step (4) is changed to: 70 parts by weight of aluminum oxide, 3 parts by weight of calcined bauxite, 7 parts by weight of asphalt, 12 parts by weight of silicon carbide, 23 parts by weight of sintering aid, and 1.1 parts by weight of magnesium fluoride are mixed, and then 10wt% of the total weight of silane coupling agent is added to obtain a ceramic raw material; 60 parts by weight of the ceramic raw material is taken, and deionized water and zirconium oxide grinding balls are added to a ball mill in a mass ratio of 1:1:1, the ball mill speed is 200r / min, the ball milling time is 4.5h, and then poured into a low-speed stirring tank, and added 20 parts by mass of spherical graphite powder with a particle size of 15 μm, 7 parts by mass of polyvinyl alcohol, and 14 parts by mass of high-temperature resistant alumina aerogel fiber are stirred at 200 rpm for 2 hours, and the materials are sent to a spray drying tower for granulation. The air inlet temperature in the drying tower is 300°C, and the air outlet temperature is 150°C. The collected powder is passed through an 80-mesh sieve, filled into a mold, and then put into a cold isostatic press with an isostatic pressing pressure of 140 MPa to obtain a green body; the silane coupling agent is KH-540 and 3-aminopropyltriethoxysilane mixed in a mass ratio of 1:1; the borax and basic magnesium carbonate in the sintering aid are mixed in a boron:magnesium molar ratio of 1.5:1.
[0044] Effect example
[0045] The following Table 1 shows the performance analysis results of the ceramics using Examples 1 to 6 of the present invention; the following Table 2 shows the performance analysis results of the ceramics using Example 1 of the present invention and Comparative Examples 1 to 7.
[0046] Table 1
[0047] Examples 1-6 show the porosity, average pore size, density and flexural strength of porous ceramic materials with different particle sizes and addition amounts of pore formers. The internal porosity and pore size of porous ceramics are effectively controlled by adjusting the addition amount of pore formers and the particle size of pore formers. As the addition amount of pore formers and the particle size of pore formers increase, the density and flexural strength of porous ceramics decrease. The flexural strength of porous ceramic materials in each embodiment of the present invention is at a relatively high level.
[0048] Table 2
[0049] By comparing the experimental data of Example 1 with that of Comparative Example 1, it can be found that the porous structure of the aerogel fiber itself can increase the number of pores in the porous ceramic, and at the same time form a micro-skeleton effect with the internal whiskers to support the interior of the ceramic and enhance the pore strength, thereby improving the strength of the ceramic; by comparing the experimental data of Example 1 with those of Comparative Examples 2 and 3, it can be found that the presence of borax and basic magnesium carbonate can achieve sufficient sintering of the ceramic, optimize the porosity and strength of the ceramic, and some raw materials can generate whiskers in situ, which work together with the aerogel fibers to enhance the strength of the ceramic. At the same time, the gas released by the thermal decomposition of basic magnesium carbonate can work together with the porogen to ensure the strength while maximizing the porosity; from the comparison of the experimental data of Example 1 with that of Comparative Example 4, it can be found that the addition of asphalt can replace polyvinyl alcohol in During the later sintering process, the bonding effect is exerted to achieve the connection between the fibers and whiskers, thereby improving the strength of the ceramic. At the same time, during the later sintering process, solid carbon is formed to further enhance the strength of the ceramic. From the comparison of the experimental data of Example 1 and Comparative Example 5, it can be found that the staged heating adopted by the present invention is conducive to the mutual combination reaction between substances, improves the strength of the ceramic, and optimizes the porosity. From the comparison of the experimental data of Example 1 and Comparative Example 6, it can be found that the coupling agent participates in the grinding, thereby modifying the powder and building molecular bridges between the powders, which greatly improves the bonding effect and thereby improves the internal strength of the ceramic. From the comparison of the experimental data of Example 1 and Comparative Example 7, it can be found that through the two initial mechanical grindings, a uniform and refined matrix structure can be formed, and at the same time, the bonding effect is greatly improved, thereby improving the internal strength of the ceramic.
[0050] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing porous ceramics with controllable pore size and porosity, characterized in that: The method comprises the following preparation steps: (1) Nanocarbon fibers and anhydrous ethanol are ultrasonically treated at 20 kHz for 20 minutes, and aluminum sec-butoxide, deionized water at 60° C., and ethyl acetoacetate are added, and stirred at 60-80 rpm for 10-30 minutes to obtain aluminum sol; the content of the nanocarbon fibers in the aluminum sol is 1-10 wt%; (2) Aluminum sol and polyvinyl alcohol aqueous solution were mixed in a mass ratio of 9:1, stirred at 85°C and 100 rpm for 30 min, cooled to room temperature while stirring, and continued to stir at room temperature for 24 h to obtain a spinning solution, which was spun into an ethanol-liquid nitrogen bath at -100~-30°C, and the fiber was taken out and then frozen at -65°C and a pressure of 4 Pa for 24 h, and high-temperature resistant alumina aerogel fibers with a length of 0.1~0.5 mm were sheared; (3) 65-75 parts by weight of aluminum oxide, 1-5 parts by weight of calcined bauxite, 5-10 parts by weight of asphalt, 10-15 parts by weight of silicon carbide, 18-28 parts by weight of a sintering aid, and 0.9-1.4 parts by weight of magnesium fluoride are mixed, zirconium oxide grinding balls are added at a ball-to-material ratio of 5:1, the ball milling speed is 100-250 rpm, the ball milling time is 3-6 hours, 5-15 wt% of the total mass of a silane coupling agent is added, the ball-to-material ratio is maintained at 5:1, and the mixture is ball-milled at 300 rpm for 20 minutes and at 600 rpm for 40 minutes to obtain a ceramic raw material; the borax and basic magnesium carbonate in the sintering aid are mixed at a boron:magnesium molar ratio of 1.5:1; (4) Take 55-74 parts by weight of ceramic raw materials, add them into a ball mill according to a mass ratio of 1:1:1 with deionized water and zirconium oxide grinding balls, the ball mill speed is 100-250r / min, the ball mill time is 3-6h, and then pour it into a low-speed stirring tank, add 20-40 parts by weight of pore-forming agent, 5-10 parts by weight of binder, and 8-20 parts by weight of high-temperature resistant alumina aerogel fiber, stir at 100-300rpm for 1-3h, send the material into a spray drying tower for granulation, the air inlet temperature in the drying tower is 200-300℃, and the air outlet temperature is 100-150℃, the collected powder is sieved through an 80-mesh sieve, filled into a mold, and then put into a cold isostatic press, the isostatic pressing pressure is 80-200MPa, and a green body is obtained; (5) The green body is sintered in an atmospheric furnace, first heated to 200-300°C, kept warm for 30 minutes, then heated to 600°C, kept warm for 5-10 hours, then heated to 800-1000°C, kept warm for 1 hour, and finally heated to 1300-1500°C, kept warm for 1-3 hours to obtain porous ceramics with controllable pore size and porosity.
2. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The particle size of the nano carbon fiber in step (1) is 50-100 nm.
3. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The molar ratio of aluminum sec-butoxide, anhydrous ethanol, deionized water and ethyl acetoacetate in step (1) is 1:4-16:1.2-2:0.01-0.
1.
4. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The concentration of the polyvinyl alcohol aqueous solution in step (2) is 15 mg / mL.
5. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The volume ratio of ethanol to liquid nitrogen in the ethanol-liquid nitrogen bath in step (2) is 1-6:1-5.
6. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The spinning conditions in step (2) are as follows: the discharge speed of the spinning solution is 1-5 m / min, and the spinning needle size is 10-200 μm.
7. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The asphalt in step (3) is coal tar, which is a material produced during the coking process of coal and has a softening point in the range of 60-120°C.
8. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The silane coupling agent in step (3) is a mixture of KH-540 and 3-aminopropyltriethoxysilane in a mass ratio of 1:
1.
9. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The pore-forming agent in step (4) is spherical graphite carbon powder with a particle size of 15-50 μm.
10. The method for preparing a porous ceramic with controllable pore size and porosity according to claim 1, characterized in that: The binder in step (4) is polyvinyl alcohol.