A wear-resistant and impact-resistant polyurethane material and preparation method thereof
By modifying the preparation method of polyurethane materials, Si-O bonds, CF bonds and DOPO structures are introduced to form a thermally reversible cross-linked network, which solves the problem of easy damage and aging of polyurethane materials in air-dropped water bladders, improves the wear resistance and stability of the materials, and makes them suitable for disaster relief and field operations.
Patent Information
- Application Number
- CN202411180863.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing polyurethane materials are easily damaged by dragging and friction in air-dropped water bladders, and are prone to aging in the field, affecting the normal conduct of disaster relief and field operations.
Polyurethane was prepared by polymerizing polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2,4-diisocyanobenzene, and then mixed with modified nano-silica and molded to form a wear-resistant and impact-resistant polyurethane material. Modifications such as Si-O bonds, CF bonds, DOPO structure and sulfonium salt were introduced to form a thermally reversible crosslinked network.
The wear resistance, flame retardancy, antibacterial properties, hydrophobicity, and anti-aging properties of polyurethane materials have been improved, enhancing the durability and stability of water bladders and making them suitable for complex outdoor environments.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a wear-resistant and impact-resistant polyurethane material and a preparation method thereof. Background Art
[0002] Polyurethane, whose full name is polyurethane, is a polymer material formed by polycondensation reaction of polyols and polyisocyanates. It is widely used in textiles, construction, aviation, transportation, medicine, electronics and other fields, and is also one of the important materials for preparing protective layers of airdrop water bags. Airdrop water bags are mainly used for storage and transportation of water in disaster relief and rescue, and can also be used as water replenishment equipment for individual field operations. Since the use environment of airdrop water bags is usually in the field with complex terrain, the water bags will be repeatedly dragged and rubbed when airdropped to the ground, which can easily cause the water bags to break, which will seriously affect the normal progress of emergency rescue and field operations; at the same time, the sun and rain in the field will also aggravate the aging of the polyurethane protective layer on the surface of the water bag. Therefore, it is necessary to invent a polyurethane material with excellent wear resistance and aging resistance, which is used to prepare the protective layer of the water bag, improve the wear resistance and aging resistance of the water bag, and provide protection for emergency rescue and field operations, which has important practical significance and broad market prospects. Summary of the invention
[0003] The purpose of the present invention is to provide a wear-resistant and impact-resistant polyurethane material and a preparation method thereof, so as to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A wear-resistant and impact-resistant polyurethane material is prepared by polymerizing polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2,4-diisocyanobenzene to obtain polyurethane; reacting polyurethane and 4-(3-aminopropyl)-2,6-di-tert-butylphenol to obtain modified polyurethane; reacting pre-modified nano-silica and 2-bromomethylfuran to obtain modified nano-silica; uniformly mixing the modified polyurethane and the modified nano-silica, and performing compression molding to obtain the wear-resistant and impact-resistant polyurethane material;
[0006] The functionalized siloxane oligomer is prepared by ring-opening polymerization of functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane and end-capping with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane;
[0007] The functionalized cyclotetrasiloxane is prepared by reacting heptamethylcyclotetrasiloxane and N-allylmaleimide;
[0008] The pre-modified nano-silica is prepared by polymerizing aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid on pre-treated nano-silica.
[0009] The pretreated nano silicon dioxide is prepared by reacting nano silicon dioxide and aminopropyltriethoxysilane.
[0010] A method for preparing a wear-resistant and impact-resistant polyurethane material, the method for preparing a wear-resistant and impact-resistant polyurethane material comprising the following preparation steps:
[0011] (1) Functionalized cyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide and toluene are mixed in a mass ratio of 1:(0.6~0.8):(0.01~0.03):(0.01~0.03):(10~12), stirred at 65~75℃, 300~500r / min for 30~40min, added a capping agent of 0.2~0.3 times the mass of the functionalized cyclotetrasiloxane, continued to stir and react for 18~22min, cooled to 40~50℃ and continued to stir for 8~10min, cooled to room temperature, washed with an equal volume of deionized water and toluene, allowed to stand for stratification, removed the aqueous phase, repeated washing 3~5 times, took the organic phase and placed it in a drying oven, dried at 50~60℃ under vacuum conditions for 8~10h to obtain a functionalized siloxane oligomer;
[0012] (2) Mix polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and N,N-dimethylformamide in a mass ratio of 1:(0.6~0.8):(0.3~0.5):(20~30) and stir at 50~60°C and 300~500r / min for 20~30min. Add 1-chloromethyl-2,4-diisocyanobenzene (2.3~2.5 times the mass of polyether polyol) and dibutyltin dilaurate (0.04~0.06 times the mass of polyether polyol). Continue stirring and reacting for 9~11min and raise the temperature to 88~92℃, continue stirring to react for 4~5h, dry at 50~60℃ under vacuum conditions for 8~10h to obtain polyurethane; mix polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine, and N,N-dimethylformamide in a mass ratio of 1:(0.6~0.8):(0.03~0.05):(10~12) evenly, stir at 50~60℃, 300~500r / min to react for 2~3h, and dry at 50~60℃ under vacuum conditions for 8~10h to obtain modified polyurethane;
[0013] (3) Add aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid in a molar ratio of 1:(0.8-0.9) to N,N-dimethylformamide (20-30 times the mass of aminoethyl sulfide), add pretreated nano-silica (0.6-0.8 times the mass of aminoethyl sulfide), add dicyclohexylcarbodiimide (0.03-0.05 times the mass of aminoethyl sulfide), and stir at 70-80°C and 300-500 r / min to react. The pre-modified nano-silica was prepared by mixing the pre-modified nano-silica, 2-bromomethylfuran and tetrahydrofuran in a mass ratio of 1:(2-3):(10-12), stirring at 10-30°C and 300-500r / min for 20-24h, filtering, washing with ether for 3-5 times, and drying at 50-60°C for 8-10h under vacuum conditions to obtain modified nano-silica.
[0014] (4) The modified polyurethane and modified nano-silica are mixed evenly in a mass ratio of 1:(0.03-0.05), placed in an internal mixer, stirred at 190-200°C for 10-12 minutes, poured into a mold, and compression molded to obtain a wear-resistant and impact-resistant polyurethane material.
[0015] As an optimization, the preparation method of the functionalized cyclotetrasiloxane in step (1) is as follows: heptamethylcyclotetrasiloxane and N-allylmaleimide are added in a molar ratio of 1:1 to toluene with a mass of 8 to 10 times that of heptamethylcyclotetrasiloxane, and 0.03 to 0.05 times that of heptamethylcyclotetrasiloxane is added with chloroplatinic acid, and the mixture is stirred at 70 to 80°C and 300 to 500 r / min for 3 to 4 hours, and dried at 50 to 60°C under vacuum conditions for 7 to 9 hours to obtain the functionalized cyclotetrasiloxane.
[0016] As an optimization, the capping agent in step (1) is 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane.
[0017] As an optimization, the model of the polyether polyol in step (2) is HSH-240.
[0018] As an optimization, the preparation method of the pretreated nano-silica in step (3) is: nano-silica and anhydrous ethanol are mixed evenly in a mass ratio of 1:(50~60), silane hydrolyzate is added in an amount of 8~10 times the mass of the nano-silica, the mixture is stirred at 50~60°C and 300~500r / min for 2~3h, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 50~60°C under vacuum conditions for 8~10h to obtain the pretreated nano-silica.
[0019] As an optimization, the preparation method of the silane hydrolyzate is: aminopropyltriethoxysilane and anhydrous ethanol are mixed evenly in a mass ratio of 1:(20~30), the pH is adjusted to 4~6 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 10~30°C and 300~500r / min for 50~60min to prepare a silane hydrolyzate.
[0020] As an optimization, the process parameters of the compression molding in step (4) are: at 190-200°C, 2-3 MPa, holding pressure for 6-8 min, keeping the pressure constant, cooling to 90-100°C and keeping it warm for 2-3 h, and naturally cooling to room temperature before demolding and taking it out.
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0022] When preparing the wear-resistant and impact-resistant polyurethane material, the present invention comprises the following steps: reacting heptamethylcyclotetrasiloxane and N-allylmaleimide to obtain functionalized cyclotetrasiloxane; ring-opening polymerization of functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane and end-capping with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to obtain functionalized siloxane oligomer; polymerizing polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2,4-diisocyanobenzene to obtain polyurethane; and polymerizing polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butyl The modified polyurethane is prepared by reacting phenol; nano-silica and aminopropyltriethoxysilane are reacted to prepare pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid are polymerized and grown on the pretreated nano-silica to prepare pre-modified nano-silica; pre-modified nano-silica and 2-bromomethylfuran are reacted to prepare modified nano-silica; modified polyurethane and modified nano-silica are uniformly mixed and compression molded to prepare wear-resistant and impact-resistant polyurethane material.
[0023] First, the Si-H bond on heptamethylcyclotetrasiloxane is reacted with the carbon-carbon double bond on N-allylmaleimide to obtain functionalized cyclotetrasiloxane, and a maleimide group is introduced into the functionalized cyclotetrasiloxane; the functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane are ring-opened polymerized and end-capped with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to obtain a functionalized siloxane oligomer, and maleimide groups and CF bonds are introduced into the side chains of the functionalized siloxane oligomer molecules, and hydroxyl groups are introduced into both ends of the molecular chain. The maleimide groups introduced into the side chains can be The furan groups introduced on the modified nano-silica undergo a Diels-Alder addition reaction to form a thermoreversible cross-linking network, which inhibits the relative slip between the molecular chains and gives the wear-resistant and impact-resistant polyurethane material excellent self-healing and wear-resistant properties; the CF bond has a higher bond energy and lower polarizability. The matrix material containing the CF bond not only has a high repellency to aqueous substances, but also has a repellency to oily substances, which can give the wear-resistant and impact-resistant polyurethane material excellent hydrophobic and antifouling properties; the introduction of hydroxyl groups at both ends of the molecular chain can participate in the polymerization reaction of the polyurethane.
[0024] Secondly, polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2,4-diisocyanobenzene are polymerized to prepare polyurethane, Si-O bonds are introduced into the main chain of the polyurethane molecule, and chlorine atoms are introduced into the side chain; the bond energy of Si-O bonds is greater than that of CC bonds, so compared with CC bonds, Si-O bonds need to absorb more heat and their own vibration energy to resolve the energy of thermal decomposition of polymer materials, and the layered SiO2 formed by the degradation of siloxane during combustion migrates to the surface of the carbon layer, making the carbon layer denser and inhibiting The oxidation of the carbon layer enhances the stability of the carbon layer at high temperatures, giving the wear-resistant and impact-resistant polyurethane material excellent flame retardancy and high temperature resistance; the chlorine atoms introduced on the polyurethane side chain react with the amino groups on 4-(3-aminopropyl)-2,6-di-tert-butylphenol to obtain a modified polyurethane, and a hindered phenol structure is introduced on the modified polyurethane side chain. The hindered phenol structure can capture free radicals, terminate free radical chain reactions, and prevent free radical destructive effects in the polymer, thereby giving the wear-resistant and impact-resistant polyurethane material excellent anti-aging properties.
[0025] Finally, nano-silica and aminopropyltriethoxysilane are reacted to obtain pretreated nano-silica, and amino groups are introduced into the pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid are polymerized and grown on the pretreated nano-silica to obtain pre-modified nano-silica, and DOPO structure and sulfide are introduced into the pre-modified nano-silica. The DOPO structure has higher thermal stability and chemical stability than general, non-annular organic phosphates due to the presence of biphenyl ring and phenanthrene ring structure in the molecular structure, especially the side phosphorus group is introduced in the form of cyclic O=PO bond, and has better flame retardant properties, thus giving the wear-resistant and impact-resistant polyurethane material excellent flame retardant properties; the sulfide on the pre-modified nano-silica is reacted with the bromine atom on 2-bromomethylfuran to form a sulfonium salt to obtain modified nano-silica, and on the modified Sulfonium salt and furan groups are introduced into the modified nano-silica. Sulfonium salt is a cationic antibacterial structure, which can give the wear-resistant and impact-resistant polyurethane material excellent antibacterial properties; the furan group introduced on the modified nano-silica can undergo Diels-Alder addition reaction with the maleimide group introduced on the side chain of the modified polyurethane molecule to form a thermally reversible cross-linking network, inhibit the relative slip between the molecular chains, and give the wear-resistant and impact-resistant polyurethane material excellent self-healing properties and wear resistance; nano-silica has a high specific surface area and excellent mechanical properties, which can improve the strength and hardness of the matrix resin. The nano-silica is modified to increase the compatibility of the nano-silica with the matrix resin, reduce the agglomeration of the nano-silica, and make the nano-silica uniformly dispersed in the matrix resin, so as to give full play to the reinforcing effect of the nano-silica and further improve the wear resistance of the wear-resistant and impact-resistant polyurethane material. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1
[0027] A method for preparing a wear-resistant and impact-resistant polyurethane material, the method for preparing a wear-resistant and impact-resistant polyurethane material comprising the following preparation steps:
[0028] (1) Heptamethylcyclotetrasiloxane and N-allylmaleimide were added to toluene (8 times the mass of heptamethylcyclotetrasiloxane) in a molar ratio of 1:1, and chloroplatinic acid (0.03 times the mass of heptamethylcyclotetrasiloxane) was added, and the mixture was stirred at 70°C and 300 r / min for 4 h, and dried at 50°C under vacuum for 9 h to obtain functionalized cyclotetrasiloxane; functionalized cyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide, and toluene were added in a mass ratio of 1:0.6:0.01:0.0 1:10, mix evenly, react at 65°C, 300r / min with stirring for 40min, add 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane with a mass of 0.2 times that of the functionalized cyclotetrasiloxane, continue stirring and reacting for 22min, cool to 40°C and continue stirring for 10min, wash with a mixture of equal volumes of deionized water and toluene after cooling to room temperature, stand for stratification, remove the aqueous phase, repeat washing 3 times, take the organic phase and place it in a drying oven, dry it at 50°C for 10h under vacuum conditions to obtain a functionalized siloxane oligomer;
[0029] (2) Polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.6:0.3:20, stirred at 50°C and 300 r / min for 30 min, 1-chloromethyl-2,4-diisocyanobenzene (2.3 times the mass of polyether polyol) and dibutyltin dilaurate (0.04 times the mass of polyether polyol) were added, and the mixture was stirred for 11 min. The mixture was heated to 88°C and stirred for 5 h. The mixture was dried at 50°C for 10 h under vacuum to obtain polyurethane. Polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.6:0.03:10, stirred at 50°C and 300 r / min for 3 h, and dried at 50°C for 10 h under vacuum to obtain modified polyurethane.
[0030] (3) Mix aminopropyltriethoxysilane and anhydrous ethanol at a mass ratio of 1:20, adjust the pH to 4 with a 1 mol / L oxalic acid aqueous solution, stir at 10°C, 300 r / min for 60 min to prepare a silane hydrolyzate; mix nano-silica and anhydrous ethanol at a mass ratio of 1:50, add silane hydrolyzate 8 times the mass of nano-silica, stir at 50°C, 300 r / min for 3 h, filter, wash with anhydrous ethanol 3 times, and dry at 50°C under vacuum for 10 h to prepare pretreated nano-silica; mix aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid by molar ratio; The pre-modified nano-silica was prepared by adding 2-bromomethylfuran and tetrahydrofuran in a mass ratio of 1:2:10 to N,N-dimethylformamide with a mass ratio of 20 times of aminoethyl sulfide, adding pre-treated nano-silica with a mass ratio of 0.6 times of aminoethyl sulfide, adding dicyclohexylcarbodiimide with a mass ratio of 0.03 times of aminoethyl sulfide, stirring and reacting at 70°C and 300 r / min for 6 hours, filtering, washing with deionized water for 3 times, and drying at 50°C for 8 hours under vacuum conditions to obtain pre-modified nano-silica; the pre-modified nano-silica, 2-bromomethylfuran and tetrahydrofuran were uniformly mixed in a mass ratio of 1:2:10, stirring and reacting at 10°C and 300 r / min for 24 hours, filtering, washing with ether for 3 times, and drying at 50°C for 10 hours under vacuum conditions to obtain modified nano-silica;
[0031] (4) The modified polyurethane and modified nano-silica were mixed evenly in a mass ratio of 1:0.03, placed in an internal mixer, stirred at 190°C for 12 min, poured into a mold, maintained at 190°C, 2 MPa for 8 min, kept the pressure constant, cooled to 90°C and kept warm for 3 h, naturally cooled to room temperature and then demolded to obtain a wear-resistant and impact-resistant polyurethane material. Example 2
[0032] A method for preparing a wear-resistant and impact-resistant polyurethane material, the method for preparing a wear-resistant and impact-resistant polyurethane material comprising the following preparation steps:
[0033] (1) Heptamethylcyclotetrasiloxane and N-allylmaleimide were added in a molar ratio of 1:1 to toluene (9 times the mass of heptamethylcyclotetrasiloxane), and 0.04 times the mass of heptamethylcyclotetrasiloxane was added with chloroplatinic acid, and the mixture was stirred at 75°C and 400 r / min for 3.5 h. The mixture was dried at 55°C under vacuum for 8 h to obtain functionalized cyclotetrasiloxane. Functionalized cyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide and toluene were added in a mass ratio of 1:0.7:0.02:0 .02:11 mixed evenly, stirred at 70°C, 400r / min for 35min, added 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane (0.25 times the mass of functionalized cyclotetrasiloxane), continued stirring for 20min, cooled to 45°C and continued stirring for 9min, washed with an equal volume of deionized water and toluene after cooling to room temperature, allowed to stand for stratification, removed the aqueous phase, repeated washing 4 times, took the organic phase and placed it in a drying oven, dried at 55°C for 9h under vacuum conditions to obtain a functionalized siloxane oligomer;
[0034] (2) Polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.7:0.4:25, stirred at 55°C and 400 r / min for 25 min, 1-chloromethyl-2,4-diisocyanobenzene (2.4 times the mass of polyether polyol) and dibutyltin dilaurate (0.05 times the mass of polyether polyol) were added, and the mixture was stirred for 10 min. The mixture was heated to 90°C and stirred for 4.5 h. The mixture was dried at 55°C under vacuum for 9 h to obtain polyurethane. Polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.7:0.04:11, stirred at 55°C and 400 r / min for 2.5 h, and dried at 55°C under vacuum for 9 h to obtain modified polyurethane.
[0035] (3) aminopropyltriethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:25, the pH was adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 20°C and 400 r / min for 55 min to prepare a silane hydrolyzate; nano-silica and anhydrous ethanol were mixed at a mass ratio of 1:55, 9 times the mass of the nano-silica was added with the silane hydrolyzate, and the mixture was stirred at 55°C and 400 r / min for 2.5 h, filtered, washed with anhydrous ethanol for 4 times, and dried at 55°C under vacuum for 9 h to prepare pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid were mixed at a molar ratio of 1:0.85 is added to N,N-dimethylformamide with a mass ratio of 25 times of aminoethyl sulfide, and pretreated nano-silica with a mass ratio of 0.7 times of aminoethyl sulfide is added, and dicyclohexylcarbodiimide with a mass ratio of 0.04 times of aminoethyl sulfide is added, and the mixture is stirred at 75°C and 400r / min for 5.5h, filtered, washed with deionized water 4 times, and dried at 55°C for 7.5h under vacuum conditions to obtain pre-modified nano-silica; pre-modified nano-silica, 2-bromomethylfuran, and tetrahydrofuran are mixed uniformly at a mass ratio of 1:2.5:11, stirred at 20°C and 400r / min for 22h, filtered, washed with ether 4 times, and dried at 55°C for 9h under vacuum conditions to obtain modified nano-silica;
[0036] (4) The modified polyurethane and modified nano-silica were mixed evenly in a mass ratio of 1:0.04, placed in an internal mixer, stirred at 195°C for 11 minutes, poured into a mold, and maintained at 195°C and 2.5 MPa for 7 minutes. The pressure was kept constant, cooled to 95°C and kept warm for 2.5 hours. After naturally cooling to room temperature, the mold was removed to obtain a wear-resistant and impact-resistant polyurethane material. Example 3
[0037] A method for preparing a wear-resistant and impact-resistant polyurethane material, the method for preparing a wear-resistant and impact-resistant polyurethane material comprising the following preparation steps:
[0038] (1) Heptamethylcyclotetrasiloxane and N-allylmaleimide were added in a molar ratio of 1:1 to toluene (10 times the mass of heptamethylcyclotetrasiloxane), and 0.05 times the mass of heptamethylcyclotetrasiloxane was added with chloroplatinic acid, and the mixture was stirred at 80°C and 500 r / min for 3 h. The mixture was dried at 60°C under vacuum for 7 h to obtain functionalized cyclotetrasiloxane. Functionalized cyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide and toluene were added in a mass ratio of 1:0.8:0.03:0 .03:12, mix evenly, react at 75°C, 500r / min, stirring for 30min, add 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane (0.3 times the mass of functionalized cyclotetrasiloxane), continue stirring for 18min, cool to 50°C and continue stirring for 8min, wash with an equal volume of deionized water and toluene after cooling to room temperature, stand for stratification, remove the aqueous phase, repeat washing 5 times, take the organic phase and place it in a drying oven, dry it at 60°C under vacuum for 8h to obtain functionalized siloxane oligomer;
[0039] (2) Polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.8:0.5:30, stirred at 60°C and 500 r / min for 20 min, 1-chloromethyl-2,4-diisocyanobenzene (2.5 times the mass of polyether polyol) and dibutyltin dilaurate (0.06 times the mass of polyether polyol) were added, and the mixture was stirred for 9 min. The mixture was heated to 92°C and stirred for 4 h. The mixture was dried at 60°C for 8 h under vacuum to obtain polyurethane. Polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.8:0.05:12, stirred at 60°C and 500 r / min for 2 h, and dried at 60°C for 8 h under vacuum to obtain modified polyurethane.
[0040] (3) Mix aminopropyltriethoxysilane and anhydrous ethanol at a mass ratio of 1:30, adjust the pH to 6 with 1 mol / L oxalic acid aqueous solution, stir at 30°C, 500 r / min for 50 min to prepare a silane hydrolyzate; mix nano-silica and anhydrous ethanol at a mass ratio of 1:60, add silane hydrolyzate 10 times the mass of nano-silica, stir at 60°C, 500 r / min for 2 h, filter, wash with anhydrous ethanol 5 times, and dry at 60°C under vacuum for 8 h to prepare pretreated nano-silica; massage aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid The pre-modified nano-silica was prepared by adding 2-bromomethylfuran and tetrahydrofuran in a mass ratio of 1:3:12 to N,N-dimethylformamide with a mass ratio of 30 times of aminoethyl sulfide, adding pre-treated nano-silica with a mass ratio of 0.8 times of aminoethyl sulfide, adding dicyclohexylcarbodiimide with a mass ratio of 0.05 times of aminoethyl sulfide, stirring and reacting at 80°C and 500r / min for 5h, filtering, washing with deionized water for 5 times, and drying at 60°C for 7h under vacuum conditions to obtain pre-modified nano-silica; pre-modified nano-silica, 2-bromomethylfuran and tetrahydrofuran were uniformly mixed in a mass ratio of 1:3:12, stirring and reacting at 30°C and 500r / min for 20h, filtering, washing with ether for 5 times, and drying at 60°C for 8h under vacuum conditions to obtain modified nano-silica;
[0041] (4) The modified polyurethane and modified nano-silica were mixed evenly in a mass ratio of 1:0.05, placed in an internal mixer, stirred at 200°C for 10 min, poured into a mold, maintained at 200°C and 3 MPa for 6 min, kept the pressure constant, cooled to 100°C and kept warm for 2 h, naturally cooled to room temperature and then demolded to obtain a wear-resistant and impact-resistant polyurethane material.
[0042] Comparative Example 1
[0043] The difference between the preparation method of the wear-resistant and impact-resistant polyurethane material of Comparative Example 1 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: heptamethylcyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide and toluene are mixed uniformly in a mass ratio of 1:0.7:0.02:0.02:11, stirred at 70°C and 400r / min for 35min, 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane (0.25 times the mass of heptamethylcyclotetrasiloxane) is added, stirring is continued for 20min, the temperature is lowered to 45°C and stirring is continued for 9min, after cooling to room temperature, an equal volume of deionized water and toluene are mixed and washed, the mixture is allowed to stand for stratification, the aqueous phase is removed, the washing is repeated 4 times, the organic phase is placed in a drying oven, and dried at 55°C for 9h under vacuum conditions to obtain a functionalized siloxane oligomer. The remaining steps are the same as those of Example 2.
[0044] Comparative Example 2
[0045] The preparation method of the wear-resistant and impact-resistant polyurethane material of Comparative Example 2 is different from that of Example 2 in that step (1) is not performed, and step (2) is modified as follows: polyether polyol, 1,4-butanediol, and N,N-dimethylformamide are uniformly mixed in a mass ratio of 1.7:0.4:25, stirred at 55°C and 400r / min for 25min, 1-chloromethyl-2,4-diisocyanobenzene (2.4 times the mass of the polyether polyol) and dibutyl dilaurate (0.05 times the mass of the polyether polyol) are added. Base tin, continue stirring to react for 10 minutes, heat to 90°C, continue stirring to react for 4.5 hours, dry at 55°C for 9 hours under vacuum conditions to obtain polyurethane; polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine, N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:0.7:0.04:11, stir at 55°C, 400r / min for reaction for 2.5 hours, and dry at 55°C for 9 hours under vacuum conditions to obtain modified polyurethane. The remaining steps are the same as in Example 2.
[0046] Comparative Example 3
[0047] The preparation method of the wear-resistant and impact-resistant polyurethane material of Comparative Example 3 is different from that of Example 2 only in step (2), and step (2) is modified as follows: polyether polyol, functionalized siloxane oligomer, 1,4-butanediol, and N,N-dimethylformamide are uniformly mixed in a mass ratio of 1:0.7:0.4:25, stirred at 55°C and 400 r / min for 25 min, 1-chloromethyl-2,4-diisocyanobenzene (2.4 times the mass of the polyether polyol) and dibutyltin dilaurate (0.05 times the mass of the polyether polyol) are added, stirring is continued for 10 min, the temperature is raised to 90°C, stirring is continued for 4.5 h, and drying is carried out at 55°C under vacuum for 9 h to obtain modified polyurethane. The remaining steps are the same as those of Example 2.
[0048] Comparative Example 4
[0049] The preparation method of the wear-resistant and impact-resistant polyurethane material of Comparative Example 4 is different from that of Example 2 only in step (3). Step (3) is modified as follows: aminopropyl triethoxysilane and anhydrous ethanol are mixed uniformly in a mass ratio of 1:25, the pH value is adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and stirred at 20° C. and 400 r / min for 55 min to prepare a silane hydrolyzate; nano-silicon dioxide and anhydrous ethanol are mixed uniformly in a mass ratio of 1:55, silane hydrolyzate with a mass of 9 times that of nano-silicon dioxide is added, the reaction is stirred at 55° C. and 400 r / min for 2.5 h, filtered, washed with anhydrous ethanol 4 times, and placed under vacuum. 55 ℃ drying for 9h to obtain pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid were added to N,N-dimethylformamide with a molar ratio of 1:0.85, and the pretreated nano-silica with a mass of 0.7 times of aminoethyl sulfide was added, and dicyclohexylcarbodiimide with a mass of 0.04 times of aminoethyl sulfide was added, and the reaction was stirred at 75 ℃ and 400 r / min for 5.5h, filtered, washed with deionized water 4 times, and dried at 55 ℃ for 7.5h under vacuum conditions to obtain modified nano-silica. The remaining steps are the same as those in Example 2.
[0050] Comparative Example 5
[0051] The preparation method of the wear-resistant and impact-resistant polyurethane material of Comparative Example 5 is different from that of Example 2 in that step (3) is not performed, and step (4) is modified as follows: the modified polyurethane and nano-silicon dioxide are mixed uniformly at a mass ratio of 1:0.04, placed in an internal mixer, stirred at 195° C. for 11 min, poured into a mold, maintained at 195° C. and 2.5 MPa for 7 min, kept the pressure constant, cooled to 95° C. and maintained for 2.5 h, naturally cooled to room temperature, and then demolded and taken out to obtain the wear-resistant and impact-resistant polyurethane material. The remaining steps are the same as those of Example 2.
[0052] Test Example 1
[0053] Flame retardant performance test
[0054] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406.2, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 1.
[0055] Table 1
[0056]
[0057] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the wear-resistant and impact-resistant polyurethane material prepared by the present invention has good flame retardant properties.
[0058] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that the functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane are ring-opened polymerized and end-capped with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to obtain the functionalized siloxane oligomer, and hydroxyl groups are introduced at both ends of the molecular chain of the functionalized siloxane oligomer. The hydroxyl groups introduced at both ends of the molecular chain can participate in the polymerization reaction of the polyurethane, and the polyether polyol, the functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2, Polyurethane is prepared by polymerization of 4-diisocyanobenzene, and Si-O bonds are introduced into the main chain of polyurethane molecules. The bond energy of Si-O bonds is greater than that of CC bonds, so compared with CC bonds, Si-O bonds need to absorb more heat and their own vibration energy to resolve the energy of thermal decomposition of polymer materials. The layered SiO2 formed by the degradation of siloxane during combustion migrates to the surface of the carbon layer, making the carbon layer denser, inhibiting the oxidation of the carbon layer, enhancing the stability of the carbon layer at high temperatures, and giving the wear-resistant and impact-resistant polyurethane material excellent flame retardant properties.
[0059] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 5, indicating that pretreated nano-silica is prepared by reacting nano-silica and aminopropyltriethoxysilane, and amino groups are introduced into the pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid are polymerized and grown on the pretreated nano-silica to prepare pre-modified nano-silica, and a DOPO structure is introduced into the pre-modified nano-silica. The DOPO structure contains biphenyl rings and phenanthrene ring structures in its molecular structure, and in particular, the side phosphorus groups are introduced in the form of cyclic O=PO bonds, so that the DOPO structure has higher thermal stability and chemical stability than general, non-annulated organic phosphates, and better flame retardant properties, thereby giving the wear-resistant and impact-resistant polyurethane material excellent flame retardant properties.
[0060] Test Example 2
[0061] Antimicrobial performance testing
[0062] Test method: The examples and comparative examples were cut into 10 mm × 10 mm samples and sterilized by ultraviolet irradiation for 3 h; the Escherichia coli strains were activated and prepared to a concentration of 3 × 10 4 cfu / ml bacterial suspension; put the sample into the bacterial suspension, shake at 300r / min for 5min at room temperature, take 1ml of the bacterial suspension and dilute it to 100 times, take 1ml of the diluted bacterial suspension and inoculate it into agar medium, culture it at 37℃ for 16h, count the colonies according to the method in GB / T15979, and calculate the antibacterial rate. The results are shown in Table 2.
[0063] Table 2
[0064]
[0065] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the wear-resistant and impact-resistant polyurethane material prepared by the present invention has good antibacterial properties.
[0066] By comparison, the antibacterial rates of Examples 1 to 3 are greater than those of Comparative Examples 4 to 5, indicating that pretreated nano-silica is prepared by reacting nano-silica and aminopropyltriethoxysilane, and amino groups are introduced into the pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid are polymerized and grown on the pretreated nano-silica to prepare pre-modified nano-silica, and sulfide is introduced into the pre-modified nano-silica; the sulfide on the pre-modified nano-silica is reacted with the bromine atom on 2-bromomethylfuran to generate a sulfonium salt to prepare modified nano-silica, and sulfonium salt is introduced into the modified nano-silica. Sulfonium salt is a cationic antibacterial structure that can impart excellent antibacterial properties to wear-resistant and impact-resistant polyurethane materials.
[0067] Test Example 3
[0068] Hydrophobicity test
[0069] Test method: The water drop contact angles of the embodiments and comparative examples were tested using the sessile drop method on an OCA20 contact angle meter, with the water drop volume being 5 μL. The results are shown in Table 3.
[0070] Table 3
[0071]
[0072] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the wear-resistant and impact-resistant polyurethane material prepared by the present invention has good hydrophobic properties.
[0073] By comparison, the contact angles of Examples 1 to 3 are greater than the contact angle of Comparative Example 2, indicating that a functionalized siloxane oligomer is prepared by ring-opening polymerization of functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane and end-capping with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane, a CF bond is introduced into the side chain of the functionalized siloxane oligomer molecule, and hydroxyl groups are introduced into both ends of the molecular chain. The hydroxyl groups introduced into both ends of the molecular chain can participate in the polymerization reaction of polyurethane, and a CF bond is introduced into the side chain of the polyurethane molecule. The bond energy of the CF bond is relatively high and the polarizability is relatively low. The matrix material containing the CF bond has a high repellency not only to aqueous substances, but also to oily substances, and can give the wear-resistant and impact-resistant polyurethane material excellent hydrophobic and antifouling properties.
[0074] Test Example 4
[0075] Wear resistance test
[0076] Test method: The wear rates of the examples and comparative examples were tested according to GBIT3960. The results are shown in Table 4.
[0077] Table 4
[0078]
[0079] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 4, it can be found that the wear-resistant and impact-resistant polyurethane material prepared by the present invention has good wear resistance.
[0080] By comparison, the wear rates of Examples 1 to 3 are lower than those of Comparative Examples 1 to 2, indicating that the Si-H bond on heptamethylcyclotetrasiloxane is reacted with the carbon-carbon double bond on N-allylmaleimide to prepare the functionalized cyclotetrasiloxane, and the maleimide group is introduced into the functionalized cyclotetrasiloxane; the functionalized cyclotetrasiloxane and trifluoropropylmethylcyclotrisiloxane are ring-opened polymerized and end-capped with 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane to prepare the functionalized siloxane oligomer; and the functionalized siloxane is reacted with the carbon-carbon double bond on N-allylmaleimide to prepare the functionalized cyclotetrasiloxane. Maleimide groups are introduced into the side chains of the alkyl oligomer molecules, and hydroxyl groups are introduced into both ends of the molecular chains. The hydroxyl groups introduced into both ends of the molecular chains can participate in the polymerization reaction of the polyurethane, and maleimide groups are introduced into the side chains of the polyurethane molecules; the maleimide groups introduced into the side chains can undergo Diels-Alder addition reaction with the furan groups introduced into the modified nano-silica to form a thermally reversible cross-linking network, inhibit the relative slip between the molecular chains, and endow the wear-resistant and impact-resistant polyurethane material with excellent wear resistance.
[0081] By comparison, the wear rates of Examples 1 to 3 are less than those of Comparative Examples 4 to 5, indicating that pretreated nano-silica is prepared by reacting nano-silica and aminopropyltriethoxysilane, and amino groups are introduced into the pretreated nano-silica; aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid are polymerized and grown on pretreated nano-silica to prepare pre-modified nano-silica, and sulfide is introduced into the pre-modified nano-silica; the sulfide on the pre-modified nano-silica is reacted with the bromine atom on 2-bromomethylfuran to form a sulfonium salt to prepare modified nano-silica, furan groups are introduced into the modified nano-silica, and the furan groups introduced into the modified nano-silica are further reacted. The furan group can undergo a Diels-Alder addition reaction with the maleimide group introduced on the side chain of the modified polyurethane molecule to form a thermally reversible cross-linking network, inhibit the relative slip between the molecular chains, and give the wear-resistant and impact-resistant polyurethane material excellent wear resistance; the wear rate of comparative example 5 is greater than the wear rate of comparative example 4, indicating that the nano-silicon dioxide has a high specific surface area and excellent mechanical properties, can improve the strength and hardness of the matrix resin, modify the nano-silicon dioxide, increase the compatibility of the nano-silicon dioxide with the matrix resin, reduce the agglomeration of the nano-silicon dioxide, make the nano-silicon dioxide uniformly dispersed in the matrix resin, give full play to the reinforcing effect of the nano-silicon dioxide, and further improve the wear resistance of the wear-resistant and impact-resistant polyurethane material.
[0082] Test Example 5
[0083] Anti-aging performance test
[0084] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T1040, and their tensile strength was tested. The examples and comparative examples were treated at a temperature of 120°C and an oxygen concentration of 32% under normal pressure for 72 hours, and their tensile strength was tested. The change rate of the tensile strength of the examples and comparative examples before and after the thermal oxygen aging treatment was calculated. The results are shown in Table 5.
[0085] Table 5
[0086]
[0087] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 5, it can be found that the wear-resistant and impact-resistant polyurethane material prepared by the present invention has good anti-aging performance.
[0088] By comparison, the change rate of tensile strength of Examples 1 to 3 is less than the change rate of tensile strength of Comparative Example 3, indicating that polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and 1-chloromethyl-2,4-diisocyanobenzene are polymerized to prepare polyurethane, and chlorine atoms are introduced into the side chains of polyurethane molecules; the chlorine atoms introduced into the side chains of polyurethane are reacted with the amino groups on 4-(3-aminopropyl)-2,6-di-tert-butylphenol to prepare modified polyurethane, and hindered phenol structures are introduced into the side chains of modified polyurethane. The hindered phenol structures can capture free radicals, terminate free radical chain reactions, and prevent free radical destructive effects in polymers, thereby giving the wear-resistant and impact-resistant polyurethane material excellent anti-aging properties.
[0089] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a wear-resistant and impact-resistant polyurethane material, characterized in that: The method comprises the following preparation steps: (1) Functionalized cyclotetrasiloxane, trifluoropropylmethylcyclotrisiloxane, tetramethylammonium hydroxide, dimethyl sulfoxide and toluene are mixed in a mass ratio of 1:(0.6~0.8):(0.01~0.03):(0.01~0.03):(10~12), stirred at 65~75℃, 300~500r / min for 30~40min, added a capping agent of 0.2~0.3 times the mass of the functionalized cyclotetrasiloxane, continued to stir and react for 18~22min, cooled to 40~50℃ and continued to stir for 8~10min, cooled to room temperature, washed with an equal volume of deionized water and toluene, allowed to stand for stratification, removed the aqueous phase, repeated washing 3~5 times, took the organic phase and placed it in a drying oven, dried at 50~60℃ under vacuum conditions for 8~10h to obtain a functionalized siloxane oligomer; (2) Mix polyether polyol, functionalized siloxane oligomer, 1,4-butanediol and N,N-dimethylformamide in a mass ratio of 1:(0.6~0.8):(0.3~0.5):(20~30) and stir at 50~60°C and 300~500r / min for 20~30min. Add 1-chloromethyl-2,4-diisocyanobenzene (2.3~2.5 times the mass of polyether polyol) and dibutyltin dilaurate (0.04~0.06 times the mass of polyether polyol). Continue stirring and reacting for 9~11min and raise the temperature to 88~92℃, continue stirring to react for 4~5h, dry at 50~60℃ under vacuum conditions for 8~10h to obtain polyurethane; mix polyurethane, 4-(3-aminopropyl)-2,6-di-tert-butylphenol, triethylamine, and N,N-dimethylformamide in a mass ratio of 1:(0.6~0.8):(0.03~0.05):(10~12) evenly, stir at 50~60℃, 300~500r / min to react for 2~3h, and dry at 50~60℃ under vacuum conditions for 8~10h to obtain modified polyurethane; (3) Add aminoethyl sulfide and 2-[(6-oxo-6H-dibenzo[c,e][1,2]oxaphosphorin-6-yl)methyl]succinic acid in a molar ratio of 1:(0.8-0.9) to N,N-dimethylformamide (20-30 times the mass of aminoethyl sulfide), add pretreated nano-silica (0.6-0.8 times the mass of aminoethyl sulfide), add dicyclohexylcarbodiimide (0.03-0.05 times the mass of aminoethyl sulfide), and stir at 70-80°C and 300-500 r / min to react. The pre-modified nano-silica was prepared by mixing the pre-modified nano-silica, 2-bromomethylfuran and tetrahydrofuran in a mass ratio of 1:(2-3):(10-12), stirring at 10-30°C and 300-500r / min for 20-24h, filtering, washing with ether for 3-5 times, and drying at 50-60°C for 8-10h under vacuum conditions to obtain modified nano-silica. (4) The modified polyurethane and modified nano-silica are mixed uniformly in a mass ratio of 1:(0.03-0.05), placed in an internal mixer, stirred at 190-200°C for 10-12 minutes, poured into a mold, and molded to obtain a wear-resistant and impact-resistant polyurethane material; The preparation method of the functionalized cyclotetrasiloxane in step (1) is as follows: adding heptamethylcyclotetrasiloxane and N-allylmaleimide in a molar ratio of 1:1 to toluene with a mass of 8 to 10 times that of heptamethylcyclotetrasiloxane, adding chloroplatinic acid with a mass of 0.03 to 0.05 times that of heptamethylcyclotetrasiloxane, stirring at 70 to 80° C. and 300 to 500 r / min for reaction for 3 to 4 hours, and drying at 50 to 60° C. under vacuum conditions for 7 to 9 hours to obtain the functionalized cyclotetrasiloxane; The end-capping agent in step (1) is 1,3-bis(4-hydroxybutyl)tetramethyldisiloxane; The preparation method of the pretreated nano-silicon dioxide in step (3) is as follows: nano-silicon dioxide and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(50-60), silane hydrolyzate is added in an amount of 8-10 times the mass of the nano-silicon dioxide, the mixture is stirred at 50-60° C. and 300-500 r / min for 2-3 h, filtered, washed with anhydrous ethanol for 3-5 times, and dried at 50-60° C. under vacuum conditions for 8-10 h to obtain the pretreated nano-silicon dioxide; The preparation method of the silane hydrolyzate is as follows: aminopropyltriethoxysilane and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(20-30), the pH value is adjusted to 4-6 with a 1 mol / L oxalic acid aqueous solution, and the silane hydrolyzate is prepared by stirring at 10-30° C. and 300-500 r / min for 50-60 min.
2. The method for preparing a wear-resistant and impact-resistant polyurethane material according to claim 1, characterized in that: The model of the polyether polyol in step (2) is HSH-240.
3. The method for preparing a wear-resistant and impact-resistant polyurethane material according to claim 1, characterized in that: The process parameters of the compression molding in step (4) are: at 190-200°C, 2-3 MPa, holding pressure for 6-8 min, keeping the pressure constant, cooling to 90-100°C and keeping it warm for 2-3 h, and naturally cooling to room temperature before demoulding and taking it out.
4. A wear-resistant and impact-resistant polyurethane material prepared according to the method for preparing a wear-resistant and impact-resistant polyurethane material according to any one of claims 1 to 3.