A method for preparing antibacterial water-based acrylic resin ink

By adding diethanolamine-modified nanosilica and terminal benzyl chloride-based polyurethane to acrylic resin ink, a stable chemical cross-linked network and antibacterial groups are formed, which solves the problems of insufficient adhesion, water resistance and antibacterial performance of traditional inks. Significantly improves the adhesion, water resistance and antibacterial properties of the ink.

CN118685072BActive Publication Date: 2024-10-29YANTAI GOLDEN FUJI INK CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411171473.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-10-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

Traditional acrylic resin inks have low adhesion, poor water resistance and abrasion resistance, and do not have antibacterial properties.

Method used

By adding diethanolamine modified nanosilica and terminal benzyl chloride polyurethane to acrylic resin, the epoxy group of diethanolamine and KH560 modified nanosilica is used to perform a ring-opening reaction to introduce tertiary amine groups and hydroxyl groups. group, promoting nano The hydrophilicity and dispersion of silica, and the terminal benzyl chloride alcohol end-capping reaction generates terminal benzyl chloride polyurethane, forming a stable chemical cross-linked network, enhancing the adhesion and water resistance of the ink, and introducing antibacterial benzyl groups. Quaternary ammonium salt groups improve antibacterial properties.

Benefits of technology

It significantly improves the adhesion, water resistance and antibacterial performance of the ink, improves the wear resistance of the ink, and forms a stable chemical cross-linked network and antibacterial ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of inks, and discloses a preparation method of an antibacterial water-based acrylic resin ink, including 100 parts by weight of water-based acrylic resin, 10-40 parts by weight of terminal benzyl chloride polyurethane, 1-8 parts by weight of diethanolamine-modified nano-silicon dioxide, defoamer, dispersant, thickener, pigment filler; diethanolamine-modified nano-silicon dioxide contains tertiary amine groups, and acrylic resin also contains tertiary amine groups. During heat curing, tertiary amine groups of both react with the terminal benzyl chloride of polyurethane to undergo quaternization reaction, so that silicon dioxide, acrylic resin and polyurethane are bridged by chemical bonding, and the interfacial force between the three is enhanced, and the three are heat cured to form a stable chemical cross-linked network, which is conducive to improving adhesion and water resistance. At the same time, a large amount of antibacterial benzyl quaternary ammonium salt groups are introduced into the ink paint film, which significantly improves the bactericidal ability and antibacterial performance of the paint film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inks, in particular to a method for preparing an antibacterial water-based acrylic resin ink. Background Art

[0002] Ink is mainly composed of resin binders, pigments, additives, etc., and is widely used in the printing field. Among them, the resin binders mainly include acrylic resins, polyurethanes, etc., which play a decisive role in the performance of inks. The development of high-performance resin binders and inks is a research hotspot. Water-based acrylic resin inks are simple to prepare, green and environmentally friendly, and are the most widely used. However, traditional acrylic resin inks have defects such as low adhesion, poor water resistance, poor wear resistance, and no antibacterial properties.

[0003] Polyurethane has the advantages of good toughness and high mechanical strength. When added to acrylic resin, its comprehensive performance can be improved. Nano-silicon dioxide is a common nanomaterial with high mechanical properties, strong high temperature resistance, large specific surface area, and easy surface modification. It is widely used in inks, coatings and other materials. Chinese patent CN114752252B discloses a PET surface printing water-based matte oil and its preparation method. With water-based polyurethane emulsion, water-based acrylic resin emulsion, cross-linked oxidized starch modified silica matte filler and the like as raw materials, the obtained water-based matte ink has the advantages of good matte feeling, high transparency, and high substrate adhesion. However, the patent does not improve the water resistance, wear resistance, antibacterial and other properties of the matte ink. Summary of the invention

[0004] Technical problem to be solved: The present invention provides a method for preparing an antibacterial water-based acrylic resin ink, which solves the problems of low adhesion, poor water resistance and wear resistance, and lack of antibacterial properties of acrylic resin ink.

[0005] Technical solution: A method for preparing an antibacterial water-based acrylic resin ink:

[0006] S1. Add water to a flask, introduce nitrogen, heat to 75-80°C, drop a monomer solution containing acrylic acid, butyl acrylate, methyl methacrylate, 2-(dimethylamino)ethyl methacrylate (CAS No. 2867-47-2), OP-10, and sodium dodecyl sulfate, and simultaneously drop an initiator solution containing ammonium persulfate and sodium bicarbonate, and react for 30-40 minutes; then heat to 80-85°C, add additional monomer solution and initiator solution, react for 3-4 hours, cool, and add ammonia water to neutralize the solution to obtain a water-based acrylic resin.

[0007] S2. Add ethanol and KH560 modified nano-silica into a flask, stir and disperse, add diethanolamine, heat to 55-70°C and react for 18-24h, filter after the reaction, wash with ethanol, and dry to obtain diethanolamine modified nano-silica.

[0008] S3. Add dry polytetrahydrofuran ether diol and diisocyanate monomer into a flask, introduce nitrogen, heat to 75-85°C, and stir to carry out prepolymerization for 2-3 hours; then add 2,2-dihydroxymethylpropionic acid and dibutyltin dilaurate to carry out chain extension reaction for 40-60 minutes; finally, add 4-(chloromethyl)benzyl alcohol (CAS No. 16473-35-1) to carry out end-capping reaction for 30-40 minutes, cool, add triethylamine to neutralize the solution, add water, stir and disperse to obtain terminal benzyl chloride polyurethane.

[0009] S4. Add 100 parts by weight of water-based acrylic resin, 10-40 parts by weight of benzyl chloride-terminated polyurethane, 1-8 parts by weight of diethanolamine-modified nano-silica, 0.4-0.8 parts by weight of defoamer, 0.7-0.9 parts by weight of dispersant, 0.4-0.7 parts by weight of thickener, and 25-30 parts by weight of color filler into a container, disperse in a high-speed disperser, and then grind in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0010] Preferably, in S1, the mass ratio of acrylic acid, butyl acrylate, methyl methacrylate and 2-(dimethylamino)ethyl methacrylate is (3-5):(50-55):(33-40):(3-8).

[0011] Preferably, in S2, the mass ratio of KH560 modified nano-silica to diethanolamine is 100:(30-120).

[0012] Preferably, in S3, the molar ratio of polytetramethylene ether diol, diisocyanate monomer, 2,2-dihydroxymethylpropionic acid, and 4-(chloromethyl)benzyl alcohol is 1:(2.6-2.8):(1-1.2):(2-2.2).

[0013] Preferably, the diisocyanate monomer is toluene-2,4-diisocyanate or isophorone diisocyanate.

[0014] Preferably, the preparation method of KH560 modified nano-silica is: adding nano-silica to ethanol, adding ethanol solution containing KH560 after ultrasonic dispersion, heating and stirring until ethanol evaporates, washing with ethanol, drying, and grinding to obtain KH560 modified nano-silica.

[0015] Technical effect: The present invention uses diethanolamine to carry out a ring-opening reaction with the epoxy group of KH560 modified nano-silica to obtain diethanolamine modified nano-silica, thereby introducing tertiary amine groups and a large number of hydroxyl groups on the surface of the nano-silica. The present invention uses polytetrahydrofuran ether diol, toluene-2,4-diisocyanate and other monomers, and 2,2-dihydroxymethyl propionic acid to react to obtain terminal isocyanate polyurethane, and then uses 4-(chloromethyl)benzyl alcohol for end-capping to obtain terminal benzyl chloride polyurethane.

[0016] The invention adds diethanolamine-modified nano silicon dioxide and terminal benzyl chloride polyurethane to acrylic resin ink. After the nano silicon dioxide is modified by diethanolamine, a large amount of hydrophilic hydroxyl groups are introduced on the surface, thereby improving the hydrophilicity of the nano silicon dioxide, making it more dispersible in the water-based ink matrix, and being beneficial to improving the wear resistance of the ink. Meanwhile, the diethanolamine-modified nano silicon dioxide contains a tertiary amine group, and the acrylic resin also contains a tertiary amine group. During the thermal curing process, the tertiary amine groups of the two react with the terminal benzyl chloride of the polyurethane to undergo quaternization reaction, thereby bridging the silicon dioxide, the acrylic resin and the polyurethane through chemical bonding, thereby enhancing the interfacial force among the three. Meanwhile, the three are thermally cured to form a stable chemical cross-linking network, which is beneficial to improving adhesion and water resistance.

[0017] The diethanolamine-modified nano-silica, acrylic resin and terminal benzyl chloride polyurethane undergo quaternization reaction during the thermal curing process, and a large amount of antibacterial benzyl quaternary ammonium salt groups are introduced into the ink film, thereby significantly improving the bactericidal ability and antibacterial performance of the film. DETAILED DESCRIPTION

[0018] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but this is not intended to limit the present invention.

[0019] 2 g of nano-silica was added to 40 mL of ethanol, and after ultrasonic dispersion, 5 mL of ethanol solution containing 0.4 g of KH560 was added, and the mixture was heated and stirred until the ethanol was evaporated, washed with ethanol, dried, and ground to obtain KH560-modified nano-silica.

[0020] The thickener of the present invention is Tesif DR72, the defoamer is SURFYNOL MD-20, the dispersant is TEGO760W, and the nano silicon dioxide is Jikang SS-S10 with an average particle size of 50 nm. Example 1

[0021] S1. Add 4 g acrylic acid, 55 g butyl acrylate, 34 g methyl methacrylate, 3 g 2-(dimethylamino)ethyl methacrylate, 0.8 g OP-10, and 1.6 g sodium dodecyl sulfate to 80 mL of water, and stir to disperse to obtain a monomer solution; add 0.8 g ammonium persulfate and 0.5 g sodium bicarbonate to 10 mL of water to obtain an initiator solution; add 20 mL of water to a flask, pass nitrogen, heat to 75°C, drop 20 mL of the monomer solution, and simultaneously drop 3 mL of the initiator solution, and react for 30 min; then heat to 85°C, drop 60 mL of the monomer solution and 7 mL of the initiator solution, react for 4 h, cool, and add ammonia water to neutralize the solution to pH 8 to obtain a water-based acrylic resin.

[0022] S2. Add 80 mL of ethanol and 3 g of KH560 modified nano-silica to a flask, stir and disperse, add 3.6 g of diethanolamine, heat to 70°C and react for 18 hours, filter after the reaction, wash with ethanol, and dry to obtain diethanolamine modified nano-silica. The reaction formula is as follows:

[0023]

[0024] S3, add 20mmol dry polytetrahydrofuran ether diol 1000, 54mmol toluene-2,4-diisocyanate to the flask, introduce nitrogen, heat to 80°C, stir and perform prepolymerization for 2h; then add 22mmol 2,2-dihydroxymethyl propionic acid, 0.25g dibutyltin dilaurate, perform chain extension reaction for 40min; finally add 42mmol 4-(chloromethyl)benzyl alcohol, perform end-capping reaction for 40min, cool, add triethylamine to neutralize the solution to pH 7, add water, stir and disperse, and obtain terminal benzyl chloride polyurethane. The reaction formula is:

[0025]

[0026] S4. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of color filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0027] Example 2

[0028] S1. Add 5 g of acrylic acid, 50 g of butyl acrylate, 40 g of methyl methacrylate, 4.5 g of 2-(dimethylamino)ethyl methacrylate, 0.8 g of OP-10, and 1.6 g of sodium dodecyl sulfate to 80 mL of water, and stir to disperse to obtain a monomer solution; add 0.8 g of ammonium persulfate and 0.5 g of sodium bicarbonate to 10 mL of water to obtain an initiator solution; add 20 mL of water to a flask, pass nitrogen, heat to 75°C, drop 20 mL of the monomer solution, and simultaneously drop 3 mL of the initiator solution, and react for 30 min; then heat to 80°C, drop 60 mL of the monomer solution and 7 mL of the initiator solution, react for 3 h, cool, and add ammonia water to neutralize the solution to pH 8 to obtain a water-based acrylic resin.

[0029] S2. Add 70 mL of ethanol and 3 g of KH560 modified nano-silica into a flask, stir and disperse, add 2.7 g of diethanolamine, heat to 55° C. and react for 24 h. After the reaction, filter, wash with ethanol, and dry to obtain diethanolamine modified nano-silica.

[0030] S3, add 20mmol dry polytetrahydrofuran ether diol 1000, 52mmol isophorone diisocyanate into a flask, introduce nitrogen, heat to 85°C, stir and carry out prepolymerization for 2h; then add 20mmol 2,2-dihydroxymethylpropionic acid and 0.25g dibutyltin dilaurate, carry out chain extension reaction for 40min; finally add 40mmol 4-(chloromethyl)benzyl alcohol, carry out end-capping reaction for 30min, cool, add triethylamine to neutralize the solution to pH 7, add water, stir and disperse to obtain terminal benzyl chloride polyurethane.

[0031] S4. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 3 g of diethanolamine-modified nano-silica, 0.4 g of defoamer, 0.9 g of dispersant, 0.4 g of thickener, and 30 g of color filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0032] Example 3

[0033] S1. Add 5 g of acrylic acid, 51 g of butyl acrylate, 33 g of methyl methacrylate, 6 g of 2-(dimethylamino)ethyl methacrylate, 0.8 g of OP-10, and 1.6 g of sodium dodecyl sulfate to 80 mL of water, and stir to disperse to obtain a monomer solution; add 0.8 g of ammonium persulfate and 0.5 g of sodium bicarbonate to 10 mL of water to obtain an initiator solution; add 20 mL of water to a flask, pass nitrogen, heat to 75°C, drop 20 mL of the monomer solution, and simultaneously drop 3 mL of the initiator solution, and react for 40 min; then heat to 80°C, drop 60 mL of the monomer solution and 7 mL of the initiator solution, react for 3 h, cool, and add ammonia water to neutralize the solution to pH 8 to obtain a water-based acrylic resin.

[0034] S2. Add 60 mL of ethanol and 3 g of KH560 modified nano-silica into a flask, stir and disperse, add 1.8 g of diethanolamine, heat to 55° C. and react for 24 h. After the reaction, filter, wash with ethanol, and dry to obtain diethanolamine modified nano-silica.

[0035] S3, add 20mmol dry polytetrahydrofuran ether diol 1000, 56mmol toluene-2,4-diisocyanate into a flask, introduce nitrogen, heat to 75°C, stir and carry out prepolymerization for 3h; then add 24mmol 2,2-dihydroxymethylpropionic acid and 0.28g dibutyltin dilaurate, carry out chain extension reaction for 60min; finally add 44mmol 4-(chloromethyl)benzyl alcohol, carry out end-capping reaction for 40min, cool, add triethylamine to neutralize the solution to pH 7, add water, stir and disperse to obtain terminal benzyl chloride polyurethane.

[0036] S4. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 5 g of diethanolamine-modified nano-silica, 0.6 g of defoamer, 0.7 g of dispersant, 0.7 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0037] Example 4

[0038] S1. Add 3g acrylic acid, 55g butyl acrylate, 33g methyl methacrylate, 8g 2-(dimethylamino)ethyl methacrylate, 0.8g OP-10 and 1.6g sodium dodecyl sulfate to 80mL water, stir and disperse to obtain a monomer solution; add 0.8g ammonium persulfate and 0.5g sodium bicarbonate to 10mL water to obtain an initiator solution; add 20mL water to a flask, introduce nitrogen, heat to 80°C, drop 20mL of the monomer solution, and drop 3mL of the initiator solution at the same time, and react for 30min; then heat to 85°C, drop 60mL of the monomer solution and 7mL of the initiator solution, react for 3h, cool, add ammonia water to neutralize the solution to pH 8, and obtain a water-based acrylic resin.

[0039] S2. Add 60 mL of ethanol and 3 g of KH560-modified nano-silica into a flask, stir and disperse, add 0.9 g of diethanolamine, heat to 60° C. and react for 24 h. After the reaction, filter, wash with ethanol, and dry to obtain diethanolamine-modified nano-silica.

[0040] S3, add 20mmol dry polytetrahydrofuran ether diol 1000, 54mmol isophorone diisocyanate into a flask, introduce nitrogen, heat to 85°C, stir and carry out prepolymerization for 3h; then add 22mmol 2,2-dihydroxymethylpropionic acid and 0.28g dibutyltin dilaurate, carry out chain extension reaction for 40min; finally add 42mmol 4-(chloromethyl)benzyl alcohol, carry out end-capping reaction for 30min, cool, add triethylamine to neutralize the solution to pH 7, add water, stir and disperse to obtain terminal benzyl chloride polyurethane.

[0041] S4. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 8 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.9 g of dispersant, 0.4 g of thickener, and 30 g of color filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0042] The main difference between Comparative Example 1 and Example 1 is that the acrylic resin ink does not contain benzyl chloride-terminated polyurethane and diethanolamine-modified nano-silica. The details are as follows:

[0043] S1. Add 100 g of water-based acrylic resin, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain a water-based acrylic resin ink.

[0044] The main difference between Comparative Example 2 and Example 1 is that no benzyl chloride-terminated polyurethane is added to the acrylic resin ink. The details are as follows:

[0045] S1. Add 100 g of water-based acrylic resin, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0046] The main difference between Comparative Example 3 and Example 1 is that the polyurethane is not end-capped with 4-(chloromethyl)benzyl alcohol. The details are as follows:

[0047] S1. Add 20 mmol of dried polytetrahydrofuran ether diol 1000 and 54 mmol of toluene-2,4-diisocyanate into a flask, introduce nitrogen, heat to 80°C, and stir to carry out prepolymerization for 2 hours; then add 22 mmol of 2,2-dihydroxymethylpropionic acid and 0.25 g of dibutyltin dilaurate, carry out chain extension reaction for 40 minutes, cool, add triethylamine to neutralize the solution to pH 7, add water, stir and disperse to obtain polyurethane.

[0048] S2. Add 100 g of water-based acrylic resin, 10 g of polyurethane, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse the mixture in a high-speed disperser, and then grind the mixture in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0049] The main difference between Comparative Example 4 and Example 1 is that the acrylic resin ink does not contain diethanolamine-modified nano-silica. The details are as follows:

[0050] S1. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse in a high-speed disperser, and then grind in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0051] The main difference between Comparative Example 5 and Example 1 is that KH560 modified nano-silicon dioxide is added to the acrylic resin ink. The details are as follows:

[0052] S1. Add 100 g of water-based acrylic resin, 10 g of terminal benzyl chloride polyurethane, 1 g of KH560 modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0053] The antibacterial water-based acrylic resin ink was thermally cured at 70°C for 12 hours to form a paint film. The adhesion of the paint film was tested according to GB / T 1720-2020 standard.

[0054] The water resistance of the paint film is tested according to GB / T 1733-1993 standard, and then rated according to GB / T 1766-2008 standard. The higher the grade, the worse the water resistance.

[0055] The paint film was subjected to abrasion test using a printability tester, with the abrasion revolution number being 2000 revolutions. The mass of the paint film before and after abrasion was recorded, and the abrasion index S was calculated. S=(m0-m) / R, where m0 is the mass of the paint film before abrasion (mg), m is the mass of the paint film after abrasion (mg), and R is the abrasion revolution number (r). The smaller the abrasion index, the better the wear resistance.

[0056] Table 1 Ink film performance test

[0057]

[0058] Antibacterial performance test: Staphylococcus aureus and Escherichia coli were used as test bacteria. The test bacteria were cultured and activated to make 10 7 cfu / mL of bacterial suspension; 0.5mL of bacterial suspension was applied to the surface of the ink film, and then the surface of the film was covered with a sterilized polyethylene film, placed in a constant temperature incubator, and cultured at 37°C for 24h; the film surface and the polyethylene film were eluted with 20mL of saline, 0.2mL of the eluate was inoculated in beef extract peptone agar medium, and cultured at 37°C for 24h. Calculate the antibacterial rate R. R=(BC) / B×100%. B is the average number of recovered bacteria (cfu / piece) of the blank control sample, and the blank control sample is the acrylic resin ink film of Comparative Example 1. C is the average number of recovered bacteria (cfu / piece) of the experimental group.

[0059] Table 2 Antibacterial performance test of ink film

[0060]

[0061] The adhesion of the acrylic resin ink of Examples 1-4 in Table 1 reaches level 1, the water resistance level is only level 1-2, and the abrasion index is only 0.572-0.421 mg / r. It shows good adhesion, water resistance and wear resistance. This is because diethanolamine-modified nano-silica and terminal benzyl chloride polyurethane are added to the acrylic resin ink. After the nano-silica is modified by diethanolamine, a large number of hydrophilic hydroxyl groups are introduced on the surface, which improves the hydrophilicity of the nano-silica, and has better dispersibility in the water-based ink matrix, which is beneficial to improving the wear resistance of the ink. At the same time, the diethanolamine-modified nano-silica contains tertiary amine groups, and the acrylic resin also contains tertiary amine groups. During the thermal curing process, the tertiary amine groups of the two react with the terminal benzyl chloride of the polyurethane to undergo quaternization reaction, thereby bridging the silica, acrylic resin and polyurethane through chemical bonding, enhancing the interfacial force between the three, and at the same time, the three are thermally cured to form a stable chemical cross-linking network, which is beneficial to improving adhesion and water resistance.

[0062] The diethanolamine-modified nano-silica, acrylic resin and terminal benzyl chloride polyurethane in Examples 1-4 undergo quaternization reaction, introducing a large amount of antibacterial benzyl quaternary ammonium salt groups into the ink film, which significantly improves the bactericidal ability and antibacterial properties of the film.

[0063] The acrylic resin ink of Comparative Example 1 does not contain benzyl chloride-terminated polyurethane and diethanolamine-modified nano-silica, and the paint film has low adhesion, a high water resistance level, poor water resistance, a high abrasion index, and poor wear resistance.

[0064] The acrylic resin ink of Comparative Example 2 does not contain terminal benzyl chloride polyurethane, and cannot undergo quaternization reaction with water-based acrylic resin and diethanolamine-modified nano-silica. The silica and acrylic resin are not bridged by chemical bonding. The adhesion, water resistance and wear resistance of the paint film are poor. The paint film does not contain quaternary ammonium salt groups and has almost no antibacterial properties.

[0065] The polyurethane of Comparative Example 3 is not end-capped with 4-(chloromethyl)benzyl alcohol, and does not contain benzyl chloride groups, and cannot undergo quaternization reaction with water-based acrylic resin and diethanolamine-modified nano-silica. The adhesion, water resistance and wear resistance of the paint film are poor, and the paint film does not contain quaternary ammonium salt groups and has no antibacterial properties.

[0066] Comparative Example 4 does not add diethanolamine-modified nano-silica, and the wear resistance of the paint film is poor. However, during the thermal curing process, the benzyl chloride group of the benzyl chloride-terminated polyurethane can undergo quaternization reaction with the tertiary amine group of the acrylic resin to generate antibacterial quaternary ammonium salt groups, and the antibacterial properties of the paint film are significantly improved.

[0067] In Comparative Example 5, KH560 modified nano-silica is added, which does not contain a tertiary amine group and cannot undergo a quaternization reaction with the terminal benzyl chloride polyurethane, resulting in a lower interfacial force between the nano-silica and the acrylic resin and the polyurethane, and the water resistance grade and the abrasion index are higher than those in Example 1, and the water resistance and wear resistance are not good. However, the benzyl chloride group of the terminal benzyl chloride polyurethane can undergo a quaternization reaction with the tertiary amine group of the acrylic resin to generate an antibacterial quaternary ammonium salt group, and the antibacterial property of the paint film is significantly improved.

[0068] The main difference between Example 5 and Example 1 is that the amount of the benzyl chloride-terminated polyurethane is 20 g. The details are as follows:

[0069] S4. Add 100 g of water-based acrylic resin, 20 g of terminal benzyl chloride polyurethane, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse the mixture in a high-speed disperser, and then grind the mixture in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0070] The main difference between Example 6 and Example 1 is that the amount of the benzyl chloride-terminated polyurethane is 30 g. The details are as follows:

[0071] S4. Add 100 g of water-based acrylic resin, 30 g of terminal benzyl chloride polyurethane, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of pigment filler phthalocyanine blue into a container, disperse the mixture in a high-speed disperser, and then grind the mixture in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0072] The main difference between Example 7 and Example 1 is that the amount of the benzyl chloride-terminated polyurethane is 40 g. The details are as follows:

[0073] S4. Add 100 g of water-based acrylic resin, 40 g of terminal benzyl chloride polyurethane, 1 g of diethanolamine-modified nano-silica, 0.8 g of defoamer, 0.7 g of dispersant, 0.6 g of thickener, and 25 g of color filler phthalocyanine blue into a container, disperse them in a high-speed disperser, and then grind them in a ball mill to obtain an antibacterial water-based acrylic resin ink.

[0074] The properties of the ink film were tested according to the above method.

[0075] Table 3 Antibacterial water-based acrylic resin ink film performance test

[0076]

[0077] The acrylic resin inks in Examples 5-7 in Table 3 have an adhesion grade of 1, a water resistance grade of 1-2, an abrasion index of only 0.486-0.527 mg / r, and exhibit excellent antibacterial properties.

[0078] The above description of the embodiments is to facilitate the understanding and use of the present application by those skilled in the art. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present application is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the interpretation of the present application and not departing from the scope of the present application should be within the scope of protection of the present application.

Claims

1. A method for preparing an antibacterial water-based acrylic resin ink, characterized in that: The preparation method is: S1. Add water to a flask, introduce nitrogen, heat to 75-80°C, drop a monomer solution containing acrylic acid, butyl acrylate, methyl methacrylate, 2-(dimethylamino)ethyl methacrylate, OP-10, and sodium dodecyl sulfate, and simultaneously drop an initiator solution containing ammonium persulfate and sodium bicarbonate, and react for 30-40 minutes; then heat to 80-85°C, add additional monomer solution and initiator solution, react for 3-4 hours, cool, and add ammonia water to neutralize the solution to obtain a water-based acrylic resin; S2, add ethanol and KH560 modified nano-silica into a flask, stir and disperse, add diethanolamine, filter after reaction, wash, and dry to obtain diethanolamine modified nano-silica; S3, add dry polytetrahydrofuran ether diol and diisocyanate monomer into a flask, introduce nitrogen, and stir to carry out prepolymerization reaction; then add 2,2-dihydroxymethyl propionic acid and dibutyltin dilaurate to carry out chain extension reaction; finally add 4-(chloromethyl)benzyl alcohol to carry out end-capping reaction, cool, add triethylamine to neutralize the solution, add water, stir and disperse to obtain terminal benzyl chloride polyurethane; S4, adding 100 parts by weight of water-based acrylic resin, 10-40 parts by weight of benzyl chloride-terminated polyurethane, and 1-8 parts by weight of diethanolamine-modified nano-silica into a container, adding a defoamer, a dispersant, a thickener, and a color filler after stirring, dispersing in a high-speed disperser, and then grinding in a ball mill to obtain an antibacterial water-based acrylic resin ink; In S2, the mass ratio of KH560 modified nano-silica and diethanolamine is 100: (30-120); In S2, the reaction is carried out at 55-70° C. for 18-24 h.

2. The method for preparing the antibacterial water-based acrylic resin ink according to claim 1, characterized in that: In the S1, the mass ratio of acrylic acid, butyl acrylate, methyl methacrylate and 2-(dimethylamino)ethyl methacrylate is (3-5):(50-55):(33-40):(3-8).

3. The method for preparing the antibacterial water-based acrylic resin ink according to claim 1, characterized in that: In the S3, the molar ratio of polytetramethylene ether diol, diisocyanate monomer, 2,2-dihydroxymethylpropionic acid, and 4-(chloromethyl)benzyl alcohol is 1:(2.6-2.8):(1-1.2):(2-2.2).

4. The method for preparing the antibacterial water-based acrylic resin ink according to claim 3, characterized in that: The diisocyanate monomer is toluene-2,4-diisocyanate or isophorone diisocyanate.

5. The method for preparing the antibacterial water-based acrylic resin ink according to claim 1, characterized in that: In S3, the prepolymerization reaction is carried out at 75-85° C. for 2-3 hours; the chain extension reaction time is 40-60 minutes; and the end-capping reaction time is 30-40 minutes.

6. The method for preparing the antibacterial water-based acrylic resin ink according to claim 1, characterized in that: The preparation method of the KH560 modified nano-silica is as follows: adding nano-silica to ethanol, adding an ethanol solution containing KH560 after ultrasonic dispersion, heating and stirring until the ethanol is evaporated, washing, drying, and grinding to obtain the KH560 modified nano-silica.

Citation Information

Patent Citations

  • A water-based matte varnish for PET surface printing and its preparation method

    CN114752252B

  • Environment-friendly film water-based ink and preparation method thereof

    CN116218281A

  • Multi-component functional polyurethane black ink and production method thereof

    CN118206896A

  • Antibacterial UV-curable aqueous bio-based resin and application thereof in nail polish gel

    CN118496470A

  • Aqueous plastic gravure printing surface printing / composite ink, binder and preparation methods therefor

    WO2016197260A1