Magnesium phosphate inorganic glue for carbon fiber cloth reinforcement building structure and preparation method thereof

By using modified magnesium phosphate inorganic adhesive, the problem of epoxy organic adhesives being easily degraded at high temperatures is solved, the bonding performance and durability of carbon fiber cloth and concrete are improved, maintenance costs are reduced, and the high temperature stability of the structure is ensured and fire safety.

CN118685116BActive Publication Date: 2024-11-15SHANDONG JIANZHU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155574.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The epoxy organic adhesive used in the existing carbon fiber cloth reinforced concrete structure is prone to deterioration in high temperature environments, resulting in bond failure and poor durability, requiring frequent inspections, which increases maintenance costs and safety risks.

Method used

Magnesium phosphate inorganic adhesive composed of dead-burned magnesium oxide, potassium dihydrogen phosphate, ceramic powder, keramite powder, multi-walled carbon nanotubes, ethylenediaminetetraacetic acid, borax and calcium chloride were prepared through acid-base neutralization reaction. , add ceramic powder and marble powder to modify it to improve its high temperature mechanical properties and stability.

Benefits of technology

Under high temperature environment, the flexural strength and compressive strength of magnesium phosphate inorganic adhesives remain above 80%, and their high temperature resistance is significantly better than traditional epoxy organic adhesives and conventional magnesium phosphate inorganic adhesives. They have good stability, corrosion resistance, and reduce Maintenance costs improve fire safety and structural reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685116B_ABST
    Figure CN118685116B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of phosphate binders, and specifically discloses a magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth and a preparation method thereof, which is composed of the following components by mass: 100 parts of dead-burned magnesium oxide; 46-68 parts of potassium dihydrogen phosphate; 5-20 parts of ceramic powder; 5-20 parts of hornblende powder; 0.3-0.6 parts of multi-walled carbon nanotubes; 1-5 parts of dipotassium ethylenediaminetetraacetate; 1-6 parts of borax; 0.7-1 parts of calcium chloride; 20-32 parts of water. Ceramic powder and hornblende powder carry out high temperature resistant modification on magnesium phosphate inorganic glue and improve the mechanical strength of magnesium phosphate inorganic glue at room temperature and after high temperature by incorporating multi-walled carbon nanotubes. And ensure its stability as an adhesive in extreme environments such as high temperature and corrosion, solve the problem that traditional bonding glue has poor durability and needs to be frequently inspected periodically.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of phosphate binders and relates to a magnesium phosphate inorganic adhesive for reinforcing a building structure with carbon fiber cloth and a preparation method thereof. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] With the development of cities and the adjustment of industrial structure, a large number of industrial and civil buildings are facing the problems of reduced bearing capacity, insufficient reliability and durability due to reaching the design service life, early design standards not meeting the current specifications, construction defects, natural disasters and changes in usage functions. They are in urgent need of reconstruction or renovation and reinforcement. Compared with the traditional method of reinforcing concrete structures, the carbon fiber cloth reinforcement method has been widely used in the field of structural reinforcement due to its advantages of high specific strength, high specific stiffness, good corrosion resistance, wide application range and convenient construction.

[0004] At present, epoxy organic glue is commonly used as an adhesive for carbon fiber cloth reinforcement of concrete structures in actual projects. Its glass transition temperature is only 65~82℃, which is very easy to deteriorate in a fire environment, and then the bonding between the carbon fiber cloth and the reinforced components fails, resulting in failure of the reinforcement system and even causing the collapse of the building structure. In addition, epoxy organic glue has poor durability. For concrete components reinforced with CFRP cloth using organic glue, their working status should be checked regularly, and the inspection time interval should not exceed 10 years. This not only increases maintenance costs, causes damage to building decoration, affects the normal use of the structure, but also poses a challenge to the long-term safety of the structure.

[0005] Magnesium phosphate inorganic adhesive (MPIA) is a new type of cementitious material with outstanding advantages such as fast setting speed, high early strength, good bonding performance with old concrete, and low environmental impact. MPIA is mainly composed of dead-burned or dead-burned magnesium oxide, acid phosphate (mainly ammonium dihydrogen phosphate or sodium dihydrogen phosphate), retarder and admixtures in a certain proportion. Its main hydration product is struvite (MgNH4PO4·6H2O or MgKPO4·6H2O). However, struvite will decompose rapidly at around 105℃, resulting in serious loss of mechanical strength of MPIA (compared with room temperature, the flexural strength and compressive strength of MPIA after 1000℃ are reduced by 73.9%~80.5%), thus affecting its bonding performance. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a magnesium phosphate inorganic adhesive for reinforcing a building structure with a carbon fiber cloth and a preparation method thereof. The magnesium phosphate inorganic adhesive of the present invention has excellent bonding performance and high temperature resistance, and the mechanical strength and bonding performance in a high temperature environment are effectively improved.

[0007] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0008] In a first aspect, the present invention provides a magnesium phosphate inorganic adhesive for reinforcing a building structure with carbon fiber cloth, which is composed of the following components, measured by mass: 100 parts of dead-burned magnesium oxide; 46-68 parts of potassium dihydrogen phosphate; 5-20 parts of ceramic powder; 5-20 parts of amphibole powder; 0.3-0.6 parts of multi-walled carbon nanotubes; 1-5 parts of dipotassium ethylenediaminetetraacetate or disodium ethylenediaminetetraacetate; 1-6 parts of borax; 0.7-1 parts of calcium chloride; and 20-32 parts of water.

[0009] In some embodiments, the high temperature resistant magnesium phosphate inorganic glue is composed of the following components by mass: 100 parts of dead burned magnesium oxide; 50-65 parts of potassium dihydrogen phosphate; 5-20 parts of ceramic powder; 5-20 parts of amphibole powder; 0.3-0.6 parts of multi-walled carbon nanotubes; 2-5 parts of dipotassium ethylenediaminetetraacetate or disodium ethylenediaminetetraacetate; 3-6 parts of borax; 0.7-1 parts of calcium chloride; and 20-30 parts of water.

[0010] In some embodiments, the mass percentage of MgO in the dead-burned magnesium oxide is 92% to 97%.

[0011] Preferably, the particle size of the dead-burned magnesium oxide is 250-425 mesh.

[0012] In some embodiments, the particle size of the potassium dihydrogen phosphate is 32-40 mesh.

[0013] In some embodiments, the particle size of the ceramic powder is 200-300 mesh, and the particle size of the amphibole powder is 300-400 mesh.

[0014] In a second aspect, the present invention provides a method for preparing the magnesium phosphate inorganic glue for reinforcing a building structure with carbon fiber cloth, comprising the following steps: dissolving calcium chloride in a portion of water, and then uniformly mixing the calcium chloride solution with potassium dihydrogen phosphate, dipotassium ethylenediaminetetraacetate, borax, multi-walled carbon nanotubes, ceramic powder and amphibole powder to obtain a mixture;

[0015] When in use, dead-burned magnesium oxide is added to the mixture, stirred for a set time, and the remaining water is added and stirred evenly to obtain high-temperature resistant magnesium phosphate inorganic glue.

[0016] The preparation process of magnesium phosphate inorganic glue belongs to acid-base neutralization reaction. Potassium dihydrogen phosphate provides acidic components, and magnesium oxide reacts with water to provide alkaline components. The chemical reaction is rapid and violent. If a retarder is not added and the order of adding materials is adjusted, the slurry coagulation time will be too short, and it will be difficult to apply to actual projects. During preparation, the dead burned magnesium oxide and potassium dihydrogen phosphate need to be mixed step by step, and before the two are mixed, the potassium dihydrogen phosphate and the retarding component must be mixed evenly. Therefore, for the consideration of retarding, the preparation method of the present invention adopts the method of first mixing the components other than the dead burned magnesium oxide evenly, and then adding the dead burned magnesium oxide.

[0017] In summary, for the purpose of slow setting, the preparation method of the present invention adopts a method of first mixing the components other than the dead burnt magnesium oxide uniformly and then adding the dead burnt magnesium oxide.

[0018] In some embodiments, after adding the dead-burned magnesium oxide, the stirring time is 4-10 min, preferably 4-7 min.

[0019] In some embodiments, the water used to dissolve the calcium chloride accounts for 60%-80% of the total amount of water.

[0020] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0021] (1) The high temperature resistant magnesium phosphate inorganic glue used in the present invention has excellent mechanical properties after high temperature. The present invention uses ceramic powder and amphibole powder with excellent chemical stability at high temperature to modify the magnesium phosphate inorganic glue to resist high temperature, and improves the mechanical strength of the magnesium phosphate inorganic glue at room temperature and high temperature by adding multi-walled carbon nanotubes. After 200°C, its flexural strength and compressive strength can maintain more than 80% of that at room temperature, while traditional epoxy organic glue has thermal oxidation decomposition at this temperature; after 1000°C, the flexural strength and compressive strength can maintain more than 40% of that at room temperature, and the flexural strength and compressive strength are both improved by more than 50% compared with conventional magnesium phosphate inorganic glue. The high temperature resistance is significantly better than that of traditional epoxy organic glue and conventional magnesium phosphate inorganic glue.

[0022] (2) The high temperature resistant magnesium phosphate inorganic glue used in the present invention has good stability. Compared with conventional magnesium phosphate inorganic glue, the high temperature resistant magnesium phosphate inorganic glue of the present invention adds ceramic powder and hornblende powder, especially the particle size of hornblende powder is smaller than that of ceramic powder, which effectively fills the internal pores of magnesium phosphate inorganic glue (when hornblende powder and ceramic powder are co-doped, they can effectively fill tiny pores of different pore sizes, and the co-doping effect is better than that of single-doped high temperature resistant materials), and multi-walled carbon nanotubes play a bridging role, making its microstructure more compact, improving the matrix structure stability of magnesium phosphate inorganic glue in high temperature environment, thereby significantly improving it at the microscopic level. After experiencing high temperatures above 1000°C, it does not shrink, crack, or deform, and it also has strong resistance to corrosive environments such as acids, alkalis, and salts, ensuring its stability as an adhesive in extreme environments such as high temperature and corrosion, solving the problem of poor durability of traditional adhesives and the need for frequent periodic inspections, effectively reducing the maintenance cost of reinforced structures, and expanding the application scope of CFRP reinforcement technology;

[0023] (3) The high temperature resistant magnesium phosphate inorganic adhesive used in the present invention has a slow degradation of bonding performance at high temperatures. After being exposed to a high temperature of 600°C, its bonding strength is still about 25% of its strength at room temperature, while the bonding strength of epoxy organic adhesive is completely lost at 200°C, thereby ensuring the bonding reliability between the carbon fiber cloth and the concrete structure at high temperatures; solving the problem of the loss of bonding strength of traditional epoxy organic adhesives after reaching the glass transition temperature, thereby improving the fire safety of the concrete structure reinforcement system. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0025] Figure 1 This is a flow chart for preparing a magnesium phosphate inorganic adhesive test block for reinforcing a building structure with carbon fiber cloth in an embodiment of the present invention;

[0026] Figure 2 This is a graph showing the apparent characteristics of a magnesium phosphate inorganic adhesive test block for reinforcing a building structure with carbon fiber cloth according to an embodiment of the present invention after being subjected to different temperatures;

[0027] Figure 3 This is a comparison chart of the flexural strength after high temperature between the magnesium phosphate inorganic glue for reinforcing the building structure with carbon fiber cloth in the embodiment of the present invention and the conventional magnesium phosphate inorganic glue;

[0028] Figure 4 This is a comparison chart of the compressive strength after high temperature between the magnesium phosphate inorganic glue for reinforcing the building structure with carbon fiber cloth in the embodiment of the present invention and the conventional magnesium phosphate inorganic glue;

[0029] Figure 5This is an overall diagram of a magnesium phosphate inorganic adhesive test block for reinforcing a building structure with carbon fiber cloth in an embodiment of the present invention after being subjected to different temperatures after being compressively damaged;

[0030] Figure 6 This is a flow chart of applying carbon fiber cloth to reinforce building structure with magnesium phosphate inorganic glue in an embodiment of the present invention, wherein A is roughening the surface of the concrete specimen, B is applying magnesium phosphate inorganic glue on the roughening position, C is pasting the carbon fiber cloth on the magnesium phosphate inorganic glue, and D is smoothing with a scraper;

[0031] Figure 7 This is the design drawing of the double shear test specimen after high temperature in the embodiment of the present invention (unit: mm);

[0032] Figure 8 This is a comparison chart of the in-plane shear strength of magnesium phosphate inorganic adhesive and epoxy organic adhesive used for reinforcing building structures with carbon fiber cloth after different overfire temperatures in the embodiments of the present invention. DETAILED DESCRIPTION

[0033] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0034] The present invention will be further described below in conjunction with the embodiments.

[0035] In the following examples, the MgO content in the dead-burned magnesium oxide was between 92% and 97%, passed through a 425-mesh sieve, and was purchased from Haicheng Yuchen Refractory Material Manufacturing Co., Ltd.;

[0036] Potassium dihydrogen phosphate with a purity of more than 95%, passed through a 40-mesh sieve, and was purchased from Lianyungang Geli Chemical Co., Ltd.;

[0037] Ceramic powder was passed through a 250-mesh sieve and purchased from Shenzhen Changruixi New Materials Co., Ltd.;

[0038] Amphibole powder was passed through a 300-mesh sieve and purchased from Fengfeng Mineral Products Processing Plant in Lingshou County.

[0039] The purity of dipotassium ethylenediaminetetraacetate, borax and calcium chloride hexahydrate is chemically pure grade, with a purity of more than 98%.

[0040] Example 1

[0041] A magnesium phosphate inorganic adhesive for reinforcing a building structure with carbon fiber cloth consists of the following components: dead burned magnesium oxide (DBM), potassium dihydrogen phosphate (KDP), ceramic powder (TC), amphibole powder (JS), multi-walled carbon nanotubes (C), dipotassium ethylenediaminetetraacetate (SM), borax (B), calcium chloride hexahydrate (PCM), and water.

[0042] The specific preparation method is implemented according to the following steps:

[0043] Step 1: 8.2kg / m 3 Calcium chloride hexahydrate is dissolved in 3 / 4 of the total amount of water (i.e. 171.5 kg / m 3 ). Dissolving calcium chloride hexahydrate in advance can make it react better with other substances, which is conducive to achieving a better retarding effect.

[0044] Step 2: Weigh 516.8 kg / m potassium dihydrogen phosphate 3 , ceramic powder 35 kg / m 3 , hornblende powder 35kg / m 3 , Multi-walled carbon nanotubes 2.58kg / m 3 , Dipotassium ethylenediaminetetraacetate 18.2kg / m 3 , Borax 18.2kg / m 3 , and pour it into a mixing bucket and mix it for 1 min. This step is to ensure that the ceramic powder, amphibole powder and multi-walled carbon nanotubes can be evenly distributed in the mixture to achieve better high temperature resistance.

[0045] Step 3: Then add the water containing calcium chloride hexahydrate into the mixture in step 3 and continue stirring for 2 minutes.

[0046] Step 4: Weigh 912.0 kg / m of dead-burned magnesium oxide 3 , and add it into the mixture in step 4 and stir for 2 min.

[0047] Step 5: Add the remaining 1 / 4 of the water (i.e. 57.2 kg / m 3 ) is added into the mixture of step 4 and stirred for 5 min to obtain the high temperature resistant magnesium phosphate inorganic glue.

[0048] Example 2

[0049] A high temperature resistant magnesium phosphate inorganic glue, composed of the following components in parts by weight: dead burned magnesium oxide 864 kg / m 3 , potassium dihydrogen phosphate 489.6kg / m 3 、Ceramic powder 60.2kg / m 3 , hornblende powder 60.2kg / m 3 , Multi-walled carbon nanotubes 3.1kg / m 3 , Dipotassium ethylenediaminetetraacetate 17.3 kg / m 3 , Borax 17.3 kg / m 3 , calcium chloride hexahydrate 7.8 kg / m 3 、Water 216.6kg / m 3The specific preparation method is the same as that in Example 1, except that the ratio in Example 1 is changed.

[0050] Comparative Example 1

[0051] Conventional magnesium phosphate inorganic glue is composed of the following components in parts by weight: dead burned magnesium oxide 984.4 kg / m 3 , potassium dihydrogen phosphate 489.6kg / m 3 , Borax 17.3 kg / m 3 、Water 216.6kg / m 3 The specific preparation process is as follows:

[0052] S1: Weigh 489.6kg / m potassium dihydrogen phosphate 3 , Borax 17.3 kg / m 3 , and pour into a mixing bucket and mix for 1 minute;

[0053] S2: Add water to the S1 mixture and stir for 2 minutes;

[0054] S3: Weigh 984.4 kg / m of dead burned magnesium oxide 3 Add into the S2 mixture and stir for 3 minutes to obtain conventional magnesium phosphate inorganic glue.

[0055] Comparative Example 2

[0056] The difference from Example 1 is that the amphibole powder is replaced by ceramic powder, and the replaced ceramic powder is sieved through a 300-mesh sieve. The rest is the same as Example 1.

[0057] Comparative Example 3

[0058] The difference from Example 1 is that the multi-walled carbon nanotubes are omitted, and the rest are the same as Example 1.

[0059] Comparative Example 4

[0060] The difference from Example 1 is that the ceramic powder is replaced by amphibole powder, and the replaced amphibole powder is sieved through a 250-mesh sieve. The rest is the same as Example 1.

[0061] Performance Testing:

[0062] 126 magnesium phosphate inorganic glue test blocks with a size of 40 mm × 40 mm × 160 mm were prepared, wherein a control group of 21 magnesium phosphate inorganic glue test blocks were prepared using the magnesium phosphate inorganic glue in Comparative Example 1;

[0063] The 21 magnesium phosphate inorganic glue test blocks of the control group 2 were prepared using the magnesium phosphate inorganic glue in Comparative Example 2;

[0064] The 21 magnesium phosphate inorganic glue test blocks of the three control groups were prepared using the magnesium phosphate inorganic glue in Comparative Example 3;

[0065] The 21 magnesium phosphate inorganic glue test blocks of the four control groups were prepared using the magnesium phosphate inorganic glue in Comparative Example 4;

[0066] The 21 magnesium phosphate inorganic glue test blocks of one experimental group were made of the magnesium phosphate inorganic glue in Example 1;

[0067] The 21 magnesium phosphate inorganic glue test blocks of the second experimental group were made using the magnesium phosphate inorganic glue in Example 2.

[0068] Preparation and maintenance method of high temperature resistant magnesium phosphate inorganic glue test block Figure 1 conduct:

[0069] Pour the prepared magnesium phosphate inorganic slurry into a 40 mm × 40 mm × 160 mm plastic mold and vibrate it, smoothing it while vibrating until it is dense.

[0070] The surface of the specimen was covered with plastic film and demoulded after curing at room temperature (23±2℃) for 24h.

[0071] The demoulded high temperature resistant magnesium phosphate inorganic adhesive specimens were further cured in an environment of relative humidity of 50±5% and temperature of 23±2°C for 14 days.

[0072] The three groups of magnesium phosphate inorganic glue test blocks were heated to target temperatures such as room temperature, 100°C, 200°C, 400°C, 600°C, 800°C, and 1000°C at a fixed heating rate of 10°C / min (three test blocks in each group at a single target temperature). When the target temperatures were reached, the heating was stopped and the test blocks were allowed to cool naturally to room temperature.

[0073] The apparent characteristics of a group of high temperature resistant magnesium phosphate inorganic glue test blocks after experiencing different temperatures are as follows Figure 2 As shown, when the overfire temperature is below 100℃, the surface of the test block is roughly yellowish brown; when the overfire temperature rises to 400℃, the surface of the test block is gray; when the overfire temperature rises to 600℃, the surface of the test block is dark brown. When the overfire temperature is 800℃ and 1000℃, the surface color of the test block is basically the same, which is grayish white. Compared with the test blocks before experiencing high temperature, except for a small amount of transverse cracks on the surface of individual test blocks, the other test blocks have no obvious cracking, peeling, bursting and other phenomena, and the high temperature resistant magnesium phosphate inorganic glue test block has no visual shrinkage deformation after experiencing 1000℃ high temperature.

[0074] According to GB / T 17671-2021 "Test Method for Strength of Cement Mortar" (ISO method), six groups of magnesium phosphate inorganic glue test blocks were tested for flexural strength and compressive strength after high temperature. The test results of three specimens in the same group were averaged and recorded. The strength test results are as follows: Figure 3 , Figure 4 And Table 1 and Table 2. Compared with the magnesium phosphate inorganic glue specimens in the control group, the mechanical properties of the composite high-temperature resistant modified magnesium phosphate inorganic glue were significantly improved after high temperature. After experiencing a high temperature of 1000℃, its flexural strength and compressive strength were both more than 35% of the corresponding properties at room temperature, and the flexural strength and compressive strength were both increased by more than 50% compared with conventional magnesium phosphate inorganic glue. After experiencing a high temperature of 600~1000℃, the high-temperature resistant modified magnesium phosphate inorganic glue still showed a normal compressive failure morphology, such as Figure 5 As shown, it is well reflected that the high temperature resistant modified magnesium phosphate inorganic glue has overall stability at high temperature.

[0075] Table 1 Flexural strength of magnesium phosphate inorganic glue

[0076]

[0077] Table 2 Compressive strength of magnesium phosphate inorganic glue

[0078]

[0079] Compared with conventional magnesium phosphate inorganic glue, the high temperature resistant magnesium phosphate inorganic glue of the present invention adds ceramic powder and amphibole powder particles, which effectively fill the internal pores of the magnesium phosphate inorganic glue, and the multi-walled carbon nanotubes play a bridging role to make its microstructure more compact, thereby improving the matrix structure stability of the magnesium phosphate inorganic glue in a high temperature environment, making its microstructure more compact, and making the magnesium phosphate inorganic glue have good thermal stability.

[0080] The preparation of the concrete specimen reinforced with carbon fiber cloth bonded with high temperature resistant magnesium phosphate inorganic adhesive of the present invention is carried out according to the following steps:

[0081] Step 1: Roughen the area on the surface of the concrete specimen where the CFRP sheet is to be pasted, and use a blower to remove surface impurities ( Figure 6 , A);

[0082] Step 2: Properly moisten the roughened area on the surface of the concrete specimen to prevent the dry concrete surface from absorbing moisture in the high-temperature resistant magnesium phosphate inorganic glue and thus affecting the bonding performance between the two;

[0083] Step 3: Apply high temperature resistant magnesium phosphate inorganic glue as primer evenly on the roughened area of ​​the specimen surface with a thickness of 3 mm ( Figure 6 , B);

[0084] Step 4: Wet the cut carbon fiber cloth and paste it on the high temperature resistant magnesium phosphate inorganic adhesive primer, and use a scraper to repeatedly scrape along the fiber direction of the carbon fiber cloth to make the high temperature resistant magnesium phosphate inorganic adhesive primer fully infiltrate the carbon fiber cloth ( Figure 6 , C);

[0085] Step 5: Apply a layer of high temperature resistant magnesium phosphate inorganic adhesive evenly on the surface of the carbon fiber cloth with a thickness of 2mm, and smooth it with a scraper ( Figure 6 , D);

[0086] Step 6: Cure in a laboratory environment at a temperature of 23±2℃ for 14 days.

[0087] The bonding performance of the concrete specimen reinforced with carbon fiber cloth bonded with high temperature resistant magnesium phosphate inorganic adhesive of the present invention is obtained by the following method:

[0088] 38 double shear test specimens after high temperature were made and divided into 6 groups, as follows:

[0089] Group 1: 7 specimens were bonded with CFRP cloth using the high temperature resistant magnesium phosphate inorganic adhesive in Example 1, and the target temperatures were 25°C, 100°C, 200°C, 300°C, 400°C, 500°C, and 600°C, respectively;

[0090] Group 2: 7 specimens were bonded with CFRP cloth using the magnesium phosphate inorganic adhesive in Comparative Example 1, and the target temperatures were 25°C, 100°C, 200°C, 300°C, 400°C, 500°C, and 600°C respectively;

[0091] The third group: 7 specimens were bonded with CFRP cloth using the magnesium phosphate inorganic adhesive in Comparative Example 2, and the target temperatures were 25°C, 100°C, 200°C, 300°C, 400°C, 500°C, and 600°C respectively;

[0092] Group 4: 7 specimens were bonded with CFRP cloth using the magnesium phosphate inorganic adhesive in Comparative Example 3, and the target temperatures were 25°C, 100°C, 200°C, 300°C, 400°C, 500°C, and 600°C, respectively;

[0093] Group 5: 7 specimens were bonded with CFRP cloth using the magnesium phosphate inorganic adhesive in Comparative Example 4, and the target temperatures were 25°C, 100°C, 200°C, 300°C, 400°C, 500°C, and 600°C, respectively;

[0094] Group 6: Three specimens were bonded with CFRP cloth using epoxy resin (purchased from Beijing Jinhong Century Technology Co., Ltd.). When epoxy organic glue is used as the adhesive, its in-plane shear strength will be greatly reduced at a temperature of about 120°C (less than 10% of that at room temperature), thereby losing the basis for transmitting the shear force between the CFRP cloth layers and working with the concrete. Therefore, only 25°C, 100°C and 200°C target temperatures were designed.

[0095] The size of the concrete prism is 120mm×120mm×450mm, the concrete strength grade is C30, and the CFRP sheet is pasted on the two opposite sides of the concrete specimen, with a bonding length of 100mm and a bonding width of 70mm. The free lengths of the two ends of the CFRP sheet on the concrete specimen are 80mm and 50mm respectively. The specific conditions of the double shear test specimen are as follows: Figure 7 shown.

[0096] According to the "Concrete Physical and Mechanical Properties Test Method Standard" (GB / T 50081-2019), the measured concrete cube compressive strength is 30.6MPa. The CFRP cloth used is RLS-Ⅰ-300 CFRP cloth produced by Shanghai Zhinuo Decoration Materials Co., Ltd., with a thickness of 0.167mm and a density of 300g / m 2 , tensile strength is 3668MPa, elastic modulus is 240GPa, and elongation is 1.74%. The mechanical properties of epoxy organic adhesive are as follows: tensile strength is 48.8MPa, flexural strength is 93.8MPa, and compressive strength is 97.2MPa.

[0097] Before the double shear test, the specimen needs to be subjected to a high temperature test. Before the high temperature test, the specimen is placed in the furnace and the furnace top is sealed with refractory wool. The temperature is raised to the target temperature at a rate of 5℃ / min and then kept constant for 2.5 hours. When the target temperature is 100℃ and 200℃, the specimen is taken out of the furnace after being kept constant at the target temperature for 2.5 hours and naturally cooled to room temperature; when the target temperature exceeds 200℃, after the specimen reaches the constant temperature time at the target temperature, the power is turned off without opening the furnace door until the furnace temperature drops to 200℃, and then the furnace door is opened, and then it is naturally cooled to room temperature. The specimen is taken out of the furnace and placed for 3 days, and then subjected to a double shear test after high temperature.

[0098] The test results are shown in Table 3-1, Table 3-2 and Figure 8As shown, at room temperature, the bonding strength of magnesium phosphate inorganic glue is close to that of epoxy organic glue; by comparing the relative in-plane shear strength of magnesium phosphate inorganic glue and epoxy organic glue, it can be seen that before 200°C, the decrease in the in-plane shear strength of epoxy organic glue is significantly faster than that of magnesium phosphate inorganic glue; after exposure to 200°C, the in-plane shear strength of epoxy organic glue decreased by 86.6% compared with room temperature, while the residual in-plane shear strength of high-temperature resistant modified magnesium phosphate inorganic glue was as high as 4.5 times that of magnesium phosphate inorganic glue; after exposure to 600°C, the in-plane shear strength of magnesium phosphate inorganic glue in Example 1 was still about 30% of that at room temperature, which was 100% higher than that of conventional magnesium phosphate inorganic glue, while epoxy organic glue had already lost its bonding performance, thereby highlighting the fire-resistant high-temperature advantage of the high-temperature resistant magnesium phosphate inorganic glue of the present invention as an adhesive for CFRP reinforced concrete structure, ensuring the bonding reliability between CFRP cloth and concrete beam at high temperature.

[0099] Table 3-1 Test results of bonding performance between modified magnesium phosphate inorganic adhesive and epoxy resin organic adhesive after high temperature

[0100]

[0101] Table 3-2 Test results of bonding performance between modified magnesium phosphate inorganic adhesive and epoxy resin organic adhesive after high temperature

[0102]

[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A magnesium phosphate inorganic adhesive for reinforcing building structures with carbon fiber cloth, Features: The invention is composed of the following components by mass: 100 parts of dead-burned magnesium oxide; 46-68 parts of potassium dihydrogen phosphate; 5-20 parts of ceramic powder; 5-20 parts of amphibole powder; 0.3-0.6 parts of multi-walled carbon nanotubes; 1-5 parts of dipotassium ethylenediaminetetraacetate or disodium ethylenediaminetetraacetate; 1-6 parts of borax; 0.7-1 parts of calcium chloride; and 20-32 parts of water. The particle size of the ceramic powder is 200-300 mesh, and the particle size of the amphibole powder is 300-400 mesh; The method for preparing magnesium phosphate inorganic glue for carbon fiber cloth reinforcement building structure comprises the following steps: dissolving calcium chloride in a portion of water, and then uniformly mixing the calcium chloride solution with potassium dihydrogen phosphate, dipotassium ethylenediaminetetraacetate or disodium ethylenediaminetetraacetate, borax, multi-walled carbon nanotubes, ceramic powder and amphibole powder to obtain a mixture; When in use, add the dead-burned magnesium oxide into the mixture, stir for a set time, add the remaining water, stir evenly, and the mixture is obtained.

2. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1, Features: The invention is composed of the following components by mass: 100 parts of dead-burned magnesium oxide; 50-65 parts of potassium dihydrogen phosphate; 5-20 parts of ceramic powder; 5-20 parts of amphibole powder; 0.3-0.6 parts of multi-walled carbon nanotubes; 2-5 parts of dipotassium ethylenediaminetetraacetate or disodium ethylenediaminetetraacetate; 3-6 parts of borax; 0.7-1 parts of calcium chloride; and 20-30 parts of water.

3. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1 or 2, Features: The mass percentage of MgO in the dead-burned magnesium oxide is 92%-97%.

4. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1 or 2, Features: The particle size of the dead-burned magnesium oxide is 250-425 meshes.

5. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1 or 2, Features: The particle size of the potassium dihydrogen phosphate is 32-40 meshes.

6. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1, Features: After adding the dead-burned magnesium oxide, the stirring time is 4-10 minutes.

7. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 1, Features: The water used to dissolve calcium chloride accounts for 60%-80% of the total water.

8. The magnesium phosphate inorganic glue for reinforcing building structures with carbon fiber cloth according to claim 7, Features: The water used to dissolve calcium chloride accounts for 65%-75% of the total water.