A titanium-nickel alloy material and preparation method thereof

By doping enhanced graphene and Hf and Nb powders in titanium nickel alloy, the hardness and phase transition temperature of titanium nickel alloy are improved, and the problems of low hardness and insufficient wear resistance are solved, thus achieving higher mechanical strength and high temperature stability.

CN118685679BActive Publication Date: 2024-11-19SHENYANG JIENTE NEW MATERIALS DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411155446.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-19
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Traditional titanium nickel shape memory alloys have low hardness, resulting in insufficient wear resistance, and the phase transition temperature is usually lower than 100℃, making them not suitable for use in high-temperature environments.

Method used

Reinforced graphene is doped in titanium nickel alloy, and Hf powder and Nb powder are added to increase the phase transition temperature and mechanical strength of the alloy by coating nickel metal nanoparticles and zirconium nanometal ions on graphene oxide.

Benefits of technology

It significantly improves the hardness and high temperature resistance of titanium nickel alloy, enhances the interface bonding and mechanical properties of the alloy, and extends the high temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685679B_ABST
    Figure CN118685679B_ABST
Patent Text Reader

Abstract

The invention discloses a titanium-nickel alloy material and a preparation method thereof in the field of titanium-nickel alloy technology. The raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 23-34 parts of Ti powder, 43-46 parts of Ni powder, 19-29 parts of Hf powder, 5-11 parts of Nb powder, and 0.5-1 parts of enhanced graphene. The invention dopes enhanced graphene in the titanium-nickel alloy raw material, and the enhanced graphene nickel metal nanoparticles and zirconium nanometal ions coat the graphene, which can improve the interface bonding of graphene in the alloy material, and add Hf powder and Nb powder, and replace the Ti element in NiTi with the Hf element, which can improve the phase transition temperature and mechanical strength of the titanium-nickel metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of titanium-nickel alloys, and specifically refers to a titanium-nickel alloy material and a preparation method thereof. Background Art

[0002] Titanium-nickel alloy is a shape memory alloy, which refers to an alloy with a certain initial shape that is plastically deformed and fixed into another shape at low temperature, and can be restored to its original shape by heating above a critical temperature. It is widely used in a variety of technical fields, including the following main fields: Titanium-nickel alloy has good biocompatibility. In the medical field, titanium-nickel alloy is mainly used in the manufacture of medical devices, such as heart stents, orthopedic implants and dental braces; in the aerospace field, titanium-nickel alloy is used to manufacture high-performance components; titanium-nickel alloy has shape and memory effects. In the automotive industry and electrical engineering, it is used for sensors, brakes, micro switches, connectors and other micro-devices. It can be seen that nickel-titanium alloy has an important position in various high-tech fields due to its unique physical properties. Although traditional titanium-nickel shape memory alloys have excellent performance and good biocompatibility, their phase transition temperature is usually below 100°C. At the same time, nickel-titanium alloys also have a lower hardness than other cemented carbides due to their shape memory effect and superelasticity, resulting in lower wear resistance. Nickel-titanium alloys have a greater plastic deformation capacity when subjected to external forces, which means that during the friction process, the alloy surface may undergo significant plastic deformation, resulting in higher wear. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a titanium-nickel alloy material and a preparation method thereof. In order to solve the problem of low hardness of the titanium-nickel alloy, the present invention dopes enhanced graphene into the titanium-nickel alloy raw material, and the enhanced graphene nickel metal nanoparticles and zirconium nanometal ions coat the graphene, which can improve the interface bonding of the graphene in the alloy material. Hf powder and Nb powder are added, and the Ti element in NiTi is replaced by the Hf element, which can improve the phase transition temperature and mechanical strength of the titanium-nickel metal.

[0004] In order to achieve the above-mentioned object, the technical solution adopted by the present invention is as follows: The present invention proposes a titanium-nickel alloy material, wherein the raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 23-34 parts of Ti powder, 43-46 parts of Ni powder, 19-29 parts of Hf powder, 5-11 parts of Nb powder, and 0.5-1 part of enhanced graphene;

[0005] Preferably, the method for preparing the enhanced graphene specifically comprises the following steps:

[0006] P1. Disperse graphene oxide in deionized water, place it under 400W power for ultrasonic treatment, fill it with N2 after 20-30 minutes, and treat it for 15 minutes to obtain a graphene oxide dispersion for standby use;

[0007] P2. Prepare a nickel sulfate aqueous solution, add it to the graphene oxide dispersion prepared in step P1 under a nitrogen atmosphere, and stir it mechanically at 400-500 rpm for 30-40 minutes. Then, add NaBH4 solution, continue stirring and reacting for 60-90 minutes to obtain an intermediate reaction solution, place it under a nitrogen atmosphere, and set aside;

[0008] P3, prepare an aqueous solution of zirconium sulfate, add it to the intermediate reaction solution of step P2 under a nitrogen atmosphere, continue stirring at a speed of 400-500 rpm for 30-50 min, vacuum extract and wash with anhydrous ethanol, and freeze-dry to obtain enhanced graphene;

[0009] Preferably, in step P1, the mass concentration of graphene oxide in deionized water is 2.5-3 g / L;

[0010] Preferably, in step P2, the mass of nickel sulfate in the zirconium sulfate aqueous solution is 0.1-0.2 g / mL; the added volume of the zirconium sulfate aqueous solution is 12%-20% of the volume of the graphene dispersion;

[0011] Preferably, in step P2, the molar concentration of the NaBH4 solution is 1-3 mol / L; the added volume of the NaBH4 solution is 25%-50% of the volume of the graphene dispersion;

[0012] Preferably, in step P3, the mass concentration of zirconium sulfate in the zirconium sulfate aqueous solution is 30-45 g / L; the added mass of zirconium sulfate is 17.5%-23.5% of the mass of nickel sulfate.

[0013] The present invention also provides a method for preparing a titanium-nickel alloy material, which specifically comprises the following steps:

[0014] S1, dispersing the enhanced graphene in anhydrous ethanol, and uniformly dispersing by ultrasonication to obtain an enhanced graphene slurry;

[0015] S2, mixing Ti powder, Ni powder, Hf powder and Nb powder with anhydrous ethanol, and mechanically stirring at 1000-1200 rpm to form an alloy slurry;

[0016] S3, mixing the enhanced graphene slurry prepared in step S1 with the alloy slurry prepared in step S2, placing them in a ball mill for ball milling at a speed of 300-500 rpm, with a ball-to-material ratio of 4-5:1, and a ball milling time of 8-10 h, and vacuum drying to obtain a titanium-nickel alloy precursor powder;

[0017] S4, loading the titanium-nickel alloy precursor powder prepared in step S3 into a mold, transferring it to a vacuum sintering furnace, adjusting the vacuum sintering parameters, and performing discharge ion beam sintering; discharge ion beam sintering parameters: setting the vacuum degree to 1pa, heating the temperature to 600-700°C at a heating rate of 100°C / min, and keeping the temperature for 5-10min; setting the initial sintering pressure to 1MPa, and the holding pressure to 300MPa;

[0018] S5. After the discharge ion beam sintering treatment, the temperature is increased to 1000° C. at 10° C. / min, kept at this temperature for 10 min, the temperature is further increased to 1500° C., kept at this temperature for 20 min, the temperature is further increased to 1700° C., kept at this temperature for 5 min, and naturally cooled to obtain a titanium-nickel alloy material;

[0019] Preferably, in step S1, the mass concentration of the enhanced graphene in anhydrous ethanol is 0.05-0.1 g / mL;

[0020] Preferably, in step S2, the material-liquid ratio g / mL of the alloy slurry is 1:1.5-2.

[0021] The beneficial effects achieved by the present invention are as follows:

[0022] The invention provides a titanium-nickel alloy material and a preparation method thereof. The invention dopes enhanced graphene into a titanium-nickel alloy raw material, and the enhanced graphene nickel metal nanoparticles and zirconium nanometal ions coat the graphene, so that the interface bonding property of the graphene in the alloy material can be improved. Hf powder and Nb powder are added, and the Ti element in NiTi is replaced by the Hf element, so that the phase transition temperature and mechanical strength of the titanium-nickel metal can be improved. In the invention, a nickel sulfate solution and a zirconium sulfate solution are added to a graphene oxide solution in an in-situ growth manner, and a NaBH4 solution is added to reduce the metal ions, and the graphene oxide can also be reacted to generate reduced graphene oxide, so as to form a nanostructured nickel / zirconium bimetallic coating. The reduced graphene oxide composite material is a composite material in which metal nanoparticles can be evenly distributed on the surface of graphene. The metal nanoparticles on the surface of the enhanced graphene can melt during high-temperature sintering, thereby enhancing the dispersion performance between graphene and molten metal raw materials and improving the compatibility of graphene in the metal matrix. Metal carbides are formed during high-temperature sintering to improve the high-temperature resistance and hardness of the alloy material. Hf and Zr elements can replace Ti in NiTi and increase the phase transition temperature of the shape memory alloy. Nb element is a stabilizing element and has a certain solid solubility in NiTi alloy. It can strengthen the strength of the alloy matrix through solid solution and improve the mechanical properties of the titanium-nickel alloy material. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1This is a SEM image of the enhanced graphene prepared in Example 1;

[0024] Figure 2 This is a SEM image of the sintered body of the nickel-titanium alloy material prepared in this embodiment;

[0025] Figure 3 This is a graph showing the hardness results of the titanium-nickel alloy materials prepared in Examples 1-3 and Comparative Examples 1-3.

[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0029] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0030] The sources of materials used in the present invention are as follows:

[0031] Graphene oxide, brand is Sigma-Aldrich, product number is 796034, edge oxidation degree is 4-10%;

[0032] Example 1

[0033] This embodiment provides a titanium-nickel alloy material, wherein the raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 24 parts of Ti powder, 44 parts of Ni powder, 24 parts of Hf powder, 8 parts of Nb powder, and 0.5 parts of enhanced graphene;

[0034] The preparation method of enhanced graphene specifically comprises the following steps:

[0035] P1. Accurately weigh 0.3 g of graphene oxide and disperse it in 100 mL of deionized water. Transfer it to an ultrasonic processor, and ultrasonically disperse it at 400 W for 20 min. Then transfer it to a three-necked flask, fill the reaction system with N2, and bubbling it for 15 min to obtain a graphene oxide dispersion for standby use.

[0036] P2. Accurately weigh 10 g of nickel sulfate and dissolve it in 100 mL of deionized water. Mix well until the nickel sulfate is completely dissolved. Under a nitrogen atmosphere, take 13.2 mL of nickel sulfate aqueous solution and add it to the graphene oxide dispersion prepared in step P1. Use a magnetic stirrer to stir mechanically for 40 min at a speed of 450 rpm. Then, use a peristaltic pump to slowly drop 40 mL of a 1 mol / L NaBH4 aqueous solution at a speed of 1 mL / min. Continue stirring for 60 min to obtain an intermediate reaction solution, which is placed under a nitrogen atmosphere for standby use.

[0037] P3. Accurately weigh 3 g of zirconium sulfate and dissolve it in 100 mL of deionized water. Mix until the zirconium sulfate is completely dissolved to obtain an aqueous zirconium sulfate solution. Under a nitrogen atmosphere, take 10 mL of the aqueous zirconium sulfate solution and add it to the intermediate reaction solution prepared in step P2. Continue stirring the reaction at a speed of 500 rpm. After 50 minutes, transfer the reaction system to a vacuum filtration device, filter and wash the reaction with anhydrous ethanol, wash 3 times, and freeze-dry to obtain enhanced graphene.

[0038] The enhanced graphene prepared in this example was observed for its microstructure using a Quanta-200 scanning electron microscope. Figure 1 This is a SEM image of the enhanced graphene prepared in Example 1. As shown in the figure, the enhanced graphene prepared in this example is reduced graphene oxide with abundant Ni / Zr metal nanoparticles on the surface.

[0039] This embodiment also provides a method for preparing a titanium-nickel alloy material, which specifically comprises the following steps:

[0040] S1. Accurately weigh 5 g of enhanced graphene and disperse it in 100 mL of anhydrous ethanol. Ultrasonic dispersion is performed at 400 W for 30 min to obtain enhanced graphene slurry.

[0041] S2, 2.4 g of Ti powder, 4.4 g of Ni powder, 2.4 g of Hf powder and 0.8 g of Nb powder were mixed with 15 mL of anhydrous ethanol, and mechanically stirred at 1100 rpm to form an alloy slurry;

[0042] S3, taking 1 mL of the enhanced graphene slurry prepared in step S1 and mixing it with the alloy slurry prepared in step S2, placing it in a ball mill for ball milling at a speed of 300 rpm, with a ball-to-material ratio of 4:1, and a ball milling time of 10 h, and after vacuum drying, obtaining a titanium-nickel alloy precursor powder;

[0043] S4, loading the titanium-nickel alloy precursor powder prepared in step S3 into a mold, transferring it to a vacuum sintering furnace, adjusting the vacuum sintering parameters, and performing discharge ion beam sintering; the discharge ion beam sintering parameters are as follows: setting the vacuum degree to 1 Pa, heating the temperature to 600 ° C at a heating rate of 100 ° C / min, and keeping the temperature for 5 minutes; setting the initial sintering pressure to 1 MPa, and the holding pressure to 300 MPa;

[0044] S5. After the discharge ion beam sintering treatment, the temperature is increased to 1000° C. at 10° C. / min, kept at this temperature for 10 minutes, the temperature is further increased to 1500° C., kept at this temperature for 20 minutes, the temperature is further increased to 1700° C., kept at this temperature for 5 minutes, and then naturally cooled to obtain a titanium-nickel alloy material.

[0045] The enhanced graphene prepared in this example was observed for its microstructure using a Quanta-200 scanning electron microscope. Figure 2 This is the SEM image of the sintered embryo of the nickel-titanium alloy material prepared in this embodiment. According to its microstructure, it can be seen that the graphene is evenly distributed without obvious agglomeration, indicating that the enhanced graphene can be evenly dispersed in the molten alloy material during the sintering process.

[0046] Example 2

[0047] This embodiment provides a titanium-nickel alloy material, wherein the raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 23 parts of Ti powder, 43 parts of Ni powder, 29 parts of Hf powder, 5 parts of Nb powder, and 0.8 parts of enhanced graphene;

[0048] The preparation method of enhanced graphene specifically comprises the following steps:

[0049] P1. Accurately weigh 0.25 g of graphene oxide and disperse it in 100 mL of deionized water. Transfer it to an ultrasonic processor, and ultrasonically disperse it at 400 W for 20 min. Then transfer it to a three-necked flask, fill the reaction system with N2, and bubbling it for 15 min to obtain a graphene oxide dispersion for standby use.

[0050] P2. Accurately weigh 20 g of nickel sulfate and dissolve it in 100 mL of deionized water. Mix well until the nickel sulfate is completely dissolved. Under a nitrogen atmosphere, take 12.0 mL of nickel sulfate aqueous solution and add it to the graphene oxide dispersion prepared in step P1. Use a magnetic stirrer to stir mechanically for 40 min at a speed of 400 rpm. Then, use a peristaltic pump to slowly dropwise add 25 mL of a 3 mol / L NaBH4 aqueous solution at a speed of 1 mL / min. Continue stirring for 90 min to obtain an intermediate reaction solution, which is placed under a nitrogen atmosphere for standby use.

[0051] P3. Accurately weigh 4.5 g of zirconium sulfate and dissolve it in 100 mL of deionized water. Mix until the zirconium sulfate is completely dissolved to obtain an aqueous zirconium sulfate solution. Under a nitrogen atmosphere, take 10 mL of the aqueous zirconium sulfate solution and add it to the intermediate reaction solution prepared in step P2. Continue stirring the reaction at a speed of 400 rpm. After 40 minutes, transfer the reaction system to a vacuum filtration device, filter and wash the reaction with anhydrous ethanol, wash 3 times, and freeze-dry to obtain enhanced graphene.

[0052] This embodiment also provides a method for preparing a titanium-nickel alloy material, which specifically comprises the following steps:

[0053] S1. Accurately weigh 8 g of enhanced graphene and disperse it in 100 mL of anhydrous ethanol. Ultrasonic dispersion is performed at 400 W for 30 min to obtain an enhanced graphene slurry.

[0054] S2, 2.3 g of Ti powder, 4.3 g of Ni powder, 2.9 g of Hf powder and 0.5 g of Nb powder were mixed with 15 mL of anhydrous ethanol, and mechanically stirred at 1200 rpm to form an alloy slurry;

[0055] S3, taking 1 mL of the enhanced graphene slurry prepared in step S1 and mixing it with the alloy slurry prepared in step S2, placing it in a ball mill for ball milling at a speed of 400 rpm, with a ball-to-material ratio of 4.5:1, and a ball milling time of 9 h, and after vacuum drying, obtaining a titanium-nickel alloy precursor powder;

[0056] S4, loading the titanium-nickel alloy precursor powder prepared in step S3 into a mold, transferring it to a vacuum sintering furnace, adjusting the vacuum sintering parameters, and performing discharge ion beam sintering; the discharge ion beam sintering parameters are as follows: setting the vacuum degree to 1 Pa, heating the temperature to 700 ° C at a heating rate of 100 ° C / min, and keeping the temperature for 10 min; setting the initial sintering pressure to 1 MPa, and the holding pressure to 300 MPa;

[0057] S5. After the discharge ion beam sintering treatment, the temperature is increased to 1000° C. at 10° C. / min, kept at this temperature for 10 minutes, the temperature is further increased to 1500° C., kept at this temperature for 20 minutes, the temperature is further increased to 1700° C., kept at this temperature for 5 minutes, and then naturally cooled to obtain a titanium-nickel alloy material.

[0058] Example 3

[0059] This embodiment provides a titanium-nickel alloy material, wherein the raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 24 parts of Ti powder, 45 parts of Ni powder, 19 parts of Hf powder, 11 parts of Nb powder, and 1 part of enhanced graphene;

[0060] The preparation method of enhanced graphene specifically comprises the following steps:

[0061] P1. Accurately weigh 0.3 g of graphene oxide and disperse it in 100 mL of deionized water. Transfer it to an ultrasonic processor, and ultrasonically disperse it at 400 W for 20 min. Then transfer it to a three-necked flask, fill the reaction system with N2, and bubbling it for 15 min to obtain a graphene oxide dispersion for standby use.

[0062] P2. Accurately weigh 16 g of nickel sulfate and dissolve it in 100 mL of deionized water. Mix well until the nickel sulfate is completely dissolved. Under a nitrogen atmosphere, take 20 mL of nickel sulfate aqueous solution and add it to the graphene oxide dispersion prepared in step P1. Use a magnetic stirrer to stir mechanically for 40 min at a speed of 500 rpm. Then, use a peristaltic pump to slowly drop 50 mL of a 2 mol / L NaBH4 aqueous solution at a speed of 1 mL / min. Continue stirring for 75 min to obtain an intermediate reaction solution, which is placed under a nitrogen atmosphere for standby use.

[0063] P3. Accurately weigh 3.7 g of zirconium sulfate and dissolve it in 100 mL of deionized water. Mix until the zirconium sulfate is completely dissolved to obtain an aqueous zirconium sulfate solution. Under a nitrogen atmosphere, take 15 mL of the aqueous zirconium sulfate solution and add it to the intermediate reaction solution prepared in step P2. Continue stirring the reaction at a speed of 450 rpm. After 30 minutes, transfer the reaction system to a vacuum filtration device, filter and wash the reaction with anhydrous ethanol, wash 3 times, and freeze-dry to obtain enhanced graphene.

[0064] This embodiment also provides a method for preparing a titanium-nickel alloy material, which specifically comprises the following steps:

[0065] S1. Accurately weigh 10 g of enhanced graphene and disperse it in 100 mL of anhydrous ethanol. Ultrasonic dispersion is performed at 400 W for 30 min to obtain enhanced graphene slurry.

[0066] S2, 2.4 g of Ti powder, 4.5 g of Ni powder, 2.9 g of Hf powder and 1.1 g of Nb powder were mixed with 15 mL of anhydrous ethanol, and mechanically stirred at 1000 rpm to form an alloy slurry;

[0067] S3, taking 1 mL of the enhanced graphene slurry prepared in step S1 and mixing it with the alloy slurry prepared in step S2, placing it in a ball mill for ball milling at a speed of 500 rpm, with a ball-to-material ratio of 5:1, and a ball milling time of 8 h, and after vacuum drying, obtaining a titanium-nickel alloy precursor powder;

[0068] S4, loading the titanium-nickel alloy precursor powder prepared in step S3 into a mold, transferring it to a vacuum sintering furnace, adjusting the vacuum sintering parameters, and performing discharge ion beam sintering; the discharge ion beam sintering parameters are as follows: setting the vacuum degree to 1 Pa, heating the temperature to 700 ° C at a heating rate of 100 ° C / min, and keeping the temperature for 10 min; setting the initial sintering pressure to 1 MPa, and the holding pressure to 300 MPa;

[0069] S5. After the discharge ion beam sintering treatment, the temperature is increased to 1000° C. at 10° C. / min, kept at this temperature for 10 minutes, the temperature is further increased to 1500° C., kept at this temperature for 20 minutes, the temperature is further increased to 1700° C., kept at this temperature for 5 minutes, and then naturally cooled to obtain a titanium-nickel alloy material.

[0070] Comparative Example 1

[0071] This comparative example provides a titanium-nickel alloy material and a preparation method thereof, which is different from Example 1 only in that Hf powder is included in all components, and the other components and component contents are the same as those in Example 1.

[0072] Comparative Example 2

[0073] This comparative example provides a titanium-nickel alloy material and a preparation method thereof, which is different from Example 1 only in that Nb powder is included in all components, and the other components and component contents are the same as those in Example 1.

[0074] Comparative Example 3

[0075] This comparative example provides a titanium-nickel alloy material and a preparation method thereof, which differs from Example 1 only in that the enhanced graphene is replaced by commercially available ordinary reduced graphene oxide, the brand of the reduced graphene oxide is Sigma-Aldrich, and the product number is 777684, and the remaining components and component contents are the same as those in Example 1.

[0076] Experimental Example 1

[0077] In this experimental example, the hardness of the titanium-nickel alloy materials prepared in Examples 1-3 and Comparative Examples 1-3 was tested using a HXD-1000TMC / LCD Vickers hardness tester. Figure 3The hardness result diagram of the titanium-nickel alloy materials prepared in Examples 1-3 and Comparative Examples 1-3 is shown in the figure. As shown in the figure, the hardness of the nickel-titanium alloy prepared in Examples 1-3 is significantly higher than that of Comparative Examples 1-3. The hardness of the nickel-titanium alloy prepared in Examples 1-3 is 2870 MPa, 2910 MPa, and 2860 MPa, respectively; this indicates that the technical solution of the present invention has a significant effect on improving the hardness of the alloy.

[0078] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.

[0079] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A titanium-nickel alloy material, characterized in that: The raw materials for preparing the titanium-nickel alloy material include the following components in parts by weight: 23-34 parts of Ti powder, 43-46 parts of Ni powder, 19-29 parts of Hf powder, 5-11 parts of Nb powder, and 0.5-1 part of enhanced graphene; The method for preparing the enhanced graphene specifically comprises the following steps: P1. Disperse graphene oxide in deionized water, wherein the mass concentration of graphene oxide in deionized water is 2.5-3 g / L, and subject to ultrasonic treatment at 400 W power. After 20-30 min, fill with N2, and treat for 15 min to obtain a graphene oxide dispersion for standby use. P2, prepare a nickel sulfate aqueous solution, the mass concentration of nickel sulfate in the nickel sulfate aqueous solution is 0.1-0.2g / mL, add it to the graphene oxide dispersion prepared in step P1 under a nitrogen atmosphere, the added volume of the nickel sulfate aqueous solution is 12%-20% of the volume of the graphene oxide dispersion, mechanically stir at 400-500rpm, after 30-40min, add NaBH4 solution, the molar concentration of the NaBH4 solution is 1-3mol / L, and the added volume of the NaBH4 solution is 25%-50% of the volume of the graphene oxide dispersion, continue stirring and reacting for 60-90min, obtain an intermediate reaction solution, place it under a nitrogen atmosphere, and set aside; P3. Prepare an aqueous zirconium sulfate solution, wherein the mass concentration of zirconium sulfate in the aqueous zirconium sulfate solution is 30-45 g / L, and add it to the intermediate reaction solution of step P2 under a nitrogen atmosphere, wherein the added mass of zirconium sulfate is 17.5%-23.5% of the mass of nickel sulfate, and continue stirring at a speed of 400-500 rpm for 30-50 min. Wash with anhydrous ethanol in vacuum, and freeze-dry to obtain enhanced graphene.

2. A method for preparing the titanium-nickel alloy material according to claim 1, characterized in that: The specific steps include: S1, dispersing the enhanced graphene in anhydrous ethanol, and uniformly dispersing by ultrasonication to obtain an enhanced graphene slurry; S2, mixing Ti powder, Ni powder, Hf powder and Nb powder with anhydrous ethanol, and mechanically stirring at 1000-1200 rpm to form an alloy slurry; S3, mixing the enhanced graphene slurry prepared in step S1 with the alloy slurry prepared in step S2, placing them in a ball mill for ball milling at a speed of 300-500 rpm, with a ball-to-material ratio of 4-5:1, and a ball milling time of 8-10 h, and vacuum drying to obtain a titanium-nickel alloy precursor powder; S4, loading the titanium-nickel alloy precursor powder prepared in step S3 into a mold, transferring it to a vacuum sintering furnace, adjusting the vacuum sintering parameters, and performing discharge ion beam sintering; the discharge ion beam sintering parameters are as follows: setting the vacuum degree to 1Pa, heating the temperature to 600-700°C at a heating rate of 100°C / min, and keeping the temperature for 5-10min; setting the initial sintering pressure to 1MPa, and the holding pressure to 300MPa; S5. After the discharge ion beam sintering treatment, the temperature is increased to 1000° C. at 10° C. / min, kept at this temperature for 10 minutes, the temperature is further increased to 1500° C., kept at this temperature for 20 minutes, the temperature is further increased to 1700° C., kept at this temperature for 5 minutes, and then naturally cooled to obtain a titanium-nickel alloy material.

3. The method for preparing the titanium-nickel alloy material according to claim 2, characterized in that: In step S1, the mass concentration of the enhanced graphene in anhydrous ethanol is 0.05-0.1 g / mL.

4. The method for preparing the titanium-nickel alloy material according to claim 3, characterized in that: In step S2, the material-liquid ratio of the alloy slurry is 1:1.5-2 g / mL.