A production process of hard-sealed ball valve based on laser cladding

Through laser cladding technology, the metal cermet hardened layer is prepared on the valve ball and valve seat surface of the hardened ball valve, which solves the problems of high porosity and large friction coefficient of the hardened layer on the surface of the existing hardened ball valve, and achieves high hardness and low porosity With the effect of low friction coefficient, the performance and high-temperature usage capability of hard sealed ball valves are improved.

CN118685771BActive Publication Date: 2024-11-05SICHUAN SUKE FLUID CONTROL EQUIP CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411197653.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-05
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The existing hard sealed ball valves have problems such as high porosity, low bonding strength, and large friction coefficient, which leads to easy friction wear and seal failure during the opening and closing process.

Method used

Using a hard sealed ball valve production process based on laser cladding, the hard oxide phase with diffuse distribution is formed to improve hardness and wear resistance, and layered oxidation is carried out through monoclinic and orthogonal crystal systems. The material structure reduces the friction coefficient and forms a friction reducing layer composed of multiple oxides.

Benefits of technology

A hardened layer with high hardness, high wear resistance, low porosity and low friction coefficient is achieved, which improves the performance and service temperature of hard sealed ball valves, ensuring continuous friction reduction performance at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685771B_ABST
    Figure CN118685771B_ABST
Patent Text Reader

Abstract

The present invention belongs to the fields of advanced manufacturing, new materials, surface engineering and new energy, and discloses a hard-sealed ball valve production process based on laser cladding, which is characterized in that a valve ball and a valve seat with a certain roughness are machined and preheated to prepare a metal ceramic powder, and a hardened layer is prepared on the surface of the valve ball and the valve seat based on laser cladding, and the hardness and wear resistance of the ball valve surface are improved by forming a dispersed oxide hard phase, and the friction coefficient is reduced by forming a monoclinic layered oxide and a friction-reducing layer composed of multi-component oxides formed on the surface of the laser cladding hardened layer after fine grinding, pre-oxidation and grinding to improve the wear resistance of the ball valve surface. The hard-sealed ball valve production process based on laser cladding of the present invention can not only obtain high ball valve surface hardness, high wear resistance and low friction coefficient, but also the surface hardened layer has low porosity and is metallurgically bonded to the substrate, and can be used for the production of various types of high-performance hard-sealed ball valves.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hard-sealed ball valve production process, in particular to a hard-sealed ball valve production process based on laser cladding, and belongs to the fields of advanced manufacturing, new materials, surface engineering and new energy. Background Art

[0002] In the fields of petrochemical, coal chemical, polysilicon, thermal power generation, new energy, etc., high viscosity fluids, multiphase fluids with dust and solid particles, and corrosive fluid media are often transported. In these fields, hard-sealed ball valves used to realize the on-off and flow control of pipeline systems play a very important role. In the production process of hard-sealed ball valves, the valve ball and valve seat surfaces of hard-sealed ball valves are often hardened to improve their hardness, wear resistance and service life in harsh working conditions.

[0003] CN111455306A discloses a manufacturing process of a nickel-based tungsten carbide wear-resistant coating for a metal hard-sealed ball valve, comprising the following steps: S1, workpiece surface pretreatment: cleaning and roughening the surface of the machined ball and valve seat; S2, spraying the wear-resistant coating: using a supersonic flame spraying process to evenly spray the wear-resistant coating powder material onto the surface of the ball and valve seat; S3, heating and remelting: putting the sprayed ball and valve seat into a vacuum furnace in batches for heating and remelting, so that the ball and valve seat are metallurgically bonded with the wear-resistant material; S4, cooling: after remelting, the ball and valve seat are slowly cooled with the vacuum furnace; S5, grinding: using a grinding device to sequentially perform precision grinding on the cooled ball and valve seat. CN108130533A discloses a hard-sealed ball valve with high wear resistance and corrosion resistance and a preparation method. The hard-sealed ball valve comprises a steel ball valve substrate, on which a carbide metal ceramic coating of hundreds of microns and a micro-nano-scale nitride ceramic coating are sequentially synthesized, the carbide metal ceramic coating is a WC-Co-based or high-temperature-resistant Cr3C2-NiCr-based coating, and the nitride ceramic coating is a dense Cr, Ti, AlCr or other binary or multi-component nitride multilayer coating, and a preparation method thereof comprises adopting supersonic flame spraying and vacuum ion plating methods to sequentially synthesize a metal ceramic hardening layer and a nitride multilayer sealing layer on the surface of the ball valve.

[0004] In the current hard-sealed ball valve production process, after the surface of the valve ball and valve seat is hardened, its surface hardness increases and its wear resistance improves, but there are still problems such as high porosity, low bonding strength, and high friction coefficient of the surface hardened layer. During the opening and closing process of the hard-sealed ball valve, there is high contact stress between the valve ball and the valve seat sealing surface, which is very easy to cause friction and wear or even fall off, causing sealing failure. Therefore, it is urgent to develop a new hard-sealed ball valve production process to obtain a hardened layer with high hardness, high wear resistance, high bonding strength, low porosity and low friction coefficient to improve the performance of the hard-sealed ball valve. Summary of the invention

[0005] The present invention aims to provide a hard-sealed ball valve production process based on laser cladding, which meets the comprehensive requirements of high hardness, high wear resistance, high bonding strength, low porosity and low friction coefficient of the surface hardened layer of the hard-sealed ball valve under increasingly stringent working conditions. The present invention proposes to prepare metal ceramic powder, and prepare a hardened layer on the surface of the valve ball and valve seat based on laser cladding technology, and improve the surface hardness and wear resistance of the ball valve by forming a dispersed oxide hard phase, and use the formed monoclinic layered oxide and the friction-reducing layer composed of multi-element oxides formed on the surface of the laser cladding hardened layer after fine grinding, pre-oxidation and grinding to reduce the friction coefficient and improve the wear resistance of the ball valve surface.

[0006] The laser cladding-based hard-sealed ball valve production process of the present invention comprises the following steps:

[0007] (1) Preparation of monoclinic friction-reducing components of laser cladding hardening layer: Co(NO3)2·6H2O and NH4VO3 were weighed in a molar ratio of (1-2):9 and added into deionized water to prepare a solution. The concentration of NH4VO3 in the solution was 1-2 mol / L. The solution was magnetically stirred in a constant temperature water bath at 60-70℃ for 30 min, and then ammonia water was added to adjust the pH value to 7.5-8. The solution was stirred for 1-2 h and allowed to stand for 2-3 h to form a Co-containing 2+ V(OH)5 sol; weigh Ni(NO3)2 and add it into deionized water to prepare a solution with a molar concentration of 0.5~1mol / L. After magnetic stirring for 30min in a constant temperature water bath at 60~70℃, add ammonia water to adjust the pH value to 8~9, stir for 1~2h and leave for 2~3h to form Ni(OH)2 sol; weigh Ni(OH)2 sol and Co-containing sol according to the molar ratio of Ni:V element of 1:1 2+ V(OH)5 sol, and Ni(OH)2 sol was added dropwise to the Co 2+ The V(OH)5 sol was added dropwise in a constant temperature water bath at 60-70°C while being magnetically stirred, dried at 100-120°C for 1 h, and then calcined at 700-750°C for 1-2 h to prepare a Co-containing NiO-coated surface. 2+ The V2O5 nanopowder is used as the monoclinic anti-friction component of the laser cladding hardening layer; the particle size of the monoclinic anti-friction component of the laser cladding hardening layer is 40~90nm, the surface is a 10~30nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure of V2O5, Co 2+ Embedded in the interlayer of V2O5 layered structure, the interlayer spacing is from no Co 2+ The 0.437nm during embedding increases to 0.46~0.48nm, which weakens the interlayer van der Waals force and promotes interlayer sliding;

[0008] (2) Preparation of orthorhombic friction reducing component precursor of laser cladding hardening layer: Mo powder with a Fisher particle size of 0.5-1.0 μm was weighed and added to anhydrous ethanol. Ultrasonic dispersion treatment was performed for 20-40 min. The ultrasonic frequency and power were 40 kHz and 100 W, respectively, to prepare a mixed solution A with a concentration of 1-3 mol / L; Ti(OC4H9)4 was weighed and added to anhydrous ethanol and magnetically stirred for 10-20 min to prepare a solution B with a molar concentration of 0.5-1 mol / L; anhydrous ethanol and deionized water were mixed in a volume ratio of 1:1, and hydrochloric acid was added dropwise while magnetically stirring until the pH value was 3-4 to prepare a solution C; solution B was added dropwise to solution C at room temperature and magnetic stirring was maintained. After stirring, the mixture was allowed to stand for 1-2 hours. h, Ti(OH)4 sol is prepared; Ti(OH)4 sol and mixed solution A are weighed according to the Ti:Mo element molar ratio of 1:1, and Ti(OH)4 sol is added dropwise to the mixed solution A while maintaining magnetic stirring, and the mixture is placed for 1~2h and dried at 300~350℃ for 1~2h, so that Mo powder with surface coated with TiO2 is prepared as the precursor of the orthorhombic system friction reducing component of the laser cladding hardening layer, and the surface TiO2 coating layer is anatase structure with a thickness of 10~30nm;

[0009] (3) Preparation of metal ceramic agglomerates for laser cladding hardening treatment: Raw material powders are weighed according to molar percentage, of which Ni powder accounts for 32-37%, Cr powder accounts for 4-10%, monoclinic friction reducing component of laser cladding hardening layer accounts for 2-5%, precursor of orthorhombic friction reducing component of laser cladding hardening layer accounts for 1-3%, and the rest is Cr3C2 powder; the weighed raw material powders are subjected to planetary ball milling at a ball milling speed of 300-400 r / min, using Al2O3 ceramic grinding balls with a diameter of 5 mm, a ball-to-material ratio of 10:1, and anhydrous ethanol and PEG2000 forming agent. The mass ratios of the added amount to the raw material powder are 0.25:1 and 0.03:1 respectively, the ball milling time is 24-48h, and the slurry is filtered through a 400-mesh screen after the ball milling. The filtered slurry is spray dried at 110-130°C, and the speed of the atomizing disk during spray drying is 4000-7000r / min. The sintering is vacuum sintered at 1100-1200°C, and the sintering vacuum degree is 1-10Pa. After the vacuum sintering is completed, the slurry is cooled with the furnace, and crushed and airflow graded. During the sintering process, the NiO in the monoclinic friction reducing component of the laser cladding hardening layer is reduced and a Co-containing Ni-coated surface is formed. 2+ The V2O5 nanoparticles are prepared by laser cladding hardening treatment. The surface TiO2 in the orthorhombic friction reducing component precursor of the laser cladding hardening layer undergoes a solid solution reaction with Mo to form (Ti,Mo)O2 and Mo coated with (Ti,Mo)O2 on the surface. The average particle size of the prepared metal ceramic agglomerates for laser cladding hardening treatment is 30~45μm, and its composition is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo;

[0010] (4) Preparation of metal ceramic powder for laser cladding hardening treatment: first, Tween 80, n-butanol, and n-hexane were added to deionized water, with Tween 80 accounting for 16% to 33% by weight, n-butanol accounting for 7% to 14%, n-hexane accounting for 5% to 16%, and the rest being ionized water. Stir with a magnetic stirrer at 60 to 80 °C for 1 to 3 h, and then place for 3 to 6 h to form a reverse microemulsion. Ni(NO3)2 and Al(NO3)3 were weighed in a molar ratio of 1:1, and added to the reverse microemulsion to prepare a solution with a molar concentration of 0.1 to 0.5 mol / L. Ammonia water was then added to adjust the pH value of the solution to 8 to 9. Stir with a magnetic stirrer at 60 to 70 °C for 3 to 12 h. Then, the mixture was allowed to stand for 6 to 8 hours to form Ni(OH)2 sol and Al(OH)3 sol. Ni(OH)2 sol was added dropwise to Al(NO3)3 sol, and the mixture was added dropwise while being magnetically stirred in a constant temperature water bath at 60 to 70°C to form a composite sol of Ni(OH)2 coated with Al(OH)3. The composite sol of Ni(OH)2 coated with Al(OH)3 and metal ceramic agglomerates for laser cladding hardening treatment were weighed in a weight percentage of 0.5:10 to 1:10, and the metal ceramic agglomerates for laser cladding hardening treatment were completely immersed in Ni(OH)2 The composite sol coated with Al(OH)3 was placed in an electric vacuum drying oven for adsorption and drying treatment. The vacuum degree was ≤150Pa. It was first kept at 50-60℃ for 1-2h to allow the composite sol to be completely adsorbed into the pores of the metal ceramic agglomerates. Then it was dried at 110-120℃ for 2-3h. The composite sol was transformed into a composite gel of Ni(OH)2 coated with Al(OH)3. The average particle size of the prepared metal ceramic powder for laser cladding hardening treatment was 30-47μm, and its composition was Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo+ Ni(OH)2 gel+Al(OH)3 gel;

[0011] (5) Grinding and preheating treatment of valve ball and valve seat: The valve ball and valve seat substrate are manufactured by mechanical processing, and then the surface is pretreated by grinding to make the surface roughness Ra0.8~1.6μm; then the valve ball and valve seat are placed in a muffle furnace for preheating treatment, the preheating rate of the preheating treatment is 5~10℃ / min, the preheating temperature is 200~300℃, and the insulation time is 5~30min;

[0012] (6) Laser cladding hardening treatment of valve ball and valve seat surface: The prepared metal ceramic powder is used to perform laser cladding hardening treatment on the valve ball and valve seat surface that have completed the preheating treatment. The laser cladding treatment starts within 3 minutes after the valve ball and valve seat complete the preheating treatment. During laser cladding, laser coaxial argon gas is used to protect the hardened layer from oxidation, and the argon gas flow rate is 1~2L / min. The metal ceramic powder is laid on the surface of the valve ball and valve seat by side-axis powder feeding. The powder feeding rate is 12~15g / min, and the angle between the metal ceramic powder flow direction and the laser optical axis is 45~50°. The laser output power is 1200~1600W, the laser spot diameter is 2~5mm, the rotation speed of the valve ball and valve seat is 3~5r / min, and the laser cladding overlap rate is 40~60%; the formed laser cladding hardened layer contains Co 2+ The V2O5 surface is still coated by the Ni layer without carbonization. The (Ti,Mo)O2 on the Mo surface is carbonized to form (Ti,Mo)C, while the Mo in the core is not carbonized. The gel of Ni(OH)2 coated Al(OH)3 is transformed into Ni-coated nano-Al2O3. The thickness of the laser cladding hardened layer is 700~1200μm, the hardness is ≧950HV, the bonding strength of the coating is ≧400MPa, the porosity is ≤0.5%, and the phase is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)C+Mo+Al2O3; the laser cladding hardened layer is metallurgically bonded with the valve ball and valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo;

[0013] (7) Formation of anti-friction layer on the surface of valve ball and valve seat and manufacturing of hard-sealed ball valve: The surface of the valve ball and valve seat after laser cladding hardening treatment is roughly ground to make the roughness of the surface hardened layer Ra0.6~0.8μm; then the valve ball and valve seat are placed in a vacuum furnace for argon-oxygen mixed atmosphere treatment, and the initial vacuum degree of the atmosphere treatment is ≤5×10 -2 Pa, heated to 450~500℃, then filled with argon-oxygen mixed gas containing 5% oxygen and controlled the gas pressure to 2~5Pa, kept warm for 1~2h and cooled with the furnace, the Mo element on the surface of the laser cladding hardened layer is transformed into orthorhombic α-MoO3, the surface Ti element is transformed into anatase TiO2, and the other phases remain unchanged; after cooling out of the furnace, the valve ball and valve seat are ground to a surface roughness of Ra0.2~0.4μm, and after the grinding is completed, a 0.1~0.2μm thick layer is formed on the surface of the laser cladding hardened layer, which is composed of Co 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2. After the valve ball and valve seat surface are hardened and the friction reduction layer is formed, the friction coefficient is 0.08~0.12, and the wear rate is ≦5×10 -6 mm3 / (N·mm), the maximum service temperature is 660℃; finally, the valve ball and valve seat with the anti-friction layer formed on the surface are assembled with the matching valve body, valve stem, spring and bearing to manufacture the hard-sealed ball valve.

[0014] The hard sealing ball valve based on laser cladding of the present invention has a phase of Cr3C2+NiCr solid solution+Ni+Co-containing on the surface of the valve ball and valve seat substrate. 2+ The laser cladding hardened layer is composed of V2O5+(Ti,Mo)C+Mo+Al2O3; the thickness of the laser cladding hardened layer is 700~1200μm, the hardness is ≧950HV, the coating bonding strength is ≧400MPa, and the porosity is ≤0.5%; the raw materials of the laser cladding hardened layer are composed of a composite gel of Ni(OH)2 coated with Al(OH)3 and a metal ceramic agglomerate with a weight percentage of 0.5:10~1:10, wherein the molar ratio of the elements in the composite gel is Ni:Al=1:1, and the metal ceramic agglomerate has a molar percentage of Ni powder of 32~37%, Cr powder of 4~10%, and Co-containing NiO coated on the surface 2+ V2O5 powder accounts for 2~5%, Mo powder coated with TiO2 accounts for 1~3%, and the rest is Cr3C2 powder; Co-containing powder coated with NiO accounts for 1~3%. 2+ The molar ratio of the elements in the V2O5 powder is Ni:V:Co=9:9:1, the particle size is 40~90nm, the surface is a 10~30nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure with Co embedded in the interlayer. 2+ V2O5; the molar ratio of the elements in the Mo coated with TiO2 on the surface is Ti:Mo=1:1, and the TiO2 coating layer on the surface is anatase structure with a thickness of 10~30nm; the laser cladding hardened layer is metallurgically bonded to the valve ball and valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo; the surface of the laser cladding hardened layer is composed of Co-containing 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2, with a thickness of 0.1~0.2μm; the friction coefficient between the valve ball and the valve seat is 0.08~0.12, and the wear rate is ≦5×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃.

[0015] The beneficial effects of the present invention are:

[0016] (1) The valve ball and valve seat are ground to control the roughness, which can increase the contact area between the laser cladding layer and the substrate and improve the bonding strength;

[0017] (2) Preheating the valve ball and valve seat can reduce the temperature difference, reduce residual stress, increase the reactivity of the substrate to form a transition zone, and thus improve the bonding strength between the coating and the substrate;

[0018] (3) The present invention embeds Co element into the layered V2O5 in the hardened layer on the surface of the valve ball and valve seat in the hard-sealed ball valve produced by laser cladding, thereby increasing the interlayer distance, thereby promoting interlayer sliding and improving friction reduction performance;

[0019] (4) Directly adding V2O5 to the hardened layer on the surface of the valve ball and valve seat will cause the V2O5 to react and its structure to be destroyed during the coating process. In the present invention, after the surface of V2O5 is coated with NiO, NiO is reduced during the preparation of the agglomerate and laser cladding process to prevent V2O5 from being carbonized, thereby maintaining its layered structure to play a role in reducing friction;

[0020] (5) Directly adding Mo to the hardened layer on the surface of the valve ball and valve seat will cause Mo to be carbonized or to undergo a solid solution reaction with Cr3C2 during the laser cladding process and the structure to be destroyed. In the present invention, after the Mo surface is coated with TiO2, (Ti, Mo)O2 and (Ti, Mo)C are formed during the preparation of the agglomerate and the laser cladding process to avoid Mo from being carbonized, so that it can be oxidized in an argon oxygen atmosphere after laser cladding to form α-MoO3 with a layered structure;

[0021] (6) The composite sol of Ni(OH)2 coated Al(OH)3 is impregnated into the metal ceramic agglomerate, and finally Ni-coated nano-Al2O3 is formed, which can fill the voids and improve the interface wettability, thereby reducing the porosity of the coating. In addition, the formed nano-Al2O3 has a dispersion strengthening effect on the coating, which can improve the hardness and wear resistance of the coating.

[0022] (7) After laser cladding treatment, MoO3 is pre-oxidized in the atmosphere and then subjected to grinding treatment to form a multi-component anti-friction layer to achieve the effect of anti-friction;

[0023] (8) The hard-sealed ball valve produced by laser cladding has high hardness, good wear resistance, low porosity, metallurgical bonding between the hardened layer and the substrate, high service temperature, and in addition to the initial surface friction reduction layer, the hardened layer contains Co 2+ V2O5 can reduce the friction coefficient. During the friction process and oxidation conditions, Mo and Ti elements can form oxides and form a composite anti-friction layer with V2O5, ensuring continuous anti-friction performance at high service temperatures. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the production process of a hard-sealed ball valve based on laser cladding of the present invention.

[0025] Figure 2Schematic diagram of valve ball and valve seat characteristics of a hard-sealed ball valve produced based on laser cladding of the present invention. DETAILED DESCRIPTION

[0026] Embodiment 1:

[0027] A hard-sealed ball valve production process based on laser cladding, such as Figure 1 As shown, the following steps are included in sequence:

[0028] (1) Preparation of monoclinic friction-reducing components of laser cladding hardening layer: Co(NO3)2·6H2O and NH4VO3 were weighed in a molar ratio of 1:9 and added into deionized water to prepare a solution. The concentration of NH4VO3 in the solution was 1.1 mol / L. The solution was magnetically stirred in a constant temperature water bath at 60°C for 30 min, and then ammonia water was added to adjust the pH value to 7.5. The solution was stirred for 1 h and allowed to stand for 2 h to form a Co-containing 2+ V(OH)5 sol; weigh Ni(NO3)2 and add it into deionized water to prepare a solution with a molar concentration of 0.6 mol / L. After magnetic stirring in a constant temperature water bath at 65°C for 30 min, add ammonia water to adjust the pH value to 8, stir for 1 h and leave it for 2 h to form Ni(OH)2 sol; weigh Ni(OH)2 sol and Co-containing sol according to the molar ratio of Ni:V element of 1:1 2+ V(OH)5 sol, and Ni(OH)2 sol was added dropwise to the Co 2+ The V(OH)5 sol was added dropwise in a 60°C constant temperature water bath while being magnetically stirred, dried at 110°C for 1 hour, and then calcined at 710°C for 1 hour to prepare a Co-containing NiO-coated 2+ V2O5 nanopowder is used as the monoclinic anti-friction component of the laser cladding hardening layer; the particle size of the monoclinic anti-friction component of the laser cladding hardening layer is 42nm, the surface is a 12nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure of V2O5, Co 2+ Embedded in the interlayer of V2O5 layered structure, the interlayer spacing is from no Co 2+ The increase from 0.437nm to 0.468nm during embedding weakens the interlayer van der Waals force, thus promoting interlayer sliding;

[0029] (2) Preparation of orthorhombic friction reducing component precursor of laser cladding hardening layer: Mo powder with a Fresnel particle size of 0.6 μm was weighed and added to anhydrous ethanol, and ultrasonic dispersion was performed for 25 min. The ultrasonic frequency and power were 40 kHz and 100 kHz respectively. W, thereby preparing a mixed solution A with a concentration of 1.2 mol / L; weigh Ti(OC4H9)4, add it to anhydrous ethanol and stir it magnetically for 10 minutes to prepare a solution B with a molar concentration of 0.6 mol / L; mix anhydrous ethanol and deionized water in a volume ratio of 1:1, add hydrochloric acid dropwise to a pH value of 3 while stirring magnetically, and prepare a solution C; at room temperature, add solution B dropwise to solution C and keep stirring magnetically, and after the stirring is completed, let it stand for 1 hour to prepare Ti(OH)4 sol; weigh Ti(OH)4 sol and mixed solution A according to a Ti:Mo element molar ratio of 1:1, and add Ti(OH)4 sol dropwise to mixed solution A and keep stirring magnetically, let it stand for 1 hour and dry it at 320℃ for 1 hour, so as to prepare Mo powder with surface coated with TiO2 as a precursor of the orthorhombic system friction reducing component of the laser cladding hardening layer, and its surface TiO2 coating layer is an rutile structure with a thickness of 13nm;

[0030] (3) Preparation of metal ceramic agglomerates for laser cladding hardening treatment: Raw material powders were weighed according to molar percentage, of which Ni powder accounted for 32%, Cr powder accounted for 5%, monoclinic friction reducing component of laser cladding hardening layer accounted for 3%, orthorhombic friction reducing component precursor of laser cladding hardening layer accounted for 1%, and the rest was Cr3C2 powder; the weighed raw material powders were planetary ball milled at a ball milling speed of 300 r / min, using Al2O3 ceramic grinding balls with a diameter of 5 mm, a ball-to-material ratio of 10:1, and anhydrous ethanol and PEG2000. The mass ratio of the forming agent to the raw material powder is 0.25:1 and 0.03:1 respectively. The ball milling time is 30h. After the ball milling, it is filtered with a 400-mesh screen. The filtered slurry is spray-dried at 110°C. The speed of the atomizer disk during spray drying is 4500r / min. It is vacuum sintered at 110°C with a sintering vacuum degree of 2Pa. After the vacuum sintering, it is cooled in the furnace and crushed and airflow graded. During the sintering process, the NiO in the monoclinic friction reducing component of the laser cladding hardening layer is reduced and a Co-containing Ni-coated surface is formed. 2+ The V2O5 nanoparticles are prepared by laser cladding hardening treatment. The surface TiO2 in the orthorhombic friction reducing component precursor of the laser cladding hardening layer undergoes a solid solution reaction with Mo to form (Ti,Mo)O2 and Mo coated with (Ti,Mo)O2 on the surface. The average particle size of the prepared metal ceramic agglomerate for laser cladding hardening treatment is 42μm, and its composition is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo;

[0031] (4) Preparation of metal ceramic powder for laser cladding hardening treatment: first, Tween 80, n-butanol, and n-hexane were added to deionized water, with Tween 80 accounting for 17%, n-butanol accounting for 8%, and n-hexane accounting for 5%, and the rest being ionized water. The mixture was stirred at 60°C for 2 h using a magnetic stirrer, and then allowed to stand for 3 h to form a reverse microemulsion. Ni(NO3)2 and Al(NO3)3 were weighed at a molar ratio of 1:1, and added to the reverse microemulsion to prepare a solution with a molar concentration of 0.2 mol / L. Ammonia water was then added to adjust the pH value of the solution to 8. The mixture was stirred at 60°C for 4 h using a magnetic stirrer. Then, the mixture was allowed to stand for 6 hours to form Ni(OH)2 sol and Al(OH)3 sol. Ni(OH)2 sol was added dropwise to Al(NO3)3 sol, and the mixture was added dropwise while being magnetically stirred in a constant temperature water bath at 65°C to form a composite sol of Ni(OH)2 coated with Al(OH)3. The composite sol of Ni(OH)2 coated with Al(OH)3 and metal ceramic agglomerates for laser cladding hardening treatment were weighed in a weight percentage of 0.5:10, and the metal ceramic agglomerates for laser cladding hardening treatment were completely immersed in Ni(O The composite sol of Ni(OH)2 coated Al(OH)3 was prepared and placed in an electric vacuum drying oven for adsorption and drying treatment. The vacuum degree was 140Pa. The composite sol was first kept at 50°C for 1h to allow the composite sol to be completely adsorbed into the pores of the metal ceramic agglomerates. Then, the composite sol was dried at 110°C for 2h to transform into a composite gel of Ni(OH)2 coated Al(OH)3. The average particle size of the prepared metal ceramic powder for laser cladding hardening treatment was 43μm, and its composition was Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo+Ni(OH)2 gel+Al(OH)3 gel;

[0032] (5) Grinding and preheating treatment of valve ball and valve seat: The valve ball and valve seat substrate are manufactured by mechanical processing, and then the surface is pretreated by grinding to make the surface roughness Ra1.4μm; then the valve ball and valve seat are placed in a muffle furnace for preheating treatment, the preheating rate of the preheating treatment is 5℃ / min, the preheating temperature is 200℃, and the holding time is 10min;

[0033] (6) Laser cladding hardening treatment of valve ball and valve seat surface: The prepared metal ceramic powder is used to perform laser cladding hardening treatment on the valve ball and valve seat surface that have completed the preheating treatment. The laser cladding treatment starts within 3 minutes after the valve ball and valve seat complete the preheating treatment. During laser cladding, laser coaxial argon gas is used to protect the hardened layer from oxidation. The argon gas flow rate is 1L / min. The metal ceramic powder is laid on the surface of the valve ball and valve seat by side-axis powder feeding. The powder feeding rate is 12g / min, and the angle between the metal ceramic powder flow direction and the laser optical axis is 45°. The laser output power is 1300W, the laser spot diameter is 2mm, the rotation speed of the valve ball and valve seat is 3r / min, and the laser cladding overlap rate is 45%; the formed laser cladding hardened layer contains Co 2+ The V2O5 surface is still coated by the Ni layer without carbonization. The (Ti,Mo)O2 on the Mo surface is carbonized to form (Ti,Mo)C, while the Mo in the core is not carbonized. The gel of Ni(OH)2 coated Al(OH)3 is transformed into Ni-coated nano-Al2O3. The thickness of the laser cladding hardened layer is 1130μm, the hardness is 980HV, the bonding strength of the coating is 420MPa, the porosity is 0.3%, and the phase is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)C+Mo+Al2O3; the laser cladding hardened layer is metallurgically bonded with the valve ball and valve seat substrate, and there is a transition zone with a thickness of 42μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo;

[0034] (7) Formation of anti-friction layer on the surface of valve ball and valve seat and manufacturing of hard-sealed ball valve: The surface of the valve ball and valve seat after laser cladding hardening treatment is roughly ground to make the roughness of the surface hardened layer Ra0.8μm; then the valve ball and valve seat are placed in a vacuum furnace for argon-oxygen mixed atmosphere treatment, and the initial vacuum degree of the atmosphere treatment is 2×10 -2 Pa, heated to 450 ° C and then filled with argon oxygen mixed gas containing 5% oxygen and controlled the gas pressure to 3Pa, kept warm for 1h and cooled with the furnace, the Mo element on the surface of the laser cladding hardened layer was transformed into orthorhombic α-MoO3, the surface Ti element was transformed into anatase TiO2, and the other phases remained unchanged; after cooling out of the furnace, the valve ball and valve seat were ground to a surface roughness of Ra0.4μm. After the grinding was completed, a 0.1μm thick layer was formed on the surface of the laser cladding hardened layer, which was composed of Co 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2; after the valve ball and valve seat surface are hardened and the friction reduction layer is formed, the friction coefficient is 0.11 and the wear rate is 4×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃, the characteristic diagram of valve ball and valve seat is as follows Figure 2As shown; finally, the valve ball and valve seat with the anti-friction layer formed on the surface are assembled with the matching valve body, valve stem, spring and bearing to manufacture the hard-sealed ball valve.

[0035] The hard sealing ball valve based on laser cladding of the present invention has a phase of Cr3C2+NiCr solid solution+Ni+Co-containing on the surface of the valve ball and valve seat substrate. 2+ The laser cladding hardened layer is composed of V2O5+(Ti,Mo)C+Mo+Al2O3; the thickness of the laser cladding hardened layer is 1130μm, the hardness is 980HV, the coating bonding strength is 420MPa, and the porosity is 0.3%; the raw materials of the hardened layer are composed of a composite gel of Ni(OH)2 coated with Al(OH)3 and metal ceramic agglomerates with a weight percentage of 0.5:10, wherein the molar ratio of the elements in the composite gel is Ni:Al=1:1, and the metal ceramic agglomerates have a molar percentage of Ni powder of 32%, Cr powder of 5%, and Co-containing powder coated with NiO on the surface. 2+ V2O5 powder accounts for 3%, Mo powder coated with TiO2 accounts for 1%, and the rest is Cr3C2 powder; Co-containing powder coated with NiO accounts for 1%. 2+ The molar ratio of the elements in the V2O5 powder is Ni:V:Co=9:9:1, the particle size is 42nm, the surface is a 12nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure with Co embedded in the interlayer. 2+ V2O5; the molar ratio of the elements in the Mo coated with TiO2 on the surface is Ti:Mo=1:1, and the TiO2 coating layer on the surface is anatase structure with a thickness of 13nm; the laser cladding hardened layer is metallurgically bonded to the valve ball and valve seat substrate, and there is a transition zone with a thickness of 42μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo; the surface of the laser cladding hardened layer is composed of Co-containing 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2, with a thickness of 0.1μm; the friction coefficient between the valve ball and the valve seat is 0.11, and the wear rate is 4×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃.

[0036] Embodiment 2:

[0037] A hard-sealed ball valve production process based on laser cladding, such as Figure 1 As shown, the following steps are included in sequence:

[0038] (1) Preparation of monoclinic friction-reducing components of laser cladding hardened layer: Co(NO3)2·6H2O and NH4VO3 were weighed in a molar ratio of 1.7:9 and added to deionized water to prepare a solution. The concentration of NH4VO3 in the solution was 1.6 mol / L. The solution was magnetically stirred in a constant temperature water bath at 70°C for 30 min, and then ammonia water was added to adjust the pH value to 8. The solution was stirred for 1.5 h and allowed to stand for 3 h to form a Co-containing 2+ V(OH)5 sol; weigh Ni(NO3)2 and add it into deionized water to prepare a solution with a molar concentration of 0.7 mol / L. After magnetic stirring in a constant temperature water bath at 65°C for 30 min, add ammonia water to adjust the pH value to 9, stir for 1 h and leave for 3 h to form Ni(OH)2 sol; weigh Ni(OH)2 sol and Co-containing sol according to the molar ratio of Ni:V element of 1:1 2+ V(OH)5 sol, and Ni(OH)2 sol was added dropwise to the Co 2+ The V(OH)5 sol was added dropwise in a 65°C constant temperature water bath while being magnetically stirred, dried at 120°C for 1 h, and then calcined at 750°C for 1.5 h to prepare a Co-containing NiO-coated 2+ V2O5 nanopowder is used as the monoclinic anti-friction component of the laser cladding hardening layer; the particle size of the monoclinic anti-friction component of the laser cladding hardening layer is 81nm, the surface is a 25nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure of V2O5, Co 2+ Embedded in the interlayer of V2O5 layered structure, the interlayer spacing is from no Co 2+ The increase from 0.437nm to 0.472nm during embedding weakens the interlayer van der Waals force, thus promoting interlayer sliding;

[0039] (2) Preparation of orthorhombic friction reducing component precursor of laser cladding hardening layer: Mo powder with a Fresnel particle size of 0.8 μm was weighed and added to anhydrous ethanol, and ultrasonic dispersion was performed for 30 min. The ultrasonic frequency and power were 40 kHz and 100 kHz respectively. W, thereby preparing a mixed solution A with a concentration of 2 mol / L; weigh Ti(OC4H9)4, add it to anhydrous ethanol and stir it magnetically for 15 minutes to prepare a solution B with a molar concentration of 0.7 mol / L; mix anhydrous ethanol and deionized water in a volume ratio of 1:1, add hydrochloric acid dropwise to a pH value of 4 while stirring magnetically, and prepare a solution C; at room temperature, add solution B dropwise to solution C and keep stirring magnetically, and after the stirring is completed, let it stand for 2 hours to prepare Ti(OH)4 sol; weigh Ti(OH)4 sol and mixed solution A according to a Ti:Mo element molar ratio of 1:1, and add Ti(OH)4 sol dropwise to mixed solution A and keep stirring magnetically, let it stand for 1.5 hours and dry it at 340℃ for 1.5 hours to prepare Mo powder with surface coated with TiO2 as a precursor of the orthorhombic system friction reducing component of the laser cladding hardening layer, and its surface TiO2 coating layer is an rutile structure with a thickness of 22nm;

[0040] (3) Preparation of metal ceramic agglomerates for laser cladding hardening treatment: Raw material powders were weighed in molar percentage, of which Ni powder accounted for 36%, Cr powder accounted for 10%, monoclinic friction reducing component of laser cladding hardening layer accounted for 4%, orthorhombic friction reducing component precursor of laser cladding hardening layer accounted for 2%, and the rest was Cr3C2 powder; the weighed raw material powders were planetary ball milled at a ball milling speed of 380 r / min, using Al2O3 ceramic grinding balls with a diameter of 5 mm, a ball-to-material ratio of 10:1, and anhydrous ethanol and PEG2000. The mass ratio of the forming agent to the raw material powder is 0.25:1 and 0.03:1 respectively. The ball milling time is 40 hours. After the ball milling, it is filtered with a 400-mesh screen. The filtered slurry is spray-dried at 120°C. The speed of the atomizer disk during spray drying is 6000r / min. It is vacuum sintered at 1200°C with a sintering vacuum degree of 8Pa. After the vacuum sintering, it is cooled in the furnace and crushed and airflow graded. During the sintering process, the NiO in the monoclinic friction-reducing component of the laser cladding hardening layer is reduced and a Co-containing Ni-coated surface is formed. 2+ The V2O5 nanoparticles are prepared by laser cladding hardening treatment. The surface TiO2 in the orthorhombic friction reducing component precursor of the laser cladding hardening layer undergoes a solid solution reaction with Mo to form (Ti,Mo)O2 and Mo coated with (Ti,Mo)O2 on the surface. The average particle size of the prepared metal ceramic agglomerate for laser cladding hardening treatment is 35μm, and its composition is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo;

[0041] (4) Preparation of metal ceramic powder for laser cladding hardening treatment: first, Tween 80, n-butanol, and n-hexane were added to deionized water, with Tween 80 accounting for 30%, n-butanol accounting for 12%, n-hexane accounting for 11%, and the rest being ionized water. The mixture was stirred at 70°C for 2 h using a magnetic stirrer and then allowed to stand for 5 h to form a reverse microemulsion. Ni(NO3)2 and Al(NO3)3 were weighed at a molar ratio of 1:1 and added to the reverse microemulsion to prepare a solution with a molar concentration of 0.4 mol / L. Ammonia water was then added to adjust the pH value of the solution to 9. The mixture was stirred at 70°C for 10 h using a magnetic stirrer. Then, the mixture was allowed to stand for 7 hours to form Ni(OH)2 sol and Al(OH)3 sol. Ni(OH)2 sol was added dropwise to Al(NO3)3 sol, and the mixture was added dropwise while being magnetically stirred in a 70°C constant temperature water bath to form a composite sol of Ni(OH)2 coated with Al(OH)3. The composite sol of Ni(OH)2 coated with Al(OH)3 and metal ceramic agglomerates for laser cladding hardening treatment were weighed in a weight percentage of 0.8:10, and the metal ceramic agglomerates for laser cladding hardening treatment were completely immersed in Ni(OH )2 coated Al(OH)3 composite sol, and put it into an electric vacuum drying oven for adsorption and drying treatment, the vacuum degree is 120Pa, first keep it at 60℃ for 2h, so that the composite sol is completely adsorbed into the pores of the metal ceramic agglomerates, and then dry it at 120℃ for 2.5h, the composite sol is transformed into a composite gel of Ni(OH)2 coated Al(OH)3, the average particle size of the prepared metal ceramic powder for laser cladding hardening treatment is 36μm, and its composition is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo+ Ni(OH)2 gel+Al(OH)3 gel;

[0042] (5) Grinding and preheating treatment of valve ball and valve seat: The valve ball and valve seat substrate are manufactured by mechanical processing, and then the surface is pretreated by grinding to make its surface roughness Ra0.8μm; then the valve ball and valve seat are placed in a muffle furnace for preheating treatment, the preheating rate of the preheating treatment is 10℃ / min, the preheating temperature is 280℃, and the insulation time is 20min;

[0043] (6) Laser cladding hardening treatment of valve ball and valve seat surface: The prepared metal ceramic powder is used to perform laser cladding hardening treatment on the valve ball and valve seat surface that have completed the preheating treatment. The laser cladding treatment starts within 3 minutes after the valve ball and valve seat complete the preheating treatment. During laser cladding, laser coaxial argon gas is used to protect the hardened layer from oxidation. The argon gas flow rate is 2L / min. The metal ceramic powder is laid on the surface of the valve ball and valve seat by side-axis powder feeding. The powder feeding rate is 14g / min, and the angle between the metal ceramic powder flow direction and the laser optical axis is 50°. The laser output power is 1500W, the laser spot diameter is 4mm, the rotation speed of the valve ball and valve seat is 5r / min, and the laser cladding overlap rate is 55%; the formed laser cladding hardened layer contains Co 2+ The V2O5 surface is still coated by the Ni layer without carbonization. The (Ti,Mo)O2 on the Mo surface is carbonized to form (Ti,Mo)C, while the Mo in the core is not carbonized. The gel of Ni(OH)2 coated Al(OH)3 is transformed into Ni-coated nano-Al2O3. The thickness of the laser cladding hardened layer is 780μm, the hardness is 960HV, the bonding strength of the coating is 430MPa, the porosity is 0.1%, and the phase is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)C+Mo+Al2O3; the laser cladding hardened layer is metallurgically bonded with the valve ball and valve seat substrate, and there is a transition zone with a thickness of 48μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo;

[0044] (7) Formation of anti-friction layer on the surface of valve ball and valve seat and manufacturing of hard-sealed ball valve: The surface of the valve ball and valve seat after laser cladding hardening treatment is roughly ground to make the roughness of the surface hardened layer Ra0.6μm; then the valve ball and valve seat are placed in a vacuum furnace for argon-oxygen mixed atmosphere treatment, and the initial vacuum degree of the atmosphere treatment is 1×10 -2 Pa, heated to 500 ° C and then filled with argon oxygen mixed gas containing 5% oxygen and controlled the gas pressure to 4Pa, kept warm for 2 hours and then cooled with the furnace, the Mo element on the surface of the laser cladding hardened layer was transformed into orthorhombic α-MoO3, the surface Ti element was transformed into anatase TiO2, and the other phases remained unchanged; after cooling out of the furnace, the valve ball and valve seat were ground to a surface roughness of Ra0.2μm. After the grinding was completed, a 0.16μm thick layer was formed on the surface of the laser cladding hardened layer, which was composed of Co 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2; after the valve ball and valve seat surface are hardened and the friction reduction layer is formed, the friction coefficient is 0.09 and the wear rate is 3×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃; the characteristic diagram of valve ball and valve seat is as follows Figure 2As shown; finally, the valve ball and valve seat with the anti-friction layer formed on the surface are assembled with the matching valve body, valve stem, spring and bearing to manufacture the hard-sealed ball valve.

[0045] The hard sealing ball valve based on laser cladding of the present invention has a phase of Cr3C2+NiCr solid solution+Ni+Co-containing on the surface of the valve ball and valve seat substrate. 2+ The laser cladding hardened layer is composed of V2O5+(Ti,Mo)C+Mo+Al2O3; the thickness of the laser cladding hardened layer is 780μm, the hardness is 960HV, the coating bonding strength is 430MPa, and the porosity is 0.1%; the raw materials of the hardened layer are composed of a composite gel of Ni(OH)2 coated with Al(OH)3 and metal ceramic agglomerates with a weight percentage of 0.8:10, wherein the molar ratio of the elements in the composite gel is Ni:Al=1:1, and the metal ceramic agglomerates have a molar percentage of Ni powder of 36%, Cr powder of 10%, and Co-containing NiO coated on the surface 2+ V2O5 powder accounts for 4%, Mo powder coated with TiO2 accounts for 2%, and the rest is Cr3C2 powder; Co-containing powder coated with NiO accounts for 2%. 2+ The molar ratio of the elements in the V2O5 powder is Ni:V:Co=9:9:1, the particle size is 81nm, the surface is a 25nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure with Co embedded in the interlayer. 2+ V2O5; the molar ratio of the elements in the Mo coated with TiO2 on the surface is Ti:Mo=1:1, and the TiO2 coating layer on the surface is anatase structure with a thickness of 22nm; the laser cladding hardened layer is metallurgically bonded to the valve ball and valve seat substrate, and there is a transition zone with a thickness of 48μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo; the surface of the laser cladding hardened layer is composed of Co-containing 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2, with a thickness of 0.16μm; the friction coefficient between the valve ball and the valve seat is 0.09, and the wear rate is 3×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃.

Claims

1. A hard-sealed ball valve production process based on laser cladding, characterized in that: The following steps are involved: (1) Preparation of monoclinic friction reducing components of laser cladding hardened layer: Co(NO3)2·6H2O and NH4VO3 were added into deionized water to form a Co-containing 2+ V(OH)5 sol; Ni(NO3)2 is added to deionized water to form Ni(OH)2 sol; Ni(OH)2 sol is added dropwise to the Co-containing 2+ Co-containing NiO-coated nanostructured ... 2+ V2O5 nanopowder is used as the monoclinic friction-reducing component of the laser cladding hardening layer; (2) Preparation of orthorhombic friction reducing component precursor for laser cladding hardening layer: Mo powder is added to anhydrous ethanol to prepare mixed solution A; Ti(OC4H9)4 is added to anhydrous ethanol to prepare solution B; anhydrous ethanol and deionized water are prepared into solution C; solution B is added dropwise to solution C to prepare Ti(OH)4 sol; Ti(OH)4 sol is added dropwise to mixed solution A to prepare Mo powder with surface coated with TiO2 as the orthorhombic friction reducing component precursor for laser cladding hardening layer; (3) Preparation of metal ceramic agglomerates for laser cladding hardening treatment: weigh the raw material powders by molar percentage, with Ni powder accounting for 32-37%, Cr powder accounting for 4-10%, monoclinic friction reducing component accounting for 2-5%, orthorhombic friction reducing component precursor accounting for 1-3%, and the rest being Cr3C2 powder; after ball milling, filtration, and spray drying, sintering is performed at 1100-1200℃ in vacuum. During sintering, the NiO in the monoclinic friction reducing component is reduced and forms a Co-containing Ni-coated surface. 2+ The V2O5 nanoparticles, the surface TiO2 in the orthorhombic friction reducing component precursor reacts with Mo to form (Ti,Mo)O2 and Mo coated with (Ti,Mo)O2 on the surface; a metal ceramic agglomerate for laser cladding hardening treatment is prepared, and its composition is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo; (4) Preparation of metal ceramic powder for laser cladding hardening treatment: Ni(NO3)2 and Al(NO3)3 were weighed in a molar ratio of 1:1 and added to the reverse microemulsion to form Ni(OH)2 sol and Al(OH)3 sol respectively; Ni(OH)2 sol was added dropwise to Al(NO3)3 sol to form a composite sol of Ni(OH)2 coated with Al(OH)3; metal ceramic agglomerates were immersed in the composite sol, adsorbed and dried to prepare metal ceramic powder for laser cladding hardening treatment, the composition of which was Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)O2+Mo+ Ni(OH)2 gel+Al(OH)3 gel; (5) Grinding and preheating of valve ball and valve seat: The valve ball and valve seat substrate are manufactured by mechanical processing, and then the surface is pretreated by grinding to make the surface roughness Ra0.8~1.6μm; then the valve ball and valve seat are placed in a muffle furnace and preheated at 200~300℃; (6) Laser cladding hardening treatment of valve ball and valve seat surface: The prepared metal ceramic powder is used for laser cladding hardening treatment of valve ball and valve seat surface. The (Ti,Mo)O2 on the Mo surface is carbonized to form (Ti,Mo)C, and the gel of Ni(OH)2 coated Al(OH)3 is transformed into Ni-coated nano-Al2O3. The phase of laser cladding hardened layer is Cr3C2+NiCr solid solution+Ni+Co-containing 2+ V2O5+(Ti,Mo)C+Mo+Al2O3; (7) Formation of anti-friction layer on the surface of valve ball and valve seat and manufacturing of hard-sealed ball valve: The valve ball and valve seat after laser cladding hardening treatment are roughly ground and then treated in argon-oxygen mixed atmosphere. The Mo element on the surface of the laser cladding hardened layer is transformed into α-MoO3 of the orthorhombic system, and the surface Ti element is transformed into TiO2 of anatase structure. The other phases remain unchanged. After cooling out of the furnace, the valve ball and valve seat are ground against each other. 2+ The anti-friction layer is composed of V2O5+α-MoO3+TiO2; finally, the valve ball and valve seat with the anti-friction layer on the surface are assembled with the supporting parts to manufacture the hard-sealed ball valve.

2. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When preparing the monoclinic friction reducing component of the laser cladding hardening layer, Co(NO3)2·6H2O and NH4VO3 were weighed in a molar ratio of (1-2):9 and added into deionized water to prepare a solution, wherein the concentration of NH4VO3 in the solution was 1-2 mol / L; the solution was magnetically stirred in a constant temperature water bath at 60-70℃ for 30 min, and then ammonia water was added to adjust the pH value to 7.5-8, and then stirred for 1-2 h and allowed to stand for 2-3 h to form a Co-containing 2+ V(OH)5 sol; weigh Ni(NO3)2 and add it to deionized water to prepare a solution with a molar concentration of 0.5~1mol / L. After magnetic stirring in a constant temperature water bath at 60~70℃ for 30min, add ammonia water to adjust the pH value to 8~9, stir for 1~2h and leave for 2~3h to form Ni(OH)2 sol; drop Ni(OH)2 sol into the Co-containing 2+ The V(OH)5 sol with a molar ratio of Ni:V of 1:1 was added dropwise in a constant temperature water bath at 60-70℃ while being magnetically stirred, dried at 100-120℃ for 1h, and then calcined at 700-750℃ for 1-2h to prepare Co-containing NiO-coated sol. 2+ The V2O5 nanopowder is used as the monoclinic friction reducing component of the laser cladding hardening layer. Its particle size is 40~90nm, its surface is a 10~30nm thick NiO layer with NaCl structure, and its interior is a monoclinic layered structure of V2O5, Co 2+ Embedded in the interlayer of V2O5 layered structure, the interlayer spacing is from no Co 2+ The 0.437nm during embedding increases to 0.46~0.48nm.

3. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When preparing the orthorhombic friction reducing component precursor of the laser cladding hardening layer, Mo powder with a Fisher particle size of 0.5-1.0 μm was weighed, added to anhydrous ethanol, and ultrasonically dispersed for 20-40 min. The ultrasonic frequency and power were 40 kHz and 100 W, prepare a mixed solution A with a concentration of 1~3 mol / L; weigh Ti(OC4H9)4, add it to anhydrous ethanol and stir it magnetically for 10~20 minutes to prepare a solution B with a molar concentration of 0.5~1 mol / L; mix anhydrous ethanol and deionized water in a volume ratio of 1:1, add hydrochloric acid dropwise to a pH value of 3~4 while stirring magnetically to prepare a solution C; add solution B dropwise to solution C at room temperature and keep stirring magnetically, and after stirring, place it for 1~2 hours to prepare Ti(OH)4 sol; add Ti(OH)4 sol dropwise to mixed solution A, with a Ti:Mo element molar ratio of 1:1, and keep stirring magnetically, place it for 1~2 hours and dry it at 300~350℃ for 1~2 hours to prepare Mo powder with surface coated with TiO2 as a precursor of the orthorhombic system friction reducing component of the laser cladding hardening layer, and its surface TiO2 coating layer is anatase structure with a thickness of 10~30nm.

4. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When preparing metal ceramic agglomerates for laser cladding hardening treatment, the weighed raw material powder is subjected to planetary ball milling, the ball milling speed is 300-400 r / min, Al2O3 ceramic grinding balls with a diameter of 5 mm are used, the ball-to-material ratio of ball milling is 10:1, the mass ratio of anhydrous ethanol and PEG2000 forming agent to the raw material powder is 0.25:1 and 0.03:1 respectively, the ball milling time is 24-48 h, and after ball milling, it is filtered through a 400-mesh sieve. The filtered slurry is spray dried at 110-130° C., and the atomizing disk speed during spray drying is 4000-7000 r / min. It is vacuum sintered at 1100-1200° C. The sintering vacuum degree is 1-10 Pa. After the vacuum sintering is completed, it is cooled with the furnace, crushed and air flow graded to prepare metal ceramic agglomerates for laser cladding hardening treatment.

5. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When preparing metal ceramic powder for laser cladding hardening treatment, first add Tween 80, n-butanol, and n-hexane into deionized water, with Tween 80 accounting for 16% to 33% by weight, n-butanol accounting for 7% to 14%, n-hexane accounting for 5% to 16%, and the rest being ionized water. Stir with a magnetic stirrer at 60 to 80°C for 1 to 3 hours, and then place for 3 to 6 hours to form a reverse microemulsion; add Ni(NO3)2 and Al(NO3)3 to the reverse microemulsion to prepare a solution with a molar concentration of 0.1 to 0.5 mol / L, and then add ammonia water to adjust the pH value of the solution to 8 to 9, and stir with a magnetic stirrer at 60 to 70°C for 3 to 12 hours. The mixture was then allowed to stand for 6 to 8 hours to form Ni(OH)2 sol and Al(OH)3 sol. The Ni(OH)2 sol was added dropwise to the Al(NO3)3 sol in a constant temperature water bath at 60 to 70°C while being magnetically stirred to form a composite sol of Ni(OH)2 coated with Al(OH)3. The composite sol and metal ceramic agglomerates were weighed at a weight percentage of 0.5:10 to 1:10, the metal ceramic agglomerates were completely immersed in the composite sol, and placed in an electric vacuum drying oven for adsorption and drying treatment. The vacuum degree was ≤150Pa. The mixture was first kept at 50 to 60°C for 1 to 2 hours to allow the composite sol to be completely adsorbed into the pores of the metal ceramic agglomerates. The mixture was then dried at 110 to 120°C for 2 to 3 hours to convert the composite sol into a composite gel of Ni(OH)2 coated with Al(OH)3. The average particle size of the prepared metal ceramic powder for laser cladding hardening treatment was 30 to 47 μm.

6. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When the valve ball and valve seat are preheated after grinding, the heating rate of the preheating treatment is 5~10℃ / min and the insulation time is 5~30min.

7. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: The laser cladding process starts within 3 minutes after the valve ball and valve seat complete the preheating treatment; during laser cladding, the laser coaxially blows out argon to protect the hardened layer from oxidation, and the argon flow rate is 1~2L / min; the metal ceramic powder is laid on the surface of the valve ball and valve seat by the side axis powder feeding method, the powder feeding rate is 12~15g / min, and the angle between the metal ceramic powder flow direction and the laser optical axis is 45~50°; the laser output power is 1200~1600W, the laser spot diameter is 2~5mm, the rotation speed of the valve ball and valve seat is 3~5r / min, and the laser cladding overlap rate is 40~60%; the formed laser cladding hardened layer contains Co 2+ The surface of V2O5 is still covered by the Ni layer and no carbonization occurs, and the Mo in the core is not carbonized. The thickness of the prepared laser cladding hardened layer is 700~1200μm, the hardness is ≧950HV, the coating bonding strength is ≧400MPa, and the porosity is ≤0.5%; the laser cladding hardened layer is metallurgically bonded to the valve ball and valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo.

8. The laser cladding-based hard-sealed ball valve production process according to claim 1 is characterized in that: When the friction-reducing layer on the valve ball and valve seat is formed and the hard-sealed ball valve is manufactured, the roughness of the surface hardened layer is Ra0.6~0.8μm after rough grinding, and the initial vacuum degree of the valve ball and valve seat in the vacuum furnace is ≤5×10 -2 Pa, after heating to 450~500℃, fill with argon-oxygen mixed gas containing 5% oxygen and control the gas pressure to 2~5Pa, keep warm for 1~2h and then cool with the furnace; After cooling out of the furnace, the valve ball and valve seat are ground to a surface roughness of Ra0.2~0.4μm, forming a friction reduction layer with a thickness of 0.1~0.2μm; after the valve ball and valve seat surface are hardened and the friction reduction layer is formed, the friction coefficient is 0.08~0.12, and the wear rate is ≦5×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃; finally, the valve ball and valve seat with the anti-friction layer formed on the surface are assembled with the matching valve body, valve stem, spring and bearing to manufacture the hard-sealed ball valve.

9. A hard-sealed ball valve based on laser cladding, characterized in that: The hard-sealed ball valve production process based on laser cladding according to any one of claims 1 to 8 is obtained, comprising a valve ball and a valve seat substrate, wherein the surfaces of the valve ball and the valve seat substrate have a phase of Cr3C2+NiCr solid solution+Ni+Co-containing 2+ The laser cladding hardened layer is composed of V2O5+(Ti,Mo)C+Mo+Al2O3; the thickness of the laser cladding hardened layer is 700~1200μm, the hardness is ≧950HV, the coating bonding strength is ≧400MPa, and the porosity is ≤0.5%; the laser cladding hardened layer is metallurgically bonded to the valve ball and the valve seat substrate, and there is a transition zone with a thickness of 40~50μm between the two, and its phase composition is α-Fe+Cr3C2+NiCr solid solution+(Ti,Mo)C+Mo; the surface of the laser cladding hardened layer is composed of Co-containing 2+ The friction reduction layer is composed of V2O5+α-MoO3+TiO2, with a thickness of 0.1~0.2μm; the friction coefficient between the valve ball and the valve seat is 0.08~0.12, and the wear rate is ≦5×10 -6 mm 3 / (N·mm), the maximum service temperature is 660℃.

10. A hard-sealed ball valve based on laser cladding according to claim 9, characterized in that: The raw materials of the laser cladding hardening layer are composed of a composite gel of Ni(OH)2 coated with Al(OH)3 and a metal ceramic agglomerate with a weight percentage of 0.5:10~1:10, wherein the molar ratio of the elements in the composite gel is Ni:Al=1:1, and the metal ceramic agglomerate has a molar percentage of Ni powder accounting for 32~37%, Cr powder accounting for 4~10%, and Co-containing NiO coated on the surface. 2+ V2O5 powder accounts for 2~5%, Mo powder coated with TiO2 accounts for 1~3%, and the rest is Cr3C2 powder; Co-containing powder coated with NiO accounts for 1~3%. 2+ The molar ratio of the elements in the V2O5 powder is Ni:V:Co=9:9:1, the particle size is 40~90nm, the surface is a 10~30nm thick NiO layer with NaCl structure, and the interior is a monoclinic layered structure with Co embedded in the interlayer. 2+ V2O5; the molar ratio of elements in Mo coated with TiO2 on the surface is Ti:Mo=1:1, and the surface TiO2 coating layer is anatase structure with a thickness of 10~30nm.

Citation Information

Patent Citations

  • Hard-seal ball valve with high wear resistance and corrosion resistance and preparation method

    CN108130533A

  • Manufacturing process of metal seated ball valve nickel-based tungsten carbide wear-proof coating

    CN111455306A

  • Corrosion-resistant and wear-resistant coating with gradient composite structure and preparation method thereof

    CN113122841A

  • Preparation method of titanium alloy surface laser cladding coating

    CN114250466A

  • High-hardness wear-resistant ball for ball mill and preparation process of high-hardness wear-resistant ball

    CN115852269A