A kind of high-speed spinning spandex fiber and preparation method thereof
By adding glycerol monoacetate and mixed amine solution to the prepolymerization reaction, diethylene triamine and functional agent are used to optimize the spinning process parameters, the problems of spandex spinning speed and quality in the existing technology are solved, and high speed is achieved The preparation of spinning and high-quality spandex fibers improves the physical performance and production efficiency of the product.
Patent Information
- Application Number
- CN202411183461.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
When the existing dry spinning technology improves spandex spinning speed, the production efficiency is low and the spinning condition becomes worse, and the tension uniformity is poor, making it difficult to improve the spinning speed and product quality at the same time.
By adding glycerol monoacetate to the prepolymerization reaction and adding diethylene triamine and functional agent to the mixed amine solution, chain extension reaction and maturation are carried out, combined with optimizing spinning process parameters such as spinning speed and temperature, high-speed preparation is performed. Spinned spandex fiber.
It realizes the preparation of high-quality spandex fibers at a faster spinning speed, reduces production costs, improves the tension uniformity and physical properties of spandex, and improves the elongation of break and heat resistance.
Smart Images

Figure CN118685886B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material preparation, and in particular relates to high-speed spun spandex fiber and a preparation method thereof. Background Art
[0002] Spandex is the abbreviation of polyurethane fiber, which is a highly elastic synthetic fiber with high stretchability and resilience. Due to its excellent performance, it is widely used in various garments and fabrics that need to be stretched. Its production process is generally to form a prepolymer product by reacting a high molecular weight diol compound with an excess of diisocyanate, then adding an amine chain extender and a chain terminator to react to obtain a polyurethane urea spinning solution, and finally obtaining spandex after dry or wet spinning.
[0003] Since the dry spinning process is relatively mature, the quality and performance of the fibers produced are relatively good, and the continuous polymerization method used has the characteristics of high efficiency, low energy consumption, and stable product quality, it has become the most widely used method for spandex production.
[0004] Chinese patent CN102154729B discloses a method for preparing high-elongation and high-draft spandex fibers. The prepared product has high elongation and high draft characteristics, but the spinning speed is only 600-750 m / min, and the production efficiency is low. It can be seen that the production efficiency of the existing dry spinning needs to be further improved.
[0005] At present, the spinning speed of spandex production is 800-900m / min. After further increasing the speed, the spandex spinning condition will deteriorate, for example, there will be more parallel yarns, and the tension uniformity of the obtained spandex will also be poor. Summary of the invention
[0006] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:
[0007] The invention provides a preparation method of high-speed spun spandex fiber, comprising the following steps: subjecting a prepolymer raw material to a prepolymerization reaction, adding a solvent to dissolve it, then adding a mixed amine solution to carry out a chain extension reaction, adding auxiliary material additives, and then carrying out aging and spinning processes to obtain the high-speed spun spandex fiber.
[0008] Preferably, the prepolymer raw materials include polytetramethylene ether glycol and diphenylmethane-4,4'-diisocyanate.
[0009] Preferably, polytetramethylene ether glycol and diphenylmethane-4,4'-diisocyanate are used in a mass ratio of 1-5:1.
[0010] Preferably, the prepolymerization raw material is subjected to a prepolymerization reaction to obtain a prepolymerization product.
[0011] Preferably, the prepolymerization product and the solvent are used in a mass ratio of 1:1-5 to obtain a prepolymerization product solution.
[0012] Preferably, the prepolymerization product solution and the mixed amine solution are used in a mass ratio of 1-5:1.
[0013] Preferably, the auxiliary material additive and the prepolymer product solution are used in a mass ratio of 1-2:10-30.
[0014] Preferably, the mixed amine solution comprises a mixture of an amine substance and a solvent.
[0015] Preferably, the amine substances include diethylamine, 1,2-propylenediamine, ethylenediamine and diethylenetriamine.
[0016] Preferably, diethylenetriamine accounts for 0.1-0.5 wt % of the mixed amine solution.
[0017] Preferably, the amine substance accounts for 7-10 wt % of the mixed amine solution.
[0018] Preferably, the mass ratio of diethylenetriamine to diethylamine is 1-5:10-15.
[0019] Preferably, the mass ratio of diethylenetriamine to 1,2-propylenediamine is 1-5:20-30.
[0020] Preferably, the mass ratio of diethylenetriamine to ethylenediamine is 1-5:80-100.
[0021] Preferably, the auxiliary material additive comprises a mixture of auxiliary materials and solvents.
[0022] Preferably, the auxiliary materials include antioxidants and anti-yellowing agents.
[0023] Preferably, the antioxidant comprises AO-80.
[0024] Preferably, the anti-yellowing agent includes HN-150.
[0025] Preferably, the mass ratio of the solvent to the antioxidant is 1-10:1; the mass ratio of the solvent to the anti-yellowing agent is 5-50:1.
[0026] Preferably, the solvent comprises N,N-dimethylacetamide.
[0027] Preferably, the spinning process includes a spinning tunnel size of 1000-1500×450 cm, a spinning tunnel temperature of 250-260° C., a spinning speed of 1000-1200 m / min, and a spinning roll number of 100-120 rolls.
[0028] More preferably, the specific steps of the method for preparing high-speed spun spandex fiber include:
[0029] Polytetramethylene ether glycol and diphenylmethane-4,4'-diisocyanate are mixed at a mass ratio of 1-5:1 to perform a prepolymerization reaction to obtain a prepolymer product; N,N-dimethylacetamide is added to the prepolymer product at a mass ratio of the prepolymer product to N,N-dimethylacetamide of 1:1-5 to obtain a prepolymer product solution.
[0030] Amine substances are added to N,N-dimethylacetamide, wherein the amine substances include diethylamine, 1,2-propylenediamine, ethylenediamine and diethylenetriamine to obtain a mixed amine solution, wherein diethylenetriamine accounts for 0.1-0.5wt% of the mixed amine solution, the amine substances account for 7-10wt% of the mixed amine solution, and the mass ratio of diethylamine, 1,2-propylenediamine, ethylenediamine and diethylenetriamine is 10-15:20-30:80-100:1-5; the mixed amine solution is added to a prepolymer product solution to carry out a chain extension reaction and a termination reaction, and the prepolymer product solution and the mixed amine solution are used in a mass ratio of 1-5:1 to obtain a polyurethane solution.
[0031] Add auxiliary materials to N,N-dimethylacetamide, the auxiliary materials include antioxidants and anti-yellowing agents, the antioxidants include AO-80, and the anti-yellowing agents include HN-150; N,N-dimethylacetamide, antioxidants and anti-yellowing agents are used in a mass ratio of 5-50:5:1 to obtain auxiliary material additives; add the auxiliary material additives to the polyurethane solution in a mass ratio of 1:10-30 to the prepolymer product solution, and mature at 40-50°C for 24-48 hours to obtain a spandex spinning stock solution.
[0032] The spandex spinning solution is spun in a spinning tunnel of 1000-1500×450cm at 250-260°C, with a spinning roll number of 100-120 rolls and a spinning speed of 1000-1200m / min to obtain high-speed spun spandex fibers. The addition of diethylenetriamine improves the physical properties of spandex by increasing the cross-linking and hydrogen bonding between polyurethane macromolecules, thereby preparing spandex with uniform tension at a faster spinning speed.
[0033] In one embodiment of the present invention, a functional agent is added to the mixed amine solution during the preparation of the high-speed spun spandex fiber.
[0034] Preferably, the mixed amine solution comprises an amine substance and a solvent.
[0035] Preferably, the amine substances include diethylamine, 1,2-propylenediamine, ethylenediamine, functional agents and diethylenetriamine.
[0036] Preferably, diethylenetriamine accounts for 0.1-0.5 wt % of the mixed amine solution.
[0037] Preferably, the amine substance accounts for 7-10 wt % of the mixed amine solution.
[0038] Preferably, the mass ratio of diethylenetriamine to diethylamine is 1-5:10-15.
[0039] Preferably, the mass ratio of diethylenetriamine to 1,2-propylenediamine is 1-5:20-30.
[0040] Preferably, the mass ratio of diethylenetriamine to ethylenediamine is 1-5:80-100.
[0041] Preferably, the mass ratio of diethylenetriamine to the functional agent is 1-5:20-40.
[0042] Preferably, the functional agent is prepared from methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate. The added functional agent participates in the reaction to form polyurethane macromolecules, thereby improving the performance of the polyurethane macromolecules in producing soft segments of spandex, so that the soft segments of spandex have better tensile properties, and thus the spandex has better elongation at break; and the presence of benzene ring groups in the functional agent makes the spandex have better heat resistance, and in the spinning process, it can withstand the high temperature treatment of the tunnel without affecting the physical properties of the spandex.
[0043] In one embodiment of the present invention, when preparing high-speed spun spandex fibers, the prepolymer raw materials further include glycerol monoacetate.
[0044] Preferably, the prepolymer raw material includes polytetramethylene ether glycol, diphenylmethane-4,4'-diisocyanate and glycerol monoacetate.
[0045] Preferably, glycerol monoacetate and diphenylmethane-4,4'-diisocyanate are used in a mass ratio of 1:1-5. During the prepolymerization reaction, glycerol monoacetate is added, and glycerol monoacetate plays a role in the prepolymerization stage. Glycerol monoacetate participates in the prepolymerization reaction, improves the polymer structure of spandex, and makes the spandex have better elongation at break and heat resistance.
[0046] In one embodiment of the present invention, the preparation of the functional agent comprises the following steps:
[0047] Methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate are mixed to obtain a reaction solution; tetrabutyl titanate is added to the reaction solution, heated for reaction, anhydrous ethanol is added to dissolve, and the functional agent is obtained by suction filtration, rotary evaporation and drying.
[0048] Preferably, methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate are used in a molar ratio of 1:1-5.
[0049] Preferably, 0.1-0.5 wt % of tetrabutyl titanate is added to the reaction solution.
[0050] Preferably, methyl benzenesulfonate and anhydrous ethanol are used in a ratio of 1-5 mol: 500-1000 ml.
[0051] More preferably, the specific preparation steps of the functional agent include:
[0052] Methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate are mixed in a molar ratio of 1:1-5 to obtain a reaction solution, 0.1-0.5wt% of tetrabutyl titanate is added to the reaction solution, and after stirring and mixing, the temperature is raised to 130-160°C, and the temperature is maintained for reaction for 2-4 hours, the temperature is further raised to 180-200°C, and the temperature is maintained for reaction for 2-4 hours, and the reaction is cooled to room temperature, and anhydrous ethanol is added in a ratio of methyl benzenesulfonate and anhydrous ethanol of 1-5mol:500-1000ml, and the mixture is stirred to dissolve, and then suction filtration is performed, the filtrate is collected, and rotary evaporation and drying are performed to obtain a functional agent.
[0053] The invention also provides application of high-speed spun spandex fibers on fabrics.
[0054] Compared with the prior art, the present invention provides a method for preparing high-speed spun spandex fiber, wherein diethylenetriamine is added to a mixed amine solution, and then the length of the spinning tunnel is enlarged and the temperature of the spinning tunnel is increased, so that spandex can be prepared at a faster spinning speed, thereby reducing the production cost of spandex, and the prepared spandex has uniform tension. The present invention further adds glycerol monoacetate to the prepolymerization reaction, and the glycerol monoacetate participates in the prepolymerization reaction, thereby improving the polymer structure of the spandex; at the same time, a functional agent is added to the mixed amine solution, and the functional agent participates in the reaction, thereby improving the performance of the polyurethane macromolecule to produce the soft segment of spandex, so that the soft segment of the spandex has better tensile properties, and the presence of the benzene ring group in the functional agent makes the spandex have better heat resistance, thereby preparing spandex with better elongation at break and heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is the infrared spectrum of the functional agent. DETAILED DESCRIPTION
[0056] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] The experimental methods in the following examples, unless otherwise specified, are all conventional methods or conditions recommended by the manufacturer. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0058] The preparation steps of high-speed spun spandex fiber include the following steps:
[0059] 1) subjecting prepolymer raw materials, including polytetramethylene ether glycol (PTMEG) and diphenylmethane-4,4'-diisocyanate (MDI), to prepolymerization reaction to obtain a prepolymer product; adding a solvent, including N,N-dimethylacetamide (DMAC), to dissolve the prepolymer product to obtain a prepolymer product solution;
[0060] 2) adding amine substances, including diethylamine (DEA), 1,2-propylenediamine (PDA) and ethylenediamine (EDA), into a solvent to obtain a mixed amine solution;
[0061] 3) adding the mixed amine solution to the prepolymer product solution to carry out chain extension reaction and termination reaction to obtain a polyurethane solution;
[0062] 4) adding antioxidants, including AO-80, and anti-yellowing agents, including HN-150, to the solvent to obtain auxiliary material additives;
[0063] 5) Adding auxiliary material additives to the polyurethane solution, and then aging it to obtain spandex spinning solution;
[0064] 6) The spandex spinning solution is spun in a spinning tunnel to obtain high-speed spun spandex fibers.
[0065] Example 1: Preparation of high-speed spun spandex fibers
[0066] 45g of PTMEG and 15g of MDI were mixed for prepolymerization to obtain a prepolymer product, and then 120g of DMAC was added and stirred to dissolve to obtain a prepolymer product solution; 0.96g of EDA, 0.14g of DEA, 0.3g of PDA and 0.04g of diethylenetriamine (DETA) were added to 18.6g of DMAC to obtain a mixed amine solution; the mixed amine solution was added to the prepolymer product solution for chain extension reaction and termination reaction to obtain a polyurethane solution; 1g of AO-80 and 0.4g of HN-150 were added to 10g of DMAC to obtain auxiliary material additives; the auxiliary material additives were added to the polyurethane solution, aged at 40°C for 25h to obtain a spandex spinning stock solution; the spandex spinning stock solution was spun in a spinning shaft of 1380×450cm at a shaft temperature of 260°C, a roll number of 120 rolls, and a spinning speed of 1100m / min to obtain 2OD high-speed spun spandex fiber.
[0067] Example 2: Preparation of high-speed spun spandex fibers
[0068] The difference between Example 2 and Example 1 is that in Example 2, a functional agent is further added to the mixed amine solution.
[0069] The preparation of high-speed spun spandex fiber is as follows:
[0070] 45g of PTMEG and 15g of MDI are mixed for prepolymerization to obtain a prepolymer product, and then 120g of DMAC is added for stirring and dissolution to obtain a prepolymer product solution; 0.96g of EDA, 0.14DEA, 0.3g of PDA, 0.04g of DETA and 0.2g of a functional agent are added to 18.6g of DMAC to obtain a mixed amine solution; the mixed amine solution is added to the prepolymer product solution for chain extension reaction and termination reaction to obtain a polyurethane solution; 1g of AO-80 and 0.4g of HN-150 are added to 10g of DMAC to obtain an auxiliary material additive; the auxiliary material additive is added to the polyurethane solution, and aged at 40°C for 25h to obtain a spandex spinning stock solution; the spandex spinning stock solution is spun in a spinning shaft of 1380×450cm at a shaft temperature of 260°C, a roll number of 120 rolls, and a spinning speed of 1100m / min to obtain 2OD high-speed spun spandex fiber.
[0071] The preparation of the functional agent comprises the following steps:
[0072] Mix 0.2 mol of methyl benzenesulfonate and 0.2 mol of tri(2-hydroxyethyl)isocyanurate, add 0.5 wt% of tetrabutyl titanate, stir evenly, heat to 150°C to completely melt tri(2-hydroxyethyl)isocyanurate, keep warm for reaction for 2 hours, evaporate the generated methanol, then heat to 190°C at a rate of 10°C / h, continue to react for 2 hours, stop heating, stir and cool to room temperature, add 100 ml of anhydrous ethanol, continue stirring until the product is dissolved, filter, collect the filtrate, rotary evaporate, and put the product into a vacuum drying oven at 40°C for 48 hours to obtain a functional agent.
[0073] Example 3: Preparation of high-speed spun spandex fibers
[0074] The difference between Example 3 and Example 2 is that the added amount of the functional agent in Example 3 is 0.4 g, and the preparation of the functional agent is the same as that in Example 2.
[0075] Example 4: Preparation of high-speed spun spandex fibers
[0076] The difference between Example 4 and Example 3 is that in Example 4, glycerol monoacetate is also added during the prepolymerization.
[0077] The preparation of high-speed spun spandex fiber is as follows:
[0078] 45g PTMEG, 15g MDI and 5g glycerol monoacetate were mixed for prepolymerization to obtain a prepolymer product, and then 120g DMAC was added and stirred to dissolve to obtain a prepolymer product solution; 0.96g EDA, 0.14g DEA, 0.3g PDA, 0.04g DETA and 0.4g functional agent were added to 18.6g DMAC to obtain a mixed amine solution; the mixed amine solution was added to the prepolymer product solution for chain extension reaction and termination reaction to obtain a polyurethane solution; 1g AO-80 and 0.4g HN-150, to obtain auxiliary material additives; adding the auxiliary material additives into the polyurethane solution, aging at 40°C for 25 hours to obtain a spandex spinning stock solution; spinning the spandex spinning stock solution in a spinning tunnel of 1380×450 cm, at a tunnel temperature of 260°C, a roll number of 120, and a spinning speed of 1100 m / min to obtain 2OD high-speed spun spandex fibers.
[0079] Example 5: Preparation of high-speed spun spandex fibers
[0080] The difference between Example 5 and Example 4 is that the added amount of glycerol monoacetate in Example 5 is 10 g.
[0081] Comparative Example 1: Preparation of high-speed spun spandex fibers
[0082] The difference between Comparative Example 1 and Example 1 is that the mixed amine solution of Comparative Example 1 does not contain DETA.
[0083] The preparation of high-speed spun spandex fiber is as follows:
[0084] 45g of PTMEG and 15g of MDI are mixed for prepolymerization to obtain a prepolymer product, and then 120g of DMAC is added for stirring and dissolution to obtain a prepolymer product solution; 0.96g of EDA, 0.14g of DEA and 0.3g of PDA are added to 18.6g of DMAC to obtain a mixed amine solution; the mixed amine solution is added to the prepolymer product solution for chain extension reaction and termination reaction to obtain a polyurethane solution; 1g of AO-80 and 0.4g of HN-150 are added to 10g of DMAC to obtain auxiliary material additives; the auxiliary material additives are added to the polyurethane solution, aged at 40°C for 25h to obtain a spandex spinning stock solution; the spandex spinning stock solution is spun in a spinning shaft of 1380×450cm at a shaft temperature of 260°C, a roll number of 120 rolls and a spinning speed of 1100m / min to obtain 2OD high-speed spun spandex fiber.
[0085] Comparative Example 2: Preparation of high-speed spun spandex fibers
[0086] The difference between Comparative Example 2 and Comparative Example 1 is that in Comparative Example 2, spinning is performed at a spinning speed of 900 m / min.
[0087] Test Example 1: Infrared spectrum of functional agent
[0088] The results are as follows Figure 1 It can be seen that at 3300-3400cm -1 The absorption peak is the stretching vibration peak of -OH, at 3000-3100cm -1 The absorption peak is the stretching vibration peak of CH on the benzene ring, at 1700-1750cm -1 The absorption peak is the stretching vibration peak of C=O, at 1200-1300cm -1 The absorption peak is the stretching vibration peak of CN, at 1000-1100cm -1 The absorption peak is the stretching vibration peak of S=O.
[0089] Test Example 2: Elongation at break of spandex
[0090] The spandex prepared in Examples 1-5 and Comparative Examples 1-2 was kept in a standard atmosphere without tension and relaxed for 4 hours, and then tested with an iso-elongation testing machine to obtain the elongation at break of the spandex. The parameters of the iso-elongation testing machine were: a clamp spacing of 50 mm and a stretching speed of 50 mm / min.
[0091] The results are shown in Table 1. Compared with Example 1 and Comparative Example 1, it can be seen that adding DETA to the mixed amine solution makes the spandex prepared in Example 1 at a spinning speed of 1100 m / min have a better elongation at break. DETA may improve the physical properties of spandex by increasing the cross-linking and hydrogen bonding between polyurethane macromolecules, thereby preparing spandex with a better elongation at break at a faster spinning speed. Further comparing Example 1, Comparative Examples 1 and 2, it can be seen that the spandex prepared in Comparative Example 2 at a spinning speed of 900 m / min has a better elongation at break, indicating that adding DETA to the mixed amine solution increases the spinning speed of preparing spandex while ensuring that the spandex has a better elongation at break.
[0092] Comparing Examples 1, 2, and 3, it can be seen that the elongation at break of the spandex prepared in Example 1 is poor, indicating that the further addition of a functional agent to the mixed amine solution improves the elongation at break of the spandex. The functional agent may improve the performance of the spandex soft segment, thereby improving the elongation at break of the spandex. Comparing Examples 3, 4, and 5, it is shown that the addition of glycerol monoacetate further improves the elongation at break of the spandex. Glycerol monoacetate may play a role in the prepolymerization stage. Glycerol monoacetate participates in the prepolymerization reaction, improves the polymer structure of the spandex, and thereby improves the elongation at break of the spandex.
[0093] Table 1 Elongation at break of spandex
[0094]
[0095] Test Example 3: Heat resistance of spandex
[0096] The spandex prepared in Examples 1-5 and Comparative Examples 1-2 was kept in a standard atmosphere without tension for 5 hours, and then tested with an iso-elongation type strength tester to obtain the spandex's breaking strength F1. The spandex prepared in Examples 1-5 and Comparative Examples 1-2 was subjected to dry heat treatment, and then the spandex was kept in a standard atmosphere without tension for 5 hours, and then tested with an iso-elongation type strength tester to obtain the spandex's breaking strength F2. The dry heat treatment conditions were 200°C, 60s. The iso-elongation type strength tester parameters were: clamp spacing 50mm, stretching speed 50mm / min.
[0097] The heat resistance of spandex is characterized by its breaking strength retention rate, which is F2 / F1. The higher the breaking strength retention rate, the better the heat resistance of spandex.
[0098] The results are shown in Table 2. Compared with Comparative Example 1, it can be seen that the addition of DETA to the mixed amine solution in Example 1 enables the spandex prepared in Example 1 at a spinning speed of 1100 m / min to have a better retention rate of breaking strength. DETA may improve the physical properties of spandex by increasing the cross-linking and hydrogen bonding between polyurethane macromolecules, thereby being able to prepare heat-resistant spandex at a faster spinning speed.
[0099] Comparing Examples 1, 2, and 3, it can be seen that the breaking strength retention rate of Example 1 is poor, indicating that the addition of a functional agent to the mixed amine solution improves the breaking strength retention rate of spandex, and the prepared spandex has a good breaking strength retention rate, that is, better heat resistance. The functional agent containing a benzene ring may improve the heat resistance of spandex. Comparing Examples 3, 4, and 5, it is shown that the addition of glycerol monoacetate further improves the heat resistance of spandex. Glycerol monoacetate may play a role in the prepolymerization stage. Glycerol monoacetate participates in the prepolymerization reaction, improves the polymer structure of spandex, and then improves the heat resistance of spandex.
[0100] Table 2 Breaking strength retention rate of spandex
[0101]
[0102] Test Example 4: Dynamic stress CV value of spandex
[0103] The spandex of Example 1, Comparative Example 1 and Comparative Example 2 was subjected to dynamic stress testing, and the results are shown in Table 3. The smaller the dynamic stress CV value, the better the uniformity of the spandex.
[0104] Under normal 3.5 times drafting, the dynamic stress CV value of Comparative Example 1 reaches 7.1%, the dynamic stress CV value of Comparative Example 2 reaches 5.5%, and the dynamic stress CV value of Example 1 is less than 4.5%, which indicates that the spandex prepared by adding DETA to the mixed amine solution has good tension uniformity. The addition of DETA may improve the uniformity of the polyurethane solution by increasing the cross-linking and hydrogen bonding between polyurethane macromolecules, thereby enabling the spinning of spandex with good tension uniformity.
[0105] Table 3 Dynamic stress CV values of spandex
[0106]
[0107] The embodiments and / or implementation methods described above are only used to illustrate the preferred embodiments and / or implementation methods for realizing the technology of the present invention, and are not intended to limit the implementation methods of the technology of the present invention in any form. Any technical personnel in this field may make slight changes or modifications to other equivalent embodiments without departing from the scope of the technical means disclosed in the content of the present invention, but they should still be regarded as technologies or embodiments that are essentially the same as the present invention.
Claims
1. A method for preparing high-speed spun spandex fiber, comprising the following steps: The prepolymer raw material is subjected to a prepolymerization reaction, a solvent is added to dissolve it, and then a mixed amine solution is added to carry out a chain extension reaction, and then auxiliary material additives are added, followed by aging and spinning processes to obtain high-speed spun spandex fibers; The mixed amine solution comprises a mixture of an amine substance and a solvent, the auxiliary material additive comprises a mixture of an auxiliary material and a solvent, and the amine substance comprises diethylamine, 1,2-propylenediamine, ethylenediamine, a functional agent, and diethylenetriamine; The solvent includes N,N-dimethylacetamide; the prepolymer raw materials include polytetramethylene ether glycol, diphenylmethane-4,4'-diisocyanate and glycerol monoacetate; the auxiliary materials include antioxidants and anti-yellowing agents; The functional agent is prepared from methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate; methyl benzenesulfonate and tris(2-hydroxyethyl)isocyanurate are used in a molar ratio of 1:1-5; glycerol monoacetate and diphenylmethane-4,4'-diisocyanate are used in a mass ratio of 1:1-5; The mass ratio of diethylenetriamine to diethylamine is 1-5:10-15; the mass ratio of diethylenetriamine to 1,2-propylenediamine is 1-5:20-30; the mass ratio of diethylenetriamine to ethylenediamine is 1-5:80-100; the mass ratio of diethylenetriamine to the functional agent is 1-5:20-40; The amine substance accounts for 7-10wt% of the mixed amine solution; The diethylenetriamine accounts for 0.1-0.5wt% of the mixed amine solution.
2. The preparation method according to claim 1, It is characterized in that In the spinning process, the temperature of the spinning tunnel is 250-260° C., the spinning speed is 1000-1200 m / min, and the number of spinning rolls is 100-120.
3. The preparation method according to claim 1, It is characterized in that The polytetramethylene ether glycol and diphenylmethane-4,4'-diisocyanate are used in a mass ratio of 1-5:
1.
4. The high-speed spun spandex fiber prepared by the preparation method according to any one of claims 1 to 3.
5. Use of the high-speed spun spandex fiber as claimed in claim 4 on fabrics.