A spunlace-hot-rolled nonwoven fabric and its production process
Through the three-layer structure hydrospunlace-hot rolled non-woven fabric process and the use of composite nanomaterials, the problems of poor mechanical properties and high production costs of non-woven fabrics are solved, and the antibacterial and mechanical properties are improved, thus reducing production costs are reduced. .
Patent Information
- Application Number
- CN202411180846.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing non-woven fabrics are prone to damage when subjected to large forces, and their mechanical properties are poor, resulting in limited application range. At the same time, the large amount of silver-loaded antibacterial materials are added to lead to high production costs.
The production process of hydrospunlace-hot rolled non-woven fabrics with three-layer structures is made of water-soluble fibers and mixed fibers of low melting point fibers and mixed fibers of plant fibers and low melting point fibers. The hydrospuncture composite flat rolling and hot rolling process is combined with Composite nanomaterials to improve antibacterial and mechanical properties.
It realizes a non-woven fabric with soft feel, good breathability, strong antibacteriality and high mechanical strength, which reduces the use of silver, reduces production costs, and improves the density and flame retardant properties of the fiber structure.
Smart Images

Figure CN118700661B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a spunlace-hot-rolled nonwoven fabric and a production process thereof. Background Art
[0002] Non-woven fabrics, also known as non-woven fabrics, are made of directional or random fibers. They are called cloth because they have the appearance and certain properties of cloth. Non-woven fabrics are moisture-proof, breathable, flexible, lightweight, non-combustible, easy to decompose, non-toxic and non-irritating, colorful, low-priced, and recyclable. They are currently widely used in medical treatment, nursing, protection, surgery, disease prevention and treatment, etc.
[0003] In the prior art, the preparation of non-woven fabrics mainly uses polypropylene as raw material. Since the tensile strength of polypropylene is average, the non-woven fabrics prepared with polypropylene fibers are easily damaged when subjected to large forces, and the poor mechanical properties limit their scope of application.
[0004] Chinese patent document CN1346905A discloses a method for manufacturing a silver-loaded antibacterial composite nonwoven fabric, which includes the following steps: 1) Preparation of antibacterial masterbatch: 25-50% by weight of silver-loaded antibacterial material, 40-75% by weight of fiber resin, and 0-10% by weight of plastic additives are mixed and melted in a screw extruder granulator to form an antibacterial masterbatch; 2) Preparation of antibacterial spunbond web: 2-4% by weight of antibacterial masterbatch is mixed with 96-98% by weight of fiber resin, and then the antibacterial spunbond web is prepared according to a conventional spunbond process; 3) Preparation of composite antibacterial nonwoven fabric: After the antibacterial spunbond web and cotton fiber web or wood pulp fiber web are subjected to composite hydroentanglement treatment, they are dried to form a composite antibacterial nonwoven fabric. The silver-loaded antibacterial composite nonwoven fabric prepared by this method has the advantages of high antibacterial performance, durability, broad safety spectrum, and excellent comfort. This process has the disadvantage of a large amount of silver-loaded antibacterial material added, resulting in a high production cost. Summary of the invention
[0005] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to provide a spunlace-hot-rolled non-woven fabric with good antibacterial and mechanical properties.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0007] The present invention provides a production process of a spunlace-hot-rolled nonwoven fabric, comprising the following steps:
[0008] S1, unpacking the A-side fibers and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then performs a humidification treatment to obtain an A-layer cotton web;
[0009] S2, unpacking the B-side fibers and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then cross-lays the web to obtain a B-layer cotton web;
[0010] S3. After the C layer grey cloth is fed through the material roll, it is hydroentangled with the B layer cotton mesh and flattened, and then placed in the finishing agent for finishing with the A layer cotton mesh. After finishing, it is glued with glue to obtain a composite layer, and then the composite layer is pre-baked, and then combined by hot rolling and rolled up. After passing the inspection, it is packaged and shipped out.
[0011] Preferably, in step S1, the A-side fibers are mixed fibers of water-soluble fibers and low-melting-point fibers; the mass ratio of the two is 3-5:1-2.
[0012] Further preferably, the water-soluble fiber is one or more of PVA fiber, seaweed fiber, carboxymethyl cellulose fiber, and polyacrylamide fiber.
[0013] Preferably, the low-melting-point fiber is one or more of polyethylene fiber, polypropylene fiber, and polybutene fiber.
[0014] Preferably, in the step S1, the fibers on the A side are subjected to humidification treatment after forming a cotton web, and the moisture content is controlled at 25-40%.
[0015] Preferably, the B-side fiber in step S2 is a mixed fiber of plant fiber and low-melting-point fiber; the mass ratio of the two is 2-4:1-3; further preferably, the plant fiber is one or more of cotton fiber, flax fiber, and bamboo fiber.
[0016] Preferably, the pre-drying in step S3 controls the dryness of the entire cloth to be 60-80%.
[0017] Preferably, in step S3, the C layer grey cloth is one of polyester fiber, nylon fiber, polyester fiber and polypropylene fiber.
[0018] Preferably, the steps of sorting in step S3 are as follows:
[0019] Add 1-3 parts of sodium polyacrylate, 1-5 parts of sodium dodecyl sulfate and 0.5-1.5 parts of triethylamine to 50-100 parts of water, stir and mix evenly to obtain a mixed solution, add 1-2 parts of composite nanomaterials to the mixed solution, stir quickly for 30-50 minutes, and then ultrasonically treat to obtain a finishing agent; immerse the fabric in the finishing agent for 10-15 minutes, and then take out, dehydrate, shape and dry.
[0020] Further preferably, the method for preparing the composite nanomaterial comprises the following steps:
[0021] (1) adding 10-18 parts by weight of bentonite to an aqueous solution of sodium dodecyl sulfate, heating and stirring, cooling to room temperature, filtering, collecting the filter residue, washing the filter residue with water, drying, grinding, and then adding it to anhydrous ethanol, to which 40-60 parts by weight of an ethanol solution of n-butyl titanate is added dropwise; after the addition is complete, reacting at room temperature, adding 50-150 parts by weight of water, stirring, standing, centrifuging, collecting solids, washing the solids, and calcining them in a muffle furnace to obtain porous bentonite;
[0022] (2) ultrasonically dispersing 7-15 parts by weight of graphene oxide in water to obtain a graphene oxide suspension; adding 50-150 parts by weight of an aqueous silver nitrate solution and stirring the mixture evenly; adding an aqueous NaOH solution and mixing the mixture to obtain a mixed solution; transferring the mixed solution into a high-pressure reactor for a hydrothermal reaction; after the reaction is completed, cooling to room temperature, filtering, collecting solids, washing the solids with water, drying, and then calcining to obtain graphene-loaded silver oxide;
[0023] (3) 5-10 parts by weight of graphene-loaded silver oxide, 3-6 parts by weight of porous bentonite, and anhydrous methanol are mixed and stirred evenly, then ultrasonically treated, heated, and 1.5-3.5 parts by weight of KH550 silane coupling agent are added, stirred for reaction, and after the reaction is completed, cooled and filtered to collect the filter cake, and the filter cake is dried to obtain the composite nanomaterial.
[0024] Preferably, the pressure of the water spunlace process in step S3 is 6-10 MPa, and the water needle aperture is 0.3-0.5 mm.
[0025] Preferably, the hot rolling temperature in step S3 is 180-200°C.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The nonwoven fabric of the present invention has a three-layer structure. Its manufacturing process is to firstly use a spunlace process to compound the B-layer cotton web and the C-layer grey cloth and then combine them with the A-layer cotton web by hot rolling. It has the advantages of soft hand feeling, good air permeability, good antibacterial property, high mechanical strength, etc.
[0028] 2) The A-layer cotton web and the B-layer cotton web of the present invention use bicomponent fibers, which have better fluffiness and softness and better liquid absorption performance compared to single-type polypropylene fibers. The B-layer cotton web is mechanically reinforced by a hydroentanglement process, which is beneficial to the density of the fabric structure, thereby improving the mechanical properties of the fabric, and is also beneficial to the affinity between the fibers during the hot rolling process, and the phenomenon of fiber loss will not occur;
[0029] 3) In the composite nanomaterial of the present invention, silver oxide grows in situ on graphene, which prevents the agglomeration of silver oxide, reduces the amount of silver used, and reduces the cost. Bentonite is functionalized by sodium dodecyl sulfate, and hydrolyzed in the layered structure of bentonite to generate titanium sol particles, which avoids the agglomeration of nanomaterial titanium dioxide and increases the action sites of nanomaterials. The silver oxide loaded on graphene enters the mesopores of bentonite, thereby improving the stability and durability of porous bentonite. In addition, the adsorption of bacteria by graphene and porous bentonite is more conducive to the action of silver oxide and titanium dioxide on bacteria, thereby improving its antibacterial performance.
[0030] 4) The composite nanomaterial of the present invention can be deposited into the gaps between fibers and well combined with the fibers during the hot rolling process, making the structure between the fibers denser and improving the mechanical properties and flame retardant properties of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a production process flow chart of the spunlace-hot-rolled nonwoven fabric. DETAILED DESCRIPTION
[0032] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be described clearly and completely below. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The sources of some raw materials used in the present invention are as follows:
[0034] Graphene oxide, particle size <5 μm, was purchased from Beijing Meiston Technology Development Co., Ltd.
[0035] Bentonite, mesh number 40, was purchased from Sishui County Yitong Bentonite Co., Ltd.
[0036] Example 1
[0037] A production process of spunlace-hot-rolled nonwoven fabric, the specific process flow is as follows Figure 1 As shown, the following steps are included:
[0038] S1. After unpacking 500g PVA fiber and 200g polypropylene fiber, feed the cotton into an air pressure automatic cotton box. The air pressure automatic cotton box processes the fiber into uniform sieved cotton and then feeds it to a carding machine. The carding machine humidifies the sieved cotton into a cotton web to obtain an A-layer cotton web, and controls the moisture content of the cotton web to be 30%;
[0039] S2, unpacking 400g of flax fiber and 300g of polypropylene fiber and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then cross-lays the web to obtain a B-layer cotton web;
[0040] S3. The polypropylene fiber cloth is fed through a material roll and then hydroentangled with the B-layer cotton mesh and flattened, and then placed in a finishing agent for finishing with the A-layer cotton mesh. The pressure of the hydroentanglement process is 10MPa, and the aperture of the water needle is 0.5mm. After finishing, the composite layer is bonded with glue, and then the composite is pre-baked. The dryness of the whole cloth is controlled at 70% by pre-baking. Then, it is combined by hot rolling at 200℃ and then rolled up. After passing the inspection, it is packaged and shipped out.
[0041] The steps in step S3 are as follows:
[0042] Add 30 g of sodium polyacrylate, 50 g of sodium dodecyl sulfate and 15 g of triethylamine to 1000 parts of water, stir and mix evenly to obtain a mixed solution, add 20 g of the composite nanomaterial to the mixed solution, stir at 2000 rpm for 40 min, and then ultrasonically treat at 1200 W for 15 min to obtain a finishing agent; immerse the fabric in the finishing agent for 15 min, and then take it out for dehydration, setting and drying.
[0043] The preparation method of the composite nanomaterial comprises the following steps:
[0044] (1) 13 g of bentonite was added to 250 mL of a 25 wt% aqueous solution of sodium dodecyl sulfate, and stirred at 70 °C for 8 h. After stirring, the mixture was cooled to room temperature, filtered, and the residue was collected. The residue was washed with water, dried, and ground. Then, the residue was added to 180 mL of anhydrous ethanol, and 45 g of a 40 wt% ethanol solution of n-butyl titanate was added dropwise thereto. After the addition was completed, the mixture was reacted at room temperature for 5 h, 100 g of water was added, the mixture was stirred at 700 rpm for 15 min, and then allowed to stand for 18 h. The mixture was centrifuged at 2000 rpm for 5 min, and the solid matter was collected. The solid matter was washed with anhydrous ethanol and then calcined in a muffle furnace at 500 °C for 2 h to obtain porous bentonite.
[0045] (2) ultrasonically dispersing 10 g of graphene oxide in 600 mL of water to obtain a graphene oxide suspension; adding 80 mL of a 2 mol / L silver nitrate aqueous solution and stirring to mix evenly; adding 10 mL of a 2 mol / L sodium hydroxide aqueous solution and mixing to obtain a mixed solution; transferring the mixed solution into a high-pressure reactor and subjecting it to a hydrothermal reaction at 200° C. for 5 h; after the reaction is completed, cooling to room temperature, filtering, collecting solids, washing the solids with water, drying, and calcining at 700° C. for 2 h to obtain graphene-supported silver oxide;
[0046] (3) 6.8 g of graphene-loaded silver oxide, 4.6 g of porous bentonite, and 200 mL of anhydrous methanol were mixed and stirred evenly, and then ultrasonically treated at 200 W, 20 kHz, and room temperature for 10 min, heated to 80° C., 1.8 g of KH550 silane coupling agent was added, and the mixture was stirred for 2 h. After the reaction was completed, the mixture was cooled to room temperature and the filter cake was collected by filtration. The filter cake was dried to obtain the composite nanomaterial.
[0047] Example 2
[0048] A production process of spunlace-hot-rolled nonwoven fabrics, comprising the following steps:
[0049] S1. Unpack 300g PVA fiber and 100g polypropylene fiber and feed them into an air pressure automatic cotton box. The air pressure automatic cotton box processes the fibers into uniform sieved cotton and then feeds them into a carding machine. The carding machine humidifies the sieved cotton into a cotton web to obtain an A-layer cotton web, and controls the moisture content of the cotton web to be 20%;
[0050] S2, unpacking 200g of flax fiber and 100g of polypropylene fiber and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then cross-lays the web to obtain a B-layer cotton web;
[0051] S3. After the polypropylene fiber cloth is fed through the material roll, it is hydroentangled with the B layer cotton net and rolled flat, and then placed in the finishing agent for finishing with the A layer cotton net. The pressure of the hydroentanglement process is 6MPa, and the water needle aperture is 0.3mm. After finishing, it is glued to obtain a composite layer, and then the composite is pre-baked. The pre-baking makes the dryness of the whole cloth controlled at 60%, and then it is hot-rolled at 180℃ and rolled up. After passing the inspection, it is packaged and shipped out.
[0052] The steps in step S3 are as follows:
[0053] Add 10 g of sodium polyacrylate, 10 g of sodium dodecyl sulfate and 5 g of triethylamine to 500 parts of water, stir and mix evenly to obtain a mixed solution, add 10 g of composite nanomaterial to the mixed solution, stir at 1500 rpm for 30 min, and then ultrasonically treat at 1000 W for 15 min to obtain a finishing agent; immerse the fabric in the finishing agent for 15 min, and then take out, dehydrate, shape and dry.
[0054] The preparation method of the composite nanomaterial comprises the following steps:
[0055] (1) 13 g of bentonite was added to 250 mL of 25 wt% sodium dodecyl sulfate aqueous solution, stirred at 70 ° C for 8 h, cooled to room temperature after stirring, filtered, and the filter residue was collected. The filter residue was washed with water, dried, ground, and then added to 180 mL of anhydrous ethanol, into which 45 g of 40 wt% ethanol solution of n-butyl titanate was added dropwise; after the addition was completed, the mixture was reacted at room temperature for 5 h, 100 mL of water was added, stirred at 700 rpm for 15 min, and then allowed to stand for 18 h, centrifuged at 2000 rpm for 5 min, and the solid was collected. The solid was washed with anhydrous ethanol and placed in a muffle furnace for calcination at 500 ° C for 2 h to obtain porous bentonite;
[0056] (2) ultrasonically dispersing 10 g of graphene oxide in 600 mL of water to obtain a graphene oxide suspension; adding 80 mL of a 2 mol / L silver nitrate aqueous solution and stirring to mix evenly; adding 10 mL of a 2 mol / L sodium hydroxide aqueous solution and mixing to obtain a mixed solution; transferring the mixed solution into a high-pressure reactor and subjecting it to a hydrothermal reaction at 200° C. for 5 h; after the reaction is completed, cooling to room temperature, filtering, collecting solids, washing the solids with water, drying, and calcining at 700° C. for 2 h to obtain graphene-supported silver oxide;
[0057] (3) 6.8 g of graphene-loaded silver oxide, 4.6 g of porous bentonite, and 200 mL of anhydrous methanol were mixed and stirred evenly, and then ultrasonically treated at 200 W, 20 kHz, and room temperature for 10 min, heated to 80° C., 1.8 g of KH550 silane coupling agent was added, and the mixture was stirred for 2 h. After the reaction was completed, the mixture was cooled to room temperature and the filter cake was collected by filtration. The filter cake was dried to obtain the composite nanomaterial.
[0058] Example 3
[0059] A production process of spunlace-hot-rolled nonwoven fabrics, comprising the following steps:
[0060] S1. After unpacking 400g of PVA fiber and 150g of polypropylene fiber, feed the cotton into an air pressure automatic cotton box. The air pressure automatic cotton box processes the fiber into uniform sieved cotton and then feeds it to a carding machine. The carding machine makes the sieved cotton into a cotton web and then humidifies it to obtain an A-layer cotton web, and the moisture content of the cotton web is controlled to be 40%;
[0061] S2, unpacking 300g cotton fiber and 200g polypropylene fiber and feeding them into an air pressure automatic cotton box, which processes the sieved cotton into uniform sieved cotton and then feeds it to a carding machine; the carding machine makes the fibers into a cotton web and then cross-lays the web to obtain a B-layer cotton web;
[0062] S3. Feed the polyester fiber cloth through the material roll, perform hydroentanglement composite with the B-layer cotton mesh, and then place it in the finishing agent with the A-layer cotton mesh for finishing. The pressure of the hydroentanglement process is 8MPa, and the aperture of the water needle is 0.3-0.4mm. After finishing, glue is used to bond the composite layer, and then pre-bake the composite material to control the dryness of the whole cloth at 80%. Then, hot-roll the composite material at 190℃ and then roll it up. After passing the inspection, it will be packaged and shipped out.
[0063] The steps in step S3 are as follows:
[0064] Add 20 g of sodium polyacrylate, 30 g of sodium dodecyl sulfate and 35 g of triethylamine to 800 parts of water, stir and mix evenly to obtain a mixed solution, add 14 g of composite nanomaterial to the mixed solution, stir at 2000 rpm for 40 min, and then ultrasonically treat at 1100 W for 15 min to obtain a finishing agent; immerse the fabric in the finishing agent for 15 min, and then take out, dehydrate, shape and dry.
[0065] The preparation method of the composite nanomaterial comprises the following steps:
[0066] (1) 13 g of bentonite was added to 250 mL of 25 wt% sodium dodecyl sulfate aqueous solution, stirred at 70 ° C for 8 h, cooled to room temperature after stirring, filtered, and the filter residue was collected. The filter residue was washed with water, dried, ground, and then added to 180 mL of anhydrous ethanol, into which 45 g of 40 wt% ethanol solution of n-butyl titanate was added dropwise; after the addition was completed, the mixture was reacted at room temperature for 5 h, 100 mL of water was added, stirred at 700 rpm for 15 min, and then allowed to stand for 18 h, centrifuged at 2000 rpm for 5 min, and the solid was collected. The solid was washed with anhydrous ethanol and placed in a muffle furnace for calcination at 500 ° C for 2 h to obtain porous bentonite;
[0067] (2) ultrasonically dispersing 10 g of graphene oxide in 600 mL of water to obtain a graphene oxide suspension; adding 80 mL of a 2 mol / L silver nitrate aqueous solution and stirring to mix, adding 10 mL of a 2 mol / L sodium hydroxide aqueous solution and mixing to obtain a mixed solution, transferring the mixed solution into a high-pressure reactor, and subjecting the mixed solution to a hydrothermal reaction at 200° C. for 5 h; after the reaction is completed, cooling to room temperature, filtering, collecting solids, washing the solids with water, drying, and calcining at 700° C. for 2 h to obtain graphene-supported silver oxide;
[0068] (3) 6.8 g of graphene-loaded silver oxide, 4.6 g of porous bentonite, and 200 mL of anhydrous methanol were mixed and stirred evenly, and then ultrasonically treated at 200 W, 20 kHz, and room temperature for 10 min, heated to 80° C., 1.8 g of KH550 silane coupling agent was added, and the mixture was stirred for 2 h. After the reaction was completed, the mixture was cooled to room temperature and the filter cake was collected by filtration. The filter cake was dried to obtain the composite nanomaterial.
[0069] Comparative Example 1
[0070] A production process of spunlace-hot-rolled non-woven fabric, the implementation steps are similar to those of Example 1, the difference being that the composite nanomaterial used is graphene-loaded silver oxide.
[0071] Comparative Example 2
[0072] A production process of spunlace-hot-rolled nonwoven fabric, the implementation steps are similar to those of Example 1, the difference is that the composite nano material used is porous bentonite.
[0073] Comparative Example 3
[0074] A production process of spunlace-hot-rolled non-woven fabric, the implementation steps are similar to those of Example 1, the difference is that the nano material used is silver oxide.
[0075] Comparative Example 4
[0076] A production process of spunlace-hot-rolled non-woven fabric, the implementation steps are similar to those of Example 1, the difference is that the nano material used is nano titanium dioxide.
[0077] Test Case
[0078] Antibacterial performance test:
[0079] The nonwoven fabrics obtained in Examples 1-3 were subjected to antibacterial tests with reference to the provisions of GB / T20944.3-2008 "Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method", using Escherichia coli AATCC 8099 and Staphylococcus aureus AATCC6538 as test strains. The test results are shown in Table 1:
[0080] Table 1 Test results of antibacterial properties of spunlace-hot-rolled nonwoven fabrics
[0081]
[0082] Flame retardant performance test:
[0083] According to the test method of GB / T5454-1997 "Textile Combustion Performance Test Oxygen Index Method", the limiting oxygen index of the embodiment and the comparative example was measured using a FYH830 critical oxygen index tester. The test results are shown in Table 2:
[0084] Table 2 Flame retardant test results of spunlace-hot-rolled nonwoven fabrics
[0085]
[0086] Tear resistance test:
[0087] With reference to GB / T3917.2-2009 "Tear properties of textile fabrics - Part 2: Determination of tear strength of trouser-shaped test specimens (single seam)", the tear resistance of the spunlaced-hot-rolled nonwoven fabrics obtained in various embodiments of the present invention and comparative examples was tested. The test results are shown in Table 3:
[0088] Table 3 Tear resistance test results of spunlace-hot-rolled nonwoven fabrics
[0089]
[0090] It can be seen from the experimental results in Tables 1 to 3 that the spunlace-hot-rolled non-woven fabric obtained in the embodiment of the present invention has excellent antibacterial, flame retardant and tear resistance. Compared with single-component silver oxide, titanium dioxide, graphene-loaded silver oxide, and porous bentonite, the porous bentonite combined with graphene-loaded silver oxide has the best performance. The possible reason is that the graphene-loaded silver oxide enters the mesopores of the bentonite, which improves the stability and durability of the porous bentonite. The composite nanomaterial with more action sites has better bacteria-killing performance under the synergistic adsorption of graphene and porous bentonite; and porous bentonite, as a nanomaterial, is easily broken during the hot rolling process, resulting in a decrease in its mechanical properties, and the nano antibacterial agent obtained in the embodiment can be deposited in the gap between fibers and is well combined with the fibers during the hot rolling process, making the structure between the fibers more compact, thereby improving the mechanical properties and flame retardant properties of the material.
[0091] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0092] The above embodiments are only preferred technical solutions of the present invention and should not be regarded as limiting the present invention. The protection scope of the present invention shall be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.
Claims
1. A production process for spunlace-hot-rolled nonwoven fabric, characterized in that: The steps include: S1, unpacking the A-side fibers and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then performs a humidification treatment to obtain an A-layer cotton web; S2, unpacking the B-side fibers and feeding them into an air pressure automatic cotton box, which processes the fibers into uniform sieved cotton and then feeds them into a carding machine; the carding machine makes the sieved cotton into a cotton web and then cross-lays the web to obtain a B-layer cotton web; S3, after the C layer grey cloth is fed through the material roll, it is hydroentangled with the B layer cotton net and flattened, and then it is placed in the finishing agent for finishing with the A layer cotton net. After finishing, it is glued with glue to obtain a composite layer, and then the composite layer is pre-baked, and then combined by hot rolling and rolled, and then packaged and shipped after passing the inspection; In step S1, the A-side fiber is a mixed fiber of water-soluble fiber and low-melting-point fiber; In the step S2, the fiber on the B side is a mixed fiber of plant fiber and low melting point fiber; The steps in step S3 are as follows: Add 1-3 parts of sodium polyacrylate, 1-5 parts of sodium dodecyl sulfate and 0.5-1.5 parts of triethylamine to 50-100 parts of water, stir and mix evenly to obtain a mixed solution, add 1-2 parts of composite nanomaterial to the mixed solution, stir rapidly for 30-50 minutes and then perform ultrasonic treatment to obtain a finishing agent; immerse the fabric in the finishing agent for 10-15 minutes, then take out, dehydrate, shape and dry; The preparation method of the composite nanomaterial comprises the following steps: (1) adding 10-18 parts by weight of bentonite to an aqueous solution of sodium dodecyl sulfate, heating and stirring, cooling to room temperature, filtering, collecting the filter residue, washing the filter residue with water, drying, grinding, and then adding it to anhydrous ethanol, to which 40-60 parts by weight of an ethanol solution of n-butyl titanate is added dropwise; after the addition is complete, reacting at room temperature, adding 50-150 parts by weight of water, stirring, standing, centrifuging, collecting solids, washing the solids, and calcining them in a muffle furnace to obtain porous bentonite; (2) ultrasonically dispersing 7-15 parts by weight of graphene oxide in water to obtain a graphene oxide suspension; adding 50-150 parts by weight of an aqueous silver nitrate solution and stirring the mixture evenly; adding an aqueous NaOH solution and mixing the mixture to obtain a mixed solution; transferring the mixed solution into a high-pressure reactor for a hydrothermal reaction; after the reaction is completed, cooling to room temperature, filtering, collecting solids, washing the solids with water, drying, and then calcining to obtain graphene-loaded silver oxide; (3) 5-10 parts by weight of graphene-loaded silver oxide, 3-6 parts by weight of porous bentonite, and anhydrous methanol are mixed and stirred evenly, then ultrasonically treated, heated, and 1.5-3.5 parts by weight of KH550 silane coupling agent are added, stirred for reaction, and after the reaction is completed, cooled and filtered to collect the filter cake, and the filter cake is dried to obtain the composite nanomaterial.
2. The production process according to claim 1, characterized in that: The water-soluble fiber is one or more of PVA fiber, seaweed fiber, carboxymethyl cellulose fiber and polyacrylamide fiber.
3. The production process according to claim 1, characterized in that: In the step S1, the fibers on the A side are humidified after forming a cotton web, and the moisture content is controlled at 25-40%.
4. The production process according to claim 1, characterized in that: The plant fiber is one or more of cotton fiber, flax fiber and bamboo fiber.
5. The production process according to claim 1, characterized in that: In the step S3, the C layer grey cloth is one of polyester fiber, nylon fiber and polypropylene fiber.
6. A spunlace-hot-rolled nonwoven fabric, characterized in that: The product is produced by the production process described in any one of claims 1 to 5.