A synchronous double-liquid grouting slurry and construction method for an ultra-large diameter shield tunnel
By using a dual-liquid grouting system with modified water glass and nano-alumina fibers in the construction of super-large diameter shield tunnels, the problems of grouting pipelines and unstable material performance are solved, and efficient and stable injections are achieved The slurry effect reduces construction risks and costs.
Patent Information
- Application Number
- CN202411186222.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-28
AI Technical Summary
In the existing synchronous double-liquid grouting construction methods, there are problems such as easy blockage of grouting pipe lines, unstable performance of double-liquid slurry materials, chaotic processes, and difficult to control construction quality. Especially in the construction of super-large diameter shield tunnels, the pipe sheets are floating, Water leakage, cracks and other diseases.
A dual-liquid grouting system including A slurry and B slurry, wherein A slurry consists of cement, bentonite, stabilizer and water. B slurry is composed of modified water glass, aqueous epoxy resin, aqueous epoxy curing agent, nano-alumina The fiber and hydrophobic vapor phase silica are composed of which improves the heat resistance, sealing and anti-seepage properties of the material through modification treatment, ensuring rapid gel formation and uniform grouting.
It effectively solves the problems of pipe sheet floating, water leakage and axis offset, improves the sealing and waterproof performance of grouting, shortens construction time, reduces costs, and improves the molding quality of the tunnel.
Smart Images

Figure CN118702473B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tunnel grouting, and relates to a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel and a construction method. Background Art
[0002] Shield tunnel construction is a method of building tunnels in the ground using a shield machine, which mainly includes soil excavation and excavation face support, shield advancement and lining assembly, shield tail emptying and wall back grouting and other major technical links. Among them, wall back grouting is to fill the construction gap formed by the shield tail with grouting to reduce the foundation stress release and ground deformation caused by the shield tail gap, which is one of the important links in shield construction.
[0003] The synchronous grouting materials used in the shield tunnel construction process include single-liquid slurry and double-liquid slurry. In the construction of super-large diameter shield tunnels, single-liquid slurry is generally used as the synchronous grouting material, and the single-liquid slurry is usually composed of water, cement, river sand, bentonite, admixtures, etc. However, in actual construction, it is found that the single-liquid slurry has the problem of long coagulation time and is difficult to control. At the same time, due to the presence of a certain amount of flowing groundwater in the stratum through which the shield machine passes, the single-liquid slurry will also have undesirable phenomena such as slurry not gelling, incomplete grouting, and slurry leakage, which will further induce the floating of the pipe segment, causing pipe segment misalignment, water leakage, cracks and other diseases.
[0004] The synchronous double-liquid grouting slurry is a slurry formed by mixing liquid A and liquid B in a certain volume ratio, wherein liquid A is generally a cement-based pure slurry composed of cement, stabilizer, etc., and liquid B is generally composed of water glass. The advantage of synchronous double-liquid grouting to fill the gap at the shield tail is that the slurry is quickly formed, the total amount of double-liquid slurry required is limited, and the overall grouting cost is reduced. In addition, the time of the synchronous double-liquid grouting operation is shortened, which helps to speed up the overall advancement speed of the shield and thus shorten the construction period. However, the existing synchronous double-liquid grouting construction method has technical problems such as easy blockage of the grouting pipeline, unstable performance of the double-liquid slurry material, chaotic process, and difficult control of construction quality. Therefore, there are currently few ultra-large diameter shield tunnel projects in China that use double-liquid slurry for synchronous grouting operations. Summary of the invention
[0005] The purpose of the present invention is to provide a synchronous double-liquid grouting slurry and a construction method for an ultra-large diameter shield tunnel, so as to solve the problems existing in the existing synchronous double-liquid grouting construction method, such as easy blockage of the grouting pipeline, unstable performance of the double-liquid slurry material, chaotic process, and difficult control of construction quality.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] The present application provides a super-large diameter shield tunnel synchronous double-liquid grouting slurry, which includes slurry A and slurry B. Among them, slurry A includes cement, bentonite, stabilizer and water, and slurry B includes modified water glass, water-based epoxy resin, water-based epoxy curing agent, modified or unmodified nano alumina fiber, and hydrophobic fumed silica.
[0008] In this application, cement is selected from silicate cement, ordinary silicate cement, slag silicate cement, pozzolanic silicate cement, fly ash silicate cement or composite silicate cement, and the strength grade of cement is ≥42.5. When using, agglomerated cement should not be used, cements of different brands, varieties and strength grades should not be mixed; cement that has been out of the factory for more than 3 months should not be used.
[0009] The bentonite is sodium-based bentonite, which has the characteristics of high water absorption, large expansion multiple, strong ion exchange capacity and adsorption capacity, good dispersibility in water, high colloid value, strong adhesion and good thermal stability. The quality indicators of the sodium-based bentonite used in this application are: viscosity ≥60mPa•s at 600r / min, dynamic plastic ratio ≤1.5Pa / (mPa•s), filtration loss ≤14.0cm 3 , 75μm sieve residue ≤1.5%, moisture content ≤13.0%.
[0010] Sodium bentonite can absorb cations and some small molecular ions in cement, and promote the reaction between ions and cement to form hydration products, thereby improving the early strength of cement. Sodium bentonite can also absorb and fix water and organic matter in cement, promote self-assembly and crystallization between particles, and form composite particles. These composite particles can improve the density, strength, toughness and stability of A slurry. In addition, sodium bentonite can also control the flow of water, reduce the permeability of A slurry, and thus reduce the permeability of cement concrete.
[0011] The stabilizer in the present application is a composite retarder, and specifically selected from existing stabilizers that can increase viscosity, thicken, increase plasticity or not disperse underwater to improve the stability of slurry A. At the same time, the specific selection of the composite retarder also needs to meet the technical requirements of the setting time of slurry A. More preferably, the composite retarder in the present application is selected from lignin sulfonate and its derivatives, hydroxycarboxylates, borax, sodium hexametaphosphate, alkyl phosphates, etc., wherein hydroxycarboxylates include lactate, β-hydroxybutyrate, potassium sodium tartrate, citrate or sodium salicylate, etc.
[0012] The water in this application can be tap water or fully oxidized surface water.
[0013] The modified water glass in the present application is prepared from organosilicon-modified phenolic resin and water glass. Organosilicon resin has excellent heat resistance and moisture resistance, good mechanical properties, heat resistance, acid resistance, and good chemical stability. The heat resistance and water resistance of the phenolic resin can be further improved by reacting the organosilicon monomer with the phenolic hydroxyl group or hydroxymethyl group in the phenolic resin, thereby obtaining an organosilicon-modified phenolic resin with good heat resistance, adhesion, water resistance, and ablation resistance.
[0014] Water glass is a soluble inorganic silicate with strong bonding force, and is usually used as a binder. Modification of water glass by organic silicon modified phenolic resin can make water glass heat resistant, water resistant, and ablation resistant, and can also further enhance bonding, greatly improve the performance of water glass, and improve the performance of cement concrete formed after B slurry grouting and solidification.
[0015] The preparation method of modified water glass in the present application includes: dissolving organosilicon-modified phenolic resin in organic solvents such as acetone and alcohol, adding silane coupling agent, stirring evenly to obtain a mixed solution; adding water glass to the mixed solution, stirring and reacting at 60°C to obtain modified water glass. The mass ratio of organosilicon-modified phenolic resin to water glass is (1-5): 100; the amount of organic solvent added is based on the complete dissolution of organosilicon-modified phenolic resin; the silane coupling agent is one of KH550 or KH560, and the added amount is 1-2% of the mass of organosilicon-modified phenolic resin. The modulus of water glass used in the present application is 2.65-3.40, and the concentration is 35-45°Bé.
[0016] Nano-alumina fiber is a polycrystalline inorganic fiber whose main component is alumina. It has outstanding high temperature resistance, low density and small heat capacity. After adding nano-alumina fiber to the B slurry, it can enhance the heat resistance of cement concrete formed after grouting and solidification, and at the same time reduce the weight of cement concrete to prevent collapse in the tunnel due to excessive weight.
[0017] Furthermore, the present application may also use nano-alumina fibers modified with perfluorosilane. The nano-alumina fibers modified with perfluorosilane can enhance the hydrophobicity and corrosion resistance of the nano-alumina fibers, thereby enhancing the hydrophobicity of the B slurry.
[0018] The preparation method of modified nano alumina fiber in the present application includes:
[0019] Adding nano-alumina fibers into anhydrous ethanol and performing ultrasonic dispersion to obtain a dispersion; wherein the mass volume ratio of the nano-alumina fibers to the anhydrous ethanol is 1:25;
[0020] 1H,1H,2H,2H-perfluoroalkyltrialkoxysilane and tetraethyl orthosilicate are subjected to a sol-gel reaction at 80-100° C. to obtain a gel solution; wherein the mass ratio of 1H,1H,2H,2H-perfluoroalkyltrialkoxysilane to tetraethyl orthosilicate is 1:(1-2);
[0021] The dispersion and gel solution were mixed evenly and stirred for reaction for 5 hours. After the reaction, the mixed solution was centrifuged at a spinning speed of 6000-8000 r / min and a temperature of 250°C to obtain modified nano alumina fibers.
[0022] The hydrophobic fumed silica in the present application is prepared by using hydrophilic fumed silica and active silanes such as chlorosilane or hexamethyldisilane, and has hydrophobicity. After adding hydrophobic fumed silica to the B slurry, the hydrophobic fumed silica particles with smaller particle size can form a network structure, inhibit the flow of water-based epoxy resin, accelerate the curing speed of the B slurry, and improve the bonding effect; at the same time, due to the small size of the hydrophobic fumed silica, this will increase the sealing and impermeability of the B slurry, thereby improving the sealing and impermeability of the cement concrete formed after the B slurry is grouted and solidified.
[0023] In the present application, after slurry A and slurry B are synchronously grouted in the gap at the tail of the shield, hydrophobic fumed silica, modified water glass, water-based epoxy resin and cement can react quickly to form gel, greatly shortening the gel curing time of concrete. At the same time, the generated gel can fully fill the grouting circle and form a uniform and substantial cylindrical grouting body behind the segment, so that the force borne by the segment lining structure is more balanced, which can effectively control the formation settlement deformation, inhibit the segment from floating, control the segment posture, and thus significantly reduce the probability of segment misalignment, cracking, water leakage and axis deviation. At the same time, the use of bentonite, modified or unmodified nano-alumina fiber and hydrophobic fumed silica can improve the sealing, impermeability, hydrophobicity and corrosion resistance of concrete, so that the cylindrical grouting body forms a waterproof layer with good sealing, which helps to reduce the erosion of groundwater on the segment structure and provides safety for the construction and later operation and maintenance of shield tunnels.
[0024] More preferably, in the synchronous double-liquid grouting slurry for ultra-large diameter shield tunnel provided in the present application, slurry A includes 230-400 parts of cement, 30-50 parts of bentonite, 3-5 parts of stabilizer and 790-860 parts of water in parts by weight, and slurry B includes 50-90 parts of modified water glass, 50-90 parts of water-based epoxy resin, 15-30 parts of water-based epoxy curing agent, 40-80 parts of modified nano-aluminum oxide fiber, and 40-80 parts of modified fumed silica in parts by weight.
[0025] More preferably, in the synchronous double-liquid grouting slurry for ultra-large diameter shield tunnel provided in the present application, slurry A includes 350 parts of cement, 45 parts of bentonite, 5 parts of stabilizer and 820 parts of water in parts by weight; slurry B includes 70 parts of modified water glass, 70 parts of water-based epoxy resin, 22 parts of water-based epoxy curing agent, 65 parts of modified or unmodified nano alumina fibers, and 65 parts of hydrophobic fumed silica in parts by weight.
[0026] In addition, the present application also provides a method for synchronous double-liquid grouting construction of an ultra-large diameter shield tunnel, the method comprising:
[0027] After the bentonite and water are mixed, stabilizer and cement are added in sequence and mixed evenly to form slurry A;
[0028] After mixing the waterborne epoxy resin and the waterborne epoxy curing agent, add the modified water glass, modified or unmodified nano alumina fiber, and hydrophobic fumed silica, mix well, and form a B slurry;
[0029] When the shield machine advances at a stable speed, the A slurry is automatically injected, and the B slurry is injected 10 seconds after the A slurry is injected, so as to realize dual-liquid synchronous grouting;
[0030] When the shield machine stops advancing, the injection of the B slurry is stopped 1 minute in advance, and the injection of the A slurry is stopped 10 seconds after the injection of the B slurry is stopped;
[0031] The A slurry in the slurry pipe is flushed with flowing clean water.
[0032] The present invention has the following beneficial effects:
[0033] (1) Sodium bentonite can absorb cations and some small molecular ions in cement, and promote the reaction between ions and cement to form hydration products, thereby improving the early strength of cement. Sodium bentonite can also absorb and fix water and organic matter in cement, promote self-assembly and crystallization between particles, improve the density, strength, toughness and stability of A slurry, and reduce the permeability of A slurry.
[0034] (2) Modifying water glass with organosilicon-modified phenolic resin can enhance the heat resistance, water resistance, ablation resistance and adhesion of water glass, and improve the performance of cement concrete formed after grouting and solidification of B slurry.
[0035] (3) Adding nano-alumina fibers to slurry B can enhance the heat resistance of cement concrete formed after grouting and solidification. It can also reduce the weight of cement concrete and prevent the tunnel from collapsing due to excessive weight.
[0036] (4) The perfluorosilane-modified nano-alumina fibers can also enhance the hydrophobicity and corrosion resistance of the nano-alumina fibers, thereby enhancing the hydrophobicity of slurry B.
[0037] (5) After adding hydrophobic fumed silica to slurry B, the smaller hydrophobic fumed silica particles can form a network structure, inhibit the flow of water-based epoxy resin, accelerate the curing speed of slurry B, and improve the bonding effect; at the same time, due to the smaller size of hydrophobic fumed silica, this will increase the sealing and impermeability of slurry B, thereby improving the sealing and impermeability of cement concrete formed after grouting and solidification of slurry B.
[0038] (6) After the synchronous double-liquid grouting slurry is injected into the gap at the tail of the shield, it can quickly consolidate the segment lining structure, reduce the buoyancy of the segment and the surface settlement, and reduce the segment misalignment, cracking, water leakage and other defects. It can also assist the stress of the segment lining structure and enhance the waterproof ability of the segment lining structure, thus comprehensively improving the quality of the formed tunnel.
[0039] (7) Compared with the traditional synchronous single-liquid grouting, this construction method can save the cost of synchronous grouting, reduce the grouting time, ensure the quality of the formed tunnel, and shorten the construction period. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A construction process diagram of the synchronous double-liquid grouting construction method for an ultra-large diameter shield tunnel provided in an embodiment of the present application. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is further explained and illustrated by means of specific embodiments below.
[0042] Example 1
[0043] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 350 parts of silicate cement, 45 parts of sodium bentonite, 5 parts of potassium sodium tartrate and 820 parts of water in parts by weight; slurry B comprises 70 parts of modified water glass, 70 parts of water-based epoxy resin, 22 parts of water-based epoxy curing agent, 65 parts of modified nano-alumina fiber, and 65 parts of hydrophobic fumed silica in parts by weight.
[0044] The present application also provides a method for synchronous double-liquid grouting construction of a super-large diameter shield tunnel, as shown in the attached Figure 1 As shown, the construction method includes:
[0045] S101: After bentonite and water are mixed, stabilizer and cement are added in sequence and mixed evenly to form slurry A.
[0046] The bentonite slurry making unit automatically completes the slurry preparation by setting the preparation parameters through the terminal controller, and quantitatively delivers it to the A slurry slurry making machine through the bentonite pump. The A slurry slurry making machine automatically adds a certain amount of clean water and mixes it according to the feedback electrical signal, then automatically adds a certain amount of stabilizer potassium sodium tartrate, and finally automatically adds a certain amount of cement powder through the screw conveyor, automatically mixes and stirs at high speed to form A slurry.
[0047] The prepared A slurry was stored in 4 sets of 2.4m 3 Each set of A slurry pulping unit uses a 40m 3 / h transfer hose pump for transportation, a total of 4 sets of A slurry pulping units, with a simultaneous transfer and transportation capacity of 160m 3 / h. Each two A slurry transfer hose pumps output to a volume of 15m 3 The slurry is temporarily stored in the temporary storage mixing tank, and the same model A slurry hose pump as the A slurry pump is used. After the A slurry is grouted, it is pumped into the tank truck through the reserved pipeline. A total of 6 10m 3 The prepared A slurry is transported by a tank truck, pumped into the tank truck at the auxiliary wellhead, and then transported to the transfer pump at the tail of the shield machine, and pumped to the slurry storage tank on the first floor of the No. 1 trolley by the transfer pump for storage.
[0048] S102: After mixing the water-based epoxy resin and the water-based epoxy curing agent, add modified water glass, nano-alumina fiber, and hydrophobic fumed silica, mix evenly, and form a B slurry.
[0049] The water glass pulping unit automatically completes the slurry preparation by setting the preparation parameters through the terminal controller, and conveys a certain amount of water-based epoxy resin to the B slurry pulping machine through the water glass pump. The B slurry pulping machine automatically adds a certain amount of water-based epoxy curing agent and mixes it according to the feedback electrical signal, and then automatically adds a certain amount of modified water glass, nano-alumina fiber, and hydrophobic fumed silica through the screw conveyor, and automatically mixes and stirs at high speed to form B slurry.
[0050] In an embodiment of the present application, the preparation method of modified water glass includes: dissolving organosilicon-modified phenolic resin in acetone, adding silane coupling agent KH550, and stirring to obtain a mixed solution. The amount of silane coupling agent KH550 added is 2% of the mass of the organosilicon-modified phenolic resin. Add water glass to the mixed solution, stir and react at 60°C to obtain modified water glass. The mass ratio of organosilicon-modified phenolic resin to water glass is 5:100, the modulus of water glass is 3.25, and the concentration is 40°Bé.
[0051] In an embodiment of the present application, a method for preparing modified nano-alumina fibers includes: adding nano-alumina fibers to anhydrous ethanol, ultrasonically dispersing, and obtaining a dispersion; wherein the mass volume ratio of the nano-alumina fibers to the anhydrous ethanol is 1:25; subjecting 1H, 1H, 2H, 2H-perfluoroalkyltrialkoxysilane and tetraethyl orthosilicate to a sol-gel reaction at 90°C to obtain a gel solution; wherein the mass ratio of 1H, 1H, 2H, 2H-perfluoroalkyltrialkoxysilane and tetraethyl orthosilicate is 1:1.5; mixing the dispersion and the gel solution evenly, and stirring the reaction for 5 hours; after the reaction is completed, the mixed solution is centrifuged at a spinning speed of 7000 r / min and a temperature of 250°C to obtain modified nano-alumina fibers.
[0052] The prepared B slurry was washed with 5 20m 3 PE plastic barrels are used for storage. Each plastic barrel is equipped with a B slurry pump with a slurry delivery capacity of 5m 3 / h. Among them, 3 plastic barrels are used as temporary storage containers, and the other 2 plastic barrels and delivery pumps are used as the main system for underground delivery of B slurry. The temporary storage container can add B slurry to the 2 working B slurry plastic barrels through the delivery pump. The B slurry is transported by the segment truck, which can transport 17.5m of B slurry at a time. 3 .
[0053] S103: When the advancing speed of the shield machine is stable, the A slurry is automatically injected, and the B slurry is injected 10 seconds after the A slurry is injected, so as to realize the synchronous grouting of two liquids.
[0054] The synchronous dual-liquid grouting system is associated with the tunneling system of the shield machine, and the system is equipped with an automatic alarm function. When the synchronous dual-liquid grouting system is in the initial state, the push rod is pushed to extend it into place, and the piston closes the grouting port of the shield tail to prevent external slurry and debris from entering the grouting pipe. The A liquid pipe and the backwash water pipe are filled with clean industrial water left after the previous process is completed. The advancement of the shield machine is 20-30mm / min. When the advancement speed of the shield machine is stable, the A slurry is automatically injected through the A liquid pipe, and the push rod is retracted into place at the same time, that is, the grouting port of the shield tail is opened after the piston is retracted. After the A slurry is injected for 10s, the B slurry is automatically injected through the B liquid pipe. At this time, the A slurry and the B liquid pipe are mixed at the B liquid nozzle to become a uniform cementitious material, namely, dual liquid slurry. The dual liquid grouting is carried out while the shield machine is advancing, that is, dual liquid synchronous grouting.
[0055] S104: When the shield machine stops advancing, the injection of the B slurry is stopped 1 minute in advance, and the injection of the A slurry is stopped 10 seconds after the injection of the B slurry is stopped.
[0056] S105: flushing the A slurry in the slurry pipe with flowing clean water.
[0057] After the injection of A slurry stops, the synchronous dual-liquid slurry injection system sends a feedback signal. At this time, the push rod automatically extends into place, pushing the remaining cementitious material in the grouting pipe out of the grouting port, and then starts the backwashing function of the grouting system to automatically flush the A slurry in the grouting pipe with flowing clean water, keeping the pipeline clean and preventing pipeline blockage.
[0058] Example 2
[0059] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 230 parts of ordinary Portland cement, 50 parts of bentonite, 3 parts of borax and 790 parts of water in parts by weight; slurry B comprises 50 parts of modified water glass, 50 parts of water-based epoxy resin, 30 parts of water-based epoxy curing agent, 80 parts of nano-alumina fiber, and 40 parts of hydrophobic fumed silica in parts by weight.
[0060] The method for preparing the synchronous dual-liquid grouting slurry for the ultra-large diameter shield tunnel provided in the embodiment of the present application is the same as that in Example 1.
[0061] Example 3
[0062] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 400 parts of slag silicate cement, 30 parts of bentonite, 3 parts of borax and 860 parts of water in parts by weight; slurry B comprises 90 parts of modified water glass, 90 parts of water-based epoxy resin, 15 parts of water-based epoxy curing agent, 40 parts of nano-alumina fiber, and 80 parts of hydrophobic fumed silica in parts by weight.
[0063] The method for preparing the synchronous dual-liquid grouting slurry for the ultra-large diameter shield tunnel provided in the embodiment of the present application is the same as that in Example 1.
[0064] Example 4
[0065] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 300 parts of volcanic ash silicate cement, 30-50 parts of bentonite, 3-5 parts of sodium hexametaphosphate and 790-860 parts of water in parts by weight; slurry B comprises 50-90 parts of modified water glass, 50-90 parts of water-based epoxy resin, 15-30 parts of water-based epoxy curing agent, 40-80 parts of modified or unmodified nano alumina fibers, and 40-80 parts of hydrophobic fumed silica in parts by weight.
[0066] The method for preparing the synchronous dual-liquid grouting slurry for the ultra-large diameter shield tunnel provided in the embodiment of the present application is the same as that in Example 1.
[0067] Example 5
[0068] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 230-400 parts of fly ash silicate cement, 30-50 parts of bentonite, 3-5 parts of sodium hexametaphosphate and 790-860 parts of water in parts by weight; slurry B comprises 50-90 parts of modified water glass, 50-90 parts of water-based epoxy resin, 15-30 parts of water-based epoxy curing agent, 40-80 parts of modified nano alumina fiber, and 40-80 parts of hydrophobic fumed silica in parts by weight.
[0069] The method for preparing the synchronous dual-liquid grouting slurry for the ultra-large diameter shield tunnel provided in the embodiment of the present application is the same as that in Example 1.
[0070] Example 6
[0071] An embodiment of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, the slurry comprising slurry A and slurry B, wherein slurry A comprises 230-400 parts of silicate cement, 30-50 parts of bentonite, 3-5 parts of potassium sodium tartrate and 790-860 parts of water in parts by weight; slurry B comprises 50-90 parts of modified water glass, 50-90 parts of water-based epoxy resin, 15-30 parts of water-based epoxy curing agent, 40-80 parts of modified nano alumina fiber, and 40-80 parts of hydrophobic fumed silica in parts by weight.
[0072] The method for preparing the synchronous dual-liquid grouting slurry for the ultra-large diameter shield tunnel provided in the embodiment of the present application is the same as that in Example 1.
[0073] Comparative Example 1
[0074] The comparative example of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, which includes slurry A and slurry B, wherein slurry A includes 350 parts of silicate cement, 45 parts of sodium bentonite, 5 parts of potassium sodium tartrate and 820 parts of water in parts by weight; slurry B includes 70 parts by weight of water glass.
[0075] Comparative Example 2
[0076] The comparative example of the present application provides a synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, which includes slurry A and slurry B, wherein slurry A includes 350 parts of silicate cement, 45 parts of sodium bentonite, 5 parts of potassium sodium tartrate and 820 parts of water in parts by weight; slurry B includes 70 parts by weight of modified water glass.
[0077] The viscosity and 3h water bleeding rate of the A slurry and the B slurry prepared in Examples 1-6 and Comparative Examples 1 and 2 were measured in the examples of the present application, respectively, and Table 1 was obtained. At the same time, the chemical gelation time, physical initial setting time, physical final setting time, 1-day compressive strength, 7-day compressive strength and 28-day compressive strength of the double liquid grouting slurry prepared in Examples 1-6 and Comparative Examples 1 and 2 were measured after grouting, and Table 2 was obtained.
[0078] Table 1: Performance measurement results of slurry A and slurry B prepared in Examples 1-6
[0079]
[0080] As can be seen from Table 1, in Examples 1-6 of the present application, the viscosity of slurry A is 20-35s, and the 3h water seepage rate is 3-5%; while the viscosity of slurry B is 17-25 s, and the 3h water seepage rate is 1.8-3.2%. In Comparative Examples 1 and 2, the viscosity of slurry A is 29-31s, and the 3h water seepage rate is 4.3-4.7%; while the viscosity of slurry B is 10-12s, and the 3h water seepage rate is 7.8-8.1%. Compared with slurry A and slurry B prepared in Comparative Examples 1 and 2, the viscosity and 3h water seepage rate of slurry A in the examples of the present application are slightly different; the viscosity of slurry B is significantly increased, and the 3h water seepage rate is significantly reduced. It can be seen that the synchronous dual-liquid grouting slurry provided in the examples of the present application has good impermeability and high viscosity, and can effectively reduce the erosion of groundwater on the segment structure.
[0081] Table 2: Performance test results of the double liquid grouting slurry prepared in Examples 1-6 after grouting
[0082]
[0083] As can be seen from Table 2, the chemical gelation time of the double liquid grouting slurry prepared in the embodiment of the present application after grouting is 10-45s, the physical initial setting time is 2-3.5h, the physical final setting time is 3.5-5h, the compressive strength is 0.6-1.5MPa in 1 day, the compressive strength is 1-2.5MPa in 7 days, and the compressive strength is 1.5-3MPa in 28 days. The chemical gelation time of the double liquid grouting slurry prepared in Comparative Examples 1 and 2 after grouting is 10-45s, the physical initial setting time is 4.5-5.5h, the physical final setting time is 6.5-8h, the compressive strength is 0.2-0.3MPa in 1 day, the compressive strength is 0.5-1.2MPa in 7 days, and the compressive strength is 1-1.8MPa. Compared with the double liquid grouting slurry prepared in Comparative Examples 1 and 2, the chemical gelation time, physical initial setting time, and physical final setting time of the double liquid grouting slurry in the embodiment of the present application after grouting are greatly shortened, and at the same time, the 1-day compressive strength, 7-day compressive strength, and 28-day compressive strength are significantly enhanced. It can be seen that the synchronous double liquid grouting slurry provided in the embodiment of the present application can accelerate the curing time, shorten the construction time, and at the same time can also improve the compressive strength of the cement concrete formed after the grouting.
[0084] Examples
[0085] In the embodiment of the present application, the synchronous dual-liquid grouting slurry in Example 1 is applied to a specific tunnel construction section. The conditions of the tunnel construction section are as follows: the shield section is about 7.4 km long, and the strata traversed by the shield section tunnel are mainly fine sand layers, silt, medium-coarse sand, and a small amount of silty clay. The cover thickness is about 10 to 42 m, and the maximum water pressure is 0.58 MPa. The shield machine excavation diameter is 15.97 m, and the tunnel is constructed with an average cover thickness of 20 m.
[0086] Relevant data measurements were taken on the formed tunnel, and the measurement results were as follows: the pipe segment floated within -10-10mm; the pipe segment misalignment was mainly concentrated within 5mm, accounting for 80.6% of the total, with the maximum intra-ring misalignment of 7mm and the maximum inter-ring misalignment of 8mm; the back of the pipe segment was densely grouted, with a density of 100%; the tunneling efficiency of the shield machine was 1m / h. This shows that the synchronous double-liquid grouting slurry provided in the embodiment of the present application can fully fill the gap between the pipe segment and the surrounding rock, ensuring the timeliness of synchronous grouting, and at the same time, it also well controls the misalignment between and within the pipe segment rings.
[0087] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A synchronous double-liquid grouting slurry for an ultra-large diameter shield tunnel, characterized in that: The invention comprises slurry A and slurry B, wherein the slurry A comprises 230-400 parts of cement, 30-50 parts of bentonite, 3-5 parts of stabilizer and 790-860 parts of water in parts by weight; the slurry B comprises 50-90 parts of modified water glass, 50-90 parts of waterborne epoxy resin, 15-30 parts of waterborne epoxy curing agent, 40-80 parts of modified or unmodified nano alumina fiber and 40-80 parts of hydrophobic fumed silica in parts by weight, wherein the modified water glass is prepared from organosilicon-modified phenolic resin and water glass, and the modified nano alumina fiber is perfluorosilane-modified nano alumina fiber.
2. The synchronous double-liquid grouting slurry for super-large diameter shield tunnel according to claim 1 is characterized in that: It includes slurry A and slurry B. The slurry A includes 350 parts of cement, 45 parts of bentonite, 5 parts of stabilizer and 820 parts of water in parts by weight; the slurry B includes 70 parts of modified water glass, 70 parts of water-based epoxy resin, 22 parts of water-based epoxy curing agent, 65 parts of modified or unmodified nano alumina fiber, and 65 parts of hydrophobic fumed silica in parts by weight.
3. The synchronous double-liquid grouting slurry for super-large diameter shield tunnel according to claim 1 is characterized in that: The modulus of the water glass is 2.65-3.40, and the concentration is 35-45°Bé.
4. The synchronous double-liquid grouting slurry for super-large diameter shield tunnel according to claim 1 is characterized in that: The strength grade of the cement is ≥42.5, and the cement is selected from silicate cement, ordinary silicate cement, slag silicate cement, pozzolanic silicate cement, fly ash silicate cement or composite silicate cement.
5. The synchronous double-liquid grouting slurry for super-large diameter shield tunnel according to claim 1 is characterized in that: The bentonite is sodium-based bentonite, and the quality indicators of the sodium-based bentonite are: viscosity ≥ 60 mPa•s at 600 r / min, dynamic plastic ratio ≤ 1.5 Pa / (mPa•s), and filtration loss ≤ 14.0 cm 3 , 75μm sieve residue ≤1.5%, moisture content ≤13.0%.
6. The synchronous double-liquid grouting slurry for super-large diameter shield tunnel according to claim 1 is characterized in that: The stabilizer is a composite retarder.
7. A method for synchronous double-liquid grouting construction of an ultra-large diameter shield tunnel, characterized in that: Using the ultra-large diameter shield tunnel synchronous double-liquid grouting slurry described in claim 1, the method comprises: After the bentonite and water are mixed, stabilizer and cement are added in sequence and mixed evenly to form slurry A; After mixing the waterborne epoxy resin and the waterborne epoxy curing agent, add the modified water glass, modified or unmodified nano alumina fiber, and hydrophobic fumed silica, mix well, and form a B slurry; When the shield machine advances at a stable speed, the A slurry is automatically injected, and the B slurry is injected 10 seconds after the A slurry is injected, so as to realize dual-liquid synchronous grouting; When the shield machine stops advancing, the injection of the B slurry is stopped 1 minute in advance, and the injection of the A slurry is stopped 10 seconds after the injection of the B slurry is stopped; The A slurry in the slurry pipe is flushed with flowing clean water.