Sulfonium salt monomolecular resin type photoresist containing diphenylethylene structure and preparation method and application thereof
By introducing styrene structure sulfonium salt single-molecular resin into the photoresist, the shortcomings of photoresist in high resolution and low edge roughness are solved, and efficient photolithography is achieved, suitable for deep ultraviolet and UV lithography.
Patent Information
- Application Number
- CN202411203539.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Existing photoresist materials have shortcomings in high resolution and low edge roughness, especially in the linear edge roughness and instability problems caused by chemically amplified photoresist due to acid diffusion, and the molecules of traditional molecular weight polymer resins Large volume and molecular weight dispersion affect pattern resolution.
Develop a sulfonium salt single-molecular resin containing styrene structure as the main material of non-chemical amplified photoresist. By introducing a conjugated structure, the film is prepared by spin coating to achieve high Resolution and low line edge roughness.
The photolithographic patterns with high resolution and low linear edge roughness are achieved, which avoids the acid diffusion problem in chemical amplification glue, and is suitable for deep ultraviolet and ultraviolet lithography applications due to the certainty of molecular structure and high thermal stability.
Smart Images

Figure CN118702604B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to a sulfonium salt monomolecular resin type photoresist containing a stilbene structure, and a preparation method and application thereof. Background Art
[0002] As the foundation of the development of the modern semiconductor industry, the progress of lithography technology has promoted the development of information technology. Lithography technology has developed from the initial G-line (436 nm) and I-line (365 nm) lithography to deep ultraviolet lithography (KrF (248 nm) and ArF (193 nm), to the most advanced extreme ultraviolet lithography (EUV, 13.5 nm), electron beam, ion beam lithography, etc., and photoresist materials used in lithography technology are also developing accordingly. Photoresist is also called photoresist. After being irradiated or radiated by light sources such as ultraviolet light, excimer laser, electron beam, ion beam and X-ray, the exposed area and non-exposed area of the photoresist produce significant changes in solubility, adhesion, etc. After development, the soluble part is removed to obtain a pattern. There are two types of photoresists: positive and negative. The photoresist in the exposed area is dissolved and removed during the development process, and the photoresist in the non-exposed area is retained on the substrate. The pattern formed is consistent with the mask. This type of photoresist is called positive photoresist, and vice versa. It is called negative photoresist. With the rapid development of the semiconductor industry, the resolution required by lithography technology is getting higher and higher, and the edge roughness requirements are getting smaller and smaller, which puts higher requirements on the comprehensive performance that photoresist materials can achieve.
[0003] At present, conventional high-resolution photoresists all use chemically amplified resists (CARs). The so-called "chemical amplification" means that PAG decomposes to produce acid after exposure. The acid triggers a series of chemical reactions, which significantly changes the solubility of the photoresist material in the exposed area and the non-exposed area. Then, pattern transfer can be achieved through development. However, there are a series of problems with chemically amplified photoresist systems, such as high line edge roughness (LER) and line width roughness (LWR) caused by acid diffusion, instability after exposure, etc. In order to solve these problems, the research on new non-chemically amplified photoresists (n-CARs) is receiving more and more attention. In n-CARs, the photosensitive group is connected to the main chain of the photoresist. When irradiated, the photosensitive group directly undergoes a photochemical reaction to cause chain scission or polarity change of the group, thereby achieving solubility change in the developer, so there is no acid diffusion problem in chemically amplified photoresists. In addition, non-chemically amplified photoresists are generally single-component photoresists, without other additives such as acid generators and acid diffusion inhibitors, and there is no problem of uneven dispersion between components, which further provides advantages for achieving low LER. Traditional photoresist main materials generally use molecular weight polymer resins. Such polymer resins usually affect the resolution and edge roughness of the lithographic pattern due to large molecular volume, molecular weight dispersion, and molecular chain entanglement, and cannot meet the requirements of finer resolution. Therefore, it is of great significance to develop single-molecule resin non-chemically amplified photoresists with strong lithography potential.
[0004] At present, there are related patent reports on sulfonium salt-based single-molecule resin non-chemically amplified photoresists, but ordinary sulfonium salt photoresists have poor sensitivity and short absorption wavelength. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a sulfonium salt monomolecular resin containing a stilbene structure, which can be used as a main material of a non-chemically amplified photoresist.
[0006] The technical solution of the present invention is as follows:
[0007] The compound shown in the following formula I:
[0008]
[0009] Among them, R a are the same or different and are independently selected from hydrogen, C 1-15 Alkyl, C 1-15 Alkoxy, halogenated C 1-15 Alkyl, halogenated C 1-15 Alkoxy;
[0010] R b The same or different, each independently selected from -S + R S1 RS2 or a group Z, wherein the group Z is H, C 1-15 Alkyl, C 1-15 Alkoxy, halogenated C 1-15 Alkyl, halogenated C 1-15 Alkoxy;
[0011] R S1 , R S2 The same or different, each independently selected from unsubstituted, or optionally substituted by one, two or more R S Substituted with the following groups: C 1-15 Alkyl, C 6-20 Aryl, -C 1-15 Alkyl-C 6-20 Aryl, -C 6-20 Aryl-C 1-15 alkyl;
[0012] R S are the same or different and are independently selected from oxo (=O), nitro, cyano, C 1-15 Alkyl, C 1-15 Alkoxy;
[0013] X – is an anion, for example, a halide, carboxylate, sulfate, alkylsulfonate, haloalkylsulfonate (e.g., trifluoromethanesulfonate, perfluoropropylsulfonate, perfluorobutylsulfonate), p-toluenesulfonate, an anion of sulfonamide, tetrafluoroborate, hexafluoroantimonate, hexafluorophosphate or bistrifluoromethanesulfonyl imide ion;
[0014] m is equal to the sulfonium salt group -S in the molecule + R S1 R S2 Medium S + The number of + and X – The compound is electrically neutral as a whole, and m is an integer of 1-3; that is, the compound of formula I has 1-3 groups -S + R S1 R S2 .
[0015] In some embodiments of the present invention, R a The same or different, each independently selected from H, C 1-8 Alkyl or C 1-8 Alkoxy;
[0016] R b The same or different, each independently selected from H or -S + R S1 R S2 ; R S1 , R S2The same or different, each independently selected from C 1-8 Alkyl, or one, two or more R S Substituted with the following groups: C 6-14 Aryl, C 1-6 Alkyl-C 6-14 Aryl; R S are the same or different, each independently selected from nitro, cyano, C 1-8 alkyl;
[0017] X – is a halogen ion, a carboxylate, a sulfate, an alkylsulfonate, a trifluoromethanesulfonate, a perfluoropropylsulfonate, a perfluorobutylsulfonate, a p-toluenesulfonate, an anion of a sulfonamide, a tetrafluoroborate, a hexafluoroantimonate, a hexafluorophosphate or a bistrifluoromethanesulfonyl imide ion;
[0018] m is an integer of 1-3.
[0019] In some embodiments of the present invention, the compound of formula I has 1-3 groups -S + R S1 R S2 , for example, having 1, 2, or 3 sulfonium salt groups -S + R S1 R S2 .
[0020] In some embodiments of the present invention, the compound of formula I has three sulfonium salt groups -S + R S1 R S2 , and each terminal phenyl group connected to the vinyl group has a sulfonium salt group -S + R S1 R S2 .
[0021] In some embodiments of the invention, the sulfonium salt group -S + R S1 R S2 Located at the ortho, meta or para position on the terminal phenyl group connected to the vinyl group.
[0022] In some embodiments of the present invention, R a The same or different, each independently selected from H, C 1-6 Alkyl or C 1-6 Alkoxy.
[0023] In some embodiments of the present invention, the four R a 1 of them is selected from C 1-6 Alkyl or C 1-6 alkoxy, and the other three are H.
[0024] In some embodiments of the present invention, R b The same or different, each independently selected from H or -S + R S1 R S2 ; R S1 , R S2 The same or different, each independently selected from C 1-6 Alkyl or one, two or more R S Substituted with the following groups: C 6-14 Aryl, -C 1-6 Alkyl-C 6-14 Aryl; R S are the same or different, each independently selected from nitro, cyano, C 1-6 alkyl.
[0025] In some preferred embodiments of the present invention, the R a are the same or different and are each independently selected from H, methyl, methoxy, ethyl, ethoxy, n-propyl, n-butyl or tert-butyl.
[0026] In some preferred embodiments of the present invention, R b The same or different, each independently selected from H, -S + (C 1-6 Alkyl)2, -S + (C 6-14 Aryl)2, -S + (C 6-14 Aryl) (C 1-6 Alkyl), -S + (-C 1-6 Alkyl C 6-14 Aryl) (C 1-6 Alkyl); wherein the C 6-14 The aryl group is optionally substituted by one or two of the following groups: nitro, cyano, C 1-6 alkyl.
[0027] In some preferred embodiments of the present invention, R b The same or different, each independently selected from H, -S + (C 1-3 Alkyl)2, -S + (C 6-14 Aryl)2, -S + (C 6-14 Aryl) (C 1-3 Alkyl), -S + (-C 1-3 Alkyl C 6-14 Aryl) (C 1-3 Alkyl); wherein the C 6-14The aryl group is optionally substituted by one or two of the following groups: nitro, cyano, C 1-3 alkyl.
[0028] In some preferred embodiments of the present invention, R b The same or different, each independently selected from H or the following groups:
[0029]
[0030] in, Indicates a connection key.
[0031] In some embodiments of the present invention, X - Selected from halide ion, alkyl sulfonate, halogenated alkyl sulfonate (such as trifluoromethanesulfonate, perfluoropropylsulfonate, perfluorobutylsulfonate), p-toluenesulfonate, tetrafluoroborate, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide ion.
[0032] As an example, the compound represented by formula I has the following structure:
[0033]
[0034]
[0035]
[0036] .
[0037] Optionally, the compound represented by formula I can also be subjected to ion exchange with a corresponding anion solution to obtain a compound represented by formula I with a different anion.
[0038] The present invention also provides a method for preparing the compound shown in the above formula I, comprising the following steps:
[0039] The compound represented by formula II and R S2 -L and MX react to obtain a compound of formula I;
[0040]
[0041] Wherein, L is a leaving group, such as a halogen, etc.; MX is a metal salt containing X; R b ' is a group Z or -SR S1 ; R a , R b , R S2 , X and m are as defined above;
[0042] Alternatively, the compound represented by formula II' and and trifluoromethanesulfonic anhydride to obtain a compound of formula I;
[0043]
[0044] Among them, R a Having the definition as above.
[0045] Optionally, the compound represented by formula I can also be subjected to ion exchange with a corresponding anion solution to obtain a compound represented by formula I with a different anion.
[0046] According to an embodiment of the present invention, the compound shown in formula II is prepared by the following method:
[0047] (1) The compound represented by formula V reacts with the compound represented by formula IV under the catalysis of palladium acetate to obtain a compound having a diphenylethylene structure represented by formula III:
[0048]
[0049] (2) The compound represented by formula III is reacted with 1,3,5-benzenetricarboxylic acid chloride under the catalysis of triethylamine and 4-dimethylaminopyridine (DMAP) to obtain the compound represented by formula II:
[0050]
[0051] Among them, R a With the above definition, R b ' is a group Z or -SR S1 , groups Z and R S1 Having the definition as above.
[0052] In some embodiments of the present invention, the compound wherein X is triflate is ion exchanged with other anions to obtain a compound of formula I with a different anion.
[0053] The present invention also provides use of the compound represented by the above formula I in preparing photoresist.
[0054] According to an embodiment of the present invention, the photoresist is a single-component photoresist, which contains only the compound shown in Formula I except for the solvent.
[0055] The present invention also provides a photoresist composition, which includes the compound shown in formula I.
[0056] According to an embodiment of the present invention, the photoresist composition further comprises a photoresist solvent. The photoresist solvent is, for example, selected from one, two or more of the following substances: propylene glycol methyl ether acetate (PGMEA), propylene glycol methyl ether (PGME), N,N-dimethylformamide, dimethylformamide (DMF), cyclohexanone, ethyl n-amyl ketone, ethyl isoamyl ketone, ethanol, acetonitrile, isopropanol, acetone, methyl n-amyl ketone, methyl isoamyl ketone.
[0057] According to an embodiment of the present invention, the photoresist composition is a positive or negative photoresist composition.
[0058] In some embodiments of the present invention, the photoresist composition is a single-component photoresist, which is composed of the compound represented by formula I and a photoresist solvent. That is, the photoresist composition includes only one component, namely, the compound represented by formula I, in addition to the photoresist solvent.
[0059] The present invention also provides a photoresist coating, which comprises the compound represented by formula I as described above.
[0060] The present invention also provides a method for preparing the above-mentioned photoresist coating, comprising: applying the above-mentioned photoresist composition on a substrate to prepare the coating.
[0061] In one embodiment, the applying method is spin coating.
[0062] In one embodiment, the substrate is a silicon wafer substrate.
[0063] Preferably, the photoresist coating is a thin film.
[0064] The present invention also provides the use of the compound represented by formula I, the photoresist composition or the photoresist coating in lithography, for example, in 365nm lithography, 248nm lithography, 193nm lithography, extreme ultraviolet (EUV) lithography, nanoimprint lithography or electron beam lithography, preferably in ultraviolet, extreme ultraviolet and electron beam lithography.
[0065] The compound of the present invention has good thermal stability (decomposition temperature is greater than 300° C.) due to its unique stilbene conjugated structure and sulfonium salt structure, and can be used for photolithography processing.
[0066] The beneficial effects of the present invention are as follows:
[0067] (1) The present invention provides a series of novel sulfonium salt-type molecular glasses (monomolecule resins) with a diphenylethylene structure, namely, compounds shown in Formula I, which can be used as the main material of photoresists. The raw materials are cheap and easy to obtain, and the synthesis process is simple; the present invention introduces diphenylethylene into the molecular structure to increase the conjugation effect of the compounds shown in Formula I, thereby improving the sensitivity and etching resistance of the photoresist. In addition, the structure with diphenylethylene as the core has a wide absorption wavelength range, and the absorption cutoff wavelength can reach more than 400nm, so that it can be used not only for deep ultraviolet lithography, but also for ultraviolet (365 nm) lithography.
[0068] (2) This type of single-molecule resin has good solubility in various polar solvents and can be used to prepare good thin films by spin coating, which is suitable for the requirements of photolithography processing technology. The compound shown in Formula I can be used as a single-component non-chemically amplified photoresist, avoiding the problems of uneven distribution of acid generators and acid diffusion inhibitors and uneven acid diffusion in chemically amplified photoresists. The resulting pattern has high resolution and low line edge roughness.
[0069] (3) The compound of the present invention uses a benzene ring as a basic unit and introduces a diphenylethylene structure with relatively high rigidity to maximize the etching resistance of the main material, while also improving its thermal stability, solubility and film-forming properties. The overall performance is greatly improved. The thermal decomposition temperature of the main material is greater than 300°C, which expands the application range of the material and is suitable for the requirements of photolithography processing technology.
[0070] (4) The sulfonium salt monomolecular resin based on the diphenylethylene structure described in the present invention has a definite molecular structure and a single molecular size, which can well meet the requirements of high-resolution lithography.
[0071] (5) The compound of the present invention has a long absorption wavelength due to the introduction of a stilbene structure, so that the single-molecule resin can be used not only for deep ultraviolet lithography but also for ultraviolet lithography (365 nm).
[0072] (6) The compound of the present invention introduces a diphenylethylene structure with strong conjugation, so that the non-chemically amplified photoresist with the compound as the main material has higher sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] Figure 1 This is an AFM image of the thin film of compound I-1 in Example 1 of the present invention.
[0074] Figure 2 This is an AFM image of the compound I-2 film in Example 2 of the present invention.
[0075] Figure 3 This is an AFM image of the compound I-6 film in Example 4 of the present invention.
[0076] Figure 4 The differential scanning calorimetry curve and the thermogravimetric curve of compound I-2 in Example 2 of the present invention are shown.
[0077] Figure 5 The differential scanning calorimetry curve and the thermogravimetric curve of compound I-6 in Example 4 of the present invention are shown.
[0078] Figure 6 This is the ultraviolet absorption curve of compound I-6 in Example 4 of the present invention.
[0079] Figure 7 This is a scanning electron microscope (SEM) image of the negative resist film-forming photolithography stripes (365 nm photolithography, exposure period of 2 μm) of the main material of Compound I-1 in Example 1 of the present invention.
[0080] Figure 8 This is a scanning electron microscope (SEM) image of the negative resist film-forming lithography stripes (electron beam lithography, exposure period of 80 nm) of the main material of Compound I-1 in Example 1 of the present invention.
[0081] Fig. 9 This is a scanning electron microscope (SEM) image of the negative resist film-forming lithography stripes (electron beam lithography, exposure period of 60 nm) of the main material of Compound I-1 in Example 1 of the present invention.
[0082] Fig.10 This is a scanning electron microscope (SEM) image of the negative resist film-forming lithography stripes (electron beam lithography, exposure period of 70 nm) of the main material of compound I-2 in Example 2 of the present invention.
[0083] Fig.11 This is a scanning electron microscope (SEM) image of the negative resist film-forming lithography stripes (electron beam lithography, exposure period of 60 nm) of the main material of compound I-6 in Example 4 of the present invention.
[0084] Fig.12 This is a scanning electron microscope (SEM) image of the negative resist film-forming lithography stripes (electron beam lithography, exposure period of 40 nm) of the main material of compound I-6 in Example 4 of the present invention.
[0085] Definition and explanation of terms
[0086] Unless otherwise defined, all technical and scientific terms herein have the same meaning as commonly understood by one of ordinary skill in the art to which the claimed subject matter belongs.
[0087] "More" means three or more.
[0088] The term "C 1-15 "Alkyl" is understood to mean a straight-chain or branched saturated monovalent hydrocarbon group having 1 to 15 carbon atoms. Preferably "C 1-8 Alkyl" or "C 1-6 Alkyl". The "C 1-6The term "alkyl" refers to straight-chain and branched alkyl groups having 1, 2, 3, 4, 5, or 6 carbon atoms. The alkyl group is, for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2-methylbutyl, 1-methylbutyl, 1-ethylpropyl, 1,2-dimethylpropyl, neopentyl, 1,1-dimethylpropyl, 4-methylpentyl, 3-methylpentyl, 2-methylpentyl, 1-methylpentyl, 2-ethylbutyl, 1-ethylbutyl, 3,3-dimethylbutyl, 2,2-dimethylbutyl, 1,1-dimethylbutyl, 2,3-dimethylbutyl, 1,3-dimethylbutyl, 1,2-dimethylbutyl, or the like or isomers thereof.
[0089] The term "C 1-15 "Alkoxy" is understood to mean -OC 1-15 Alkyl, where C 1-15 Alkyl has the above definition.
[0090] The term "C 6-20 "Aryl" is understood to mean a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring having 6 to 20 carbon atoms, preferably "C 6-14 The term "C 6-14 "Aryl" is understood to mean preferably a monovalent aromatic or partially aromatic monocyclic, bicyclic or tricyclic hydrocarbon ring ("C 6-14 or a ring having 9 carbon atoms ("C9 aryl"), for example indanyl or indenyl, or a ring having 10 carbon atoms ("C 10 aryl"), such as tetrahydronaphthyl, dihydronaphthyl or naphthyl, or a ring having 13 carbon atoms ("C 13 aryl"), such as fluorenyl, or a ring having 14 carbon atoms ("C 14 aryl"), such as anthracenyl. When the C 6-20 When the aryl group is substituted, it may be monosubstituted or polysubstituted. Also, there is no limitation on the substitution position, for example, it may be substituted at the ortho position, para position or meta position.
[0091] The above term “C 1-15 The definition of "alkyl" also applies to other C-containing 1-15 Alkyl groups, such as -C 1-15 Alkyl-C 6-20 Aryl, -halogenated C 1-15 Alkyl, -halogenated C 1-15 Alkoxy, etc. DETAILED DESCRIPTION
[0092] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0093] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0094] Example 1
[0095] Preparation of compound III-1, the synthetic route is as follows:
[0096]
[0097] Specific steps: 4-vinylphenol (58.4g, 1.0eq), (4-bromophenyl)(methyl)sulfane (98.8g, 1.0eq), palladium acetate catalyst (1.6g, 0.04eq), triethanolamine (72.6g, 1.0eq) were added to a 500ml two-necked bottle, nitrogen was pumped out three times to deoxygenate, and then placed in a 110℃ oil bath pot for reaction for 11h. DCM:EA =5:1 as the developing solvent for column chromatography, 400 ml of petroleum ether was used to precipitate a viscous solid, which was then recrystallized with 800 ml of ethanol to obtain a white solid with a yield of 15%. 1 HNMR (400 MHz, deuterated chloroform) 7.38 (m, 4H), 7.36 (d,2H), 6.90 (s, 2H), 6.75 (d,2H), 2.38 (s, 3H); MS(ESI) : m / z = 242.08, calcd. 15 H 14 OS + m / z =242.08 ([M] + ).
[0098] Preparation of compound II-1, the synthetic route is as follows:
[0099]
[0100] Specific steps: Add compound III-1 (4.00g, 4.0eq), DMAP (0.1512g, 0.3eq), triethylamine (2.99g, 4.0eq) to a 250ml round-bottom flask, add 90ml dry THF to dissolve the solid, dissolve 1,3,5-benzenetricarboxylic acid chloride (1.09g, 1.0eq) in 30ml THF, slowly drop into the reaction bottle, stir and react at room temperature. Stop the reaction after 7h, filter the reaction solution to obtain 3.47g of light yellow solid, with a yield of 96%. 1 H NMR (400 MHz, dimethyl sulfoxide-d6) δ 8.90 (s, 3H), 7.81(d, 6H), 7.41 – 7.36 (m, 18H), 6.90(s, 6H), 2.38 (s,9H); MS(ESI): m / z =882.21, calcd. 54 H 42 O6S3 + m / z =882.21 ([M] + ).
[0101] The synthesis route of compound Ⅰ-1 is as follows:
[0102]
[0103] Specific steps: Add compound II-1 (2.78g, 1.0eq), silver trifluoromethanesulfonate (4.85g, 6.0eq) and 45ml of dry dichloromethane to a 50ml single-mouth reaction bottle. Dissolve iodomethane (2.68g, 6.0eq) in 5ml of dichloromethane and slowly add dropwise. After the addition is complete, react at room temperature for 3h in the dark. Let the reaction solution stand and pour off the supernatant, and dissolve the solid in acetonitrile. Filter and remove the AgI precipitate in the reaction mixture to obtain a colorless solution. Remove the solvent by vacuum distillation to obtain a white foamy solid. Use methanol as the recrystallization solvent to obtain a white powdery solid with a yield of 66%. 1 H NMR (600 MHz, acetonitrile-d3)δ) δ 9.15 (s, 3H), 7.90 (s, 12H), 7.76 (d, J = 8.7 Hz, 6H), 7.49 (d,J = 16.4 Hz, 3H), 7.40 (d, J = 8.6 Hz, 6H), 7.32 (d, J = 16.4 Hz, 3H), 3.15(s, 18H).; MS(ESI): m / z =309.09, calcd. 57 H 51 O6S3 3+m / z =309.09 ([M] 3+ ); m / z =148.95, calculated for CF3SO3 - m / z=148.95 ([M] - ).
[0104] Example 2
[0105] Preparation of compound III-2, the synthetic route is as follows:
[0106]
[0107] The specific steps are the same as the first step of the preparation process in Example 1, except that 4-vinylphenol is replaced by 2-methoxy-4-vinylphenol, and the reaction yield is 38%. 1 H NMR (400 MHz, deuterated chloroform) δ 7.38 (d, 2H), 7.36 (d, 2H), 7.25-7.04 (m, 3H), 6.95 (s, 1H), 6.90 (s, 1H), 3.83 (s, 3H), 2.38 (s, 3H); MS (ESI) : m / z = 272.36, calcd. 16 H 16 O2S + m / z =272.36 ([M] + )
[0108] Preparation of compound II-2, the synthetic route is as follows:
[0109]
[0110] The specific steps are the same as the second step of the preparation process in Example 1, except that compound III-1 is replaced by compound III-2, and the reaction yield is 97%. 1 H NMR (600 MHz, dimethyl sulfoxide-d6) δ 9.02 (s, 3H), 7.57 (d, J =8.3 Hz, 6H), 7.47 (s, 3H), 7.39 – 7.18 (m, 18H), 3.87 (s, 9H), 2.38(s, 9H); MS (ESI): m / z = 972.25, calculated value C 57 H 48 O9S3 + m / z =972.25 ([M] + ).
[0111] Preparation of compound Ⅰ-2, the synthetic route is as follows:
[0112]
[0113] The specific steps are the same as the third step of the preparation process in Example 1, except that compound II-1 is replaced by compound II-2, and the reaction yield is 52%. 1 H NMR (400 MHz, acetonitrile-d3) δ 9.12 (s, 3H), 7.90 (s, 12H), 7.51 –7.42 (m, 6H), 7.38 – 7.27 (m, 9H), 3.91 (s, 9H), 3.14 (s, 18H).; MS (ESI): m / z=339.10, calcd. 60 H 57 O9S3 3+ m / z =339.10 ([M] 3+ ); m / z =148.95, calculated for CF3SO3 - m / z=148.95 ([M] - ).
[0114] Example 3
[0115] Preparation of compound III-3, the synthetic route is as follows:
[0116]
[0117] The specific steps are the same as the first step of the preparation process in Example 1, except that (4-bromophenyl)(methyl)sulfane is replaced by (3-bromophenyl)(methyl)sulfane, and the reaction yield is 30%. 1 H NMR (400 MHz, deuterated chloroform) δ 7.48 (m, 1H), 7.38 (d, 2H), 7.27-7.25 (m, 2H), 7.01(s, 1H), 6.95 (s, 1H), 6.90 (s, 1H), 6.75 (d, 2H), 2.53 (s, 3H); MS(ESI) : m / z = 242.08, calcd. 15 H 14 OS + m / z =242.08 ([M] + ).
[0118] Preparation of compound II-3, the synthetic route is as follows:
[0119]
[0120] The specific steps are the same as the second step of the preparation process in Example 1, except that compound III-1 is replaced by compound III-3, and the reaction yield is 97%. 1 H NMR (400 MHz, dimethyl sulfoxide-d6) δ 8.90 (s, 3H), 7.91(m, 3H),7.48 (d, 6H), 7.30 – 7.05 (m, 9H), 6.95 (s, 3H), 6.90(s, 3H), 2.38 (s, 9H); MS (ESI): m / z =882.21, calculated value C 54 H 42 O6S3 + m / z =882.21 ([M] + ).
[0121]
[0122] The specific steps are the same as the third step of the preparation process in Example 1, except that compound II-1 is replaced by compound II-3, and the reaction yield is 52%. 1 H NMR (600 MHz, acetonitrile-d3) δ 9.15 (s, 3H), 7.99 (m,3H), 7.82 (d,6H), 7.59 (d, 6H),7.49 (s, 6H), 7.45 (s, 3H), 7.40 (s, 3H), 3.15 (s, 18H).; MS (ESI): m / z =309.09, calculated value C 57 H 51 O6S3 3+ m / z =309.09 ([M] 3+ ); m / z =148.95, calculated for CF3SO 3- m / z=148.95 ([M] - ).
[0123] Example 4
[0124] Compound I-6 was prepared by the following synthetic route:
[0125]
[0126] The specific steps are the same as the third step of the preparation process in Example 2, except that iodomethane is replaced by 4-bromoethylbenzonitrile, and the reaction solvent is replaced by acetonitrile from dichloromethane, and the reaction yield is 50%. 1H NMR (600 MHz, acetonitrile-d3) δ9.13 (s, 3H), 7.81 (s, 6H), 7.72 (s, 12H), 7.51 – 7.42 (m, 6H), 7.32 (s,15H), 4.93 (s, 3H), 4.75 (s, 3H), 3.91 (s, 9H), 3.21 (s, 9H); MS(ESI) : m / z =440.13, calcd. 81 H 66 N3O9S3 3+ m / z =440.13 ([M] 3+ ); m / z =148.95, calculated for CF3SO 3- m / z=148.95 ([M] - ).
[0127] Example 5
[0128] Preparation of compound III-8, the synthetic route is as follows:
[0129]
[0130] The specific steps are the same as the first step of the preparation process in Example 2, except that (4-bromophenyl)(methyl)sulfane is replaced by bromobenzene, and the reaction yield is 40%. 1 H NMR (400 MHz, deuterated chloroform) δ 7.72 (d, 2H), 7.44 (m, 2H),7.30 (d,1H), 7.25-7.04 (m, 3H), 6.95 (s, 1H), 6.90 (s, 1H), 3.83 (s, 3H); MS(ESI) : m / z = 226.10, calcd. 1s H 14 O2 + m / z =226.10 ([M] + ).
[0131] Preparation of compound II-8, the synthetic route is as follows:
[0132]
[0133] The specific steps are the same as the second step of the preparation process in Example 1, except that compound III-1 is replaced by compound III-8, and the reaction yield is 95%. 1H NMR (600 MHz, dimethyl sulfoxide-d6) δ 8.82 (s, 3H), 7.57 (d, J =8.3 Hz, 6H), 7.42-7.49 (m, 12H), 7.30 (d,3H), 7.23 (d, 3H), 3.87 (s, 9H); MS(ESI) : m / z = 834.28, calcd. 54 H 42 O9 + m / z =834.28 ([M] + ).
[0134] Preparation of compound I-8, the synthetic route is as follows:
[0135]
[0136] Specific steps: Add compound II-8 (5.78g 1eq) and diphenyl sulfoxide (5.69g, 4.5eq) to a 250ml round-bottom flask, dissolve it in 20ml dry dichloromethane and place it in an acetonitrile bath (-42℃), drop 20ml of trifluoromethanesulfonic anhydride dichloromethane solution (15.76g, 8eq), and react in an acetonitrile bath in the dark for 5h after the dropwise addition. After removing most of the reaction solution through a rotary evaporator, drop it into ether to obtain a white precipitate with a yield of 72%. 1 H NMR (400 MHz, acetonitrile-d3) δ8.82 (s, 3H), 7.49 – 7.42 (m, 12H), 7.23 (d, 3H), 6.95 (s, 3H), 6.90(s, 3H),3.91 (s, 9H); MS(ESI) : m / z =463.14, calcd. 90 H 69 O9S3 3+ m / z =463.14 ([M] 3+ ); m / z=148.95, calculated for CF3SO3 - m / z=148.95 ([M] - ).
[0137] Example 6
[0138] Compounds I-1, I-2, and I-6 were dissolved in acetonitrile to prepare solutions with a concentration of 15 mg / ml. Then, the solutions were filtered with a microporous filter with a pore size of 0.22 μm to obtain spin coating solutions. The spin coating solutions were spin coated on a silicon substrate to form a film, and the uniformity and flatness of the film were analyzed using an atomic force microscope (AFM). The results are shown in the attached Figure 1 , Attachment Figure 2 And attached Figure 3 It can be seen from the figure that the obtained film is very uniform and has no crystallization phenomenon, which is conducive to the preparation of a smooth surface lithography pattern.
[0139] Example 7
[0140] The thermal stability of compounds I-2 and I-6 prepared in Example 2 and Example 4 was measured. The differential scanning calorimetry curve and thermogravimetric analysis of compound I-2 were shown in FIG. Figure 4 The differential scanning calorimetry and thermogravimetric analysis of compound I-6 are shown in Figure 5 The results show that the melting points of the two compounds are above 150°C, and the thermal decomposition temperatures are both above 300°C, which means they have good thermal stability.
[0141] Example 8
[0142] Determine the UV-visible absorption spectrum of compound I-6 in Example 4 (the solvent is acetonitrile, the test results are shown in Figure 6 . Figure 6 This indicates that the molecular structure has a long absorption wavelength and still has absorption at 365 nm.
[0143] Example 9
[0144] A negative photoresist formulation and photolithography: Compound I-1 of Example 1 was dissolved in acetonitrile to obtain a solution with a mass concentration of 15 mg / ml, filtered with a microporous filter with a pore size of 0.22 μm to obtain a spin coating solution, and a film was formed by spin coating on an untreated silicon substrate, pre-baked at 80°C for 3 minutes, and the film thickness was measured using an ellipsometer. The prepared film was exposed using a 365nm exposure machine, and a very clear 1.07 μm stripe pattern was obtained. The test results are shown in FIG. Figure 7 The prepared film was exposed using the electron beam light source of the National Nanotechnology Center. The exposure cycles were 80nm and 60nm, and very uniform lithography stripes were obtained. The test results are shown in Figure 8 and Fig. 9 The results show that the obtained patterns have good resolution, contrast and low line edge roughness.
[0145] According to the same method as above, a negative photoresist containing compound I-2 was obtained and spin-coated to form a film. The prepared film was exposed using an electron beam light source from the National Nanotechnology Center. The exposure period was 70 nm, and very uniform photolithography stripes were obtained. The test results are shown in Fig.10 The results show that the obtained patterns have good resolution, contrast and low line edge roughness.
[0146] According to the same method as above, a negative photoresist containing compound I-6 was obtained and spin-coated to form a film. The prepared film was exposed using an electron beam light source from the National Nanotechnology Center. The exposure period was 60nm and 40nm, and very uniform photolithography stripes were obtained. The test results are shown in Fig.11 and Fig.12 The results show that the obtained patterns have good resolution, contrast and low line edge roughness.
[0147] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. Compounds of formula I: Ⅰ; in, R a are the same or different and are independently selected from hydrogen, C 1-15 Alkyl, C 1-15 Alkoxy, halogenated C 1-15 Alkyl, halogenated C 1-15 Alkoxy; R b The same or different, each independently selected from -S + R S1 R S2 or a group Z, wherein the group Z is H, C 1-15 Alkyl, C 1-15 Alkoxy, halogenated C 1-15 Alkyl, halogenated C 1-15 Alkoxy; R S1 , R S2 The same or different, each independently selected from unsubstituted, or optionally substituted by one, two or more R S Substituted with the following groups: C 1-15 Alkyl, C 6-20 Aryl, -C 1-15 Alkyl-C 6-20 Aryl, -C 6-20 Aryl-C 1-15 alkyl; R S are the same or different and are independently selected from oxo, nitro, cyano, C 1-15 Alkyl, C 1-15 Alkoxy; X – is a halide ion, a carboxylate, a sulfate, an alkylsulfonate, a trifluoromethanesulfonate, a perfluoropropylsulfonate, a perfluorobutylsulfonate, a p-toluenesulfonate, an anion of a sulfonamide, a tetrafluoroborate, a hexafluoroantimonate, a hexafluorophosphate or a bistrifluoromethanesulfonyl imide ion; m is 3; The compound of formula I has three sulfonium salt groups -S + R S1 R S2 , and each terminal phenyl group connected to the vinyl group has a sulfonium salt group -S + R S1 R S2 .
2. The compound of formula (I) according to claim 1, characterized in that: R a The same or different, each independently selected from H, C 1-8 Alkyl or C 1-8 Alkoxy; R b The same or different, each independently selected from H or -S + R S1 R S2 ; R S1 , R S2 The same or different, each independently selected from C 1-8 Alkyl or one, two or more R S Substituted with the following groups: C 6-14 Aryl, -C 1-6 Alkyl-C 6-14 Aryl; R S are the same or different, each independently selected from nitro, cyano, C 1-8 alkyl.
3. The compound of formula I according to claim 1 or 2, characterized in that: R a The same or different, each independently selected from H, C 1-6 Alkyl or C 1-6 Alkoxy; R b The same or different, each independently selected from H or -S + R S1 R S2 ; R S1 , R S2 The same or different, each independently selected from C 1-6 Alkyl or one, two or more R S Substituted with the following groups: C 6-14 Aryl, -C 1-6 Alkyl-C 6-14 Aryl; R S are the same or different, each independently selected from nitro, cyano, C 1-6 alkyl.
4. The compound of formula (I) according to claim 3, characterized in that: The R a are the same or different and are each independently selected from H, methyl, methoxy, ethyl, ethoxy, n-propyl, n-butyl or tert-butyl; R b The same or different, each independently selected from H, -S + (C 1-6 Alkyl)2, -S + (C 6-14 Aryl)2, -S + (C 6-14 Aryl) (C 1-6 Alkyl), -S + (-C 1-6 Alkyl C 6-14 Aryl) (C 1-6 alkyl); wherein, C 6-14 The aryl group is optionally substituted by one or two of the following groups: nitro, cyano, C 1-6 alkyl.
5. The compound of formula (I) according to claim 4, characterized in that: The compound represented by formula I has the following structure: ; ; ; 。 6. A method for preparing a compound of formula I according to any one of claims 1 to 5, characterized in that: The steps include: The compound represented by formula II and R S2 -L and MX react to obtain a compound of formula I; ; Among them, R a , R b , R S2 , X and m have the definitions as described in any one of claims 1 to 5; L is a leaving group; MX is a metal salt containing X; R b ' is a group Z or -SR S1 ; Alternatively, the compound represented by formula II' and and trifluoromethanesulfonic anhydride to obtain a compound of formula I; ; Among them, R a It has the definition as described in any one of claims 1 to 5.
7. Use of the compound of formula I described in any one of claims 1 to 5 for preparing a photoresist.
8. A photoresist composition comprising the compound represented by formula I according to any one of claims 1 to 5.
9. Use of the compound represented by formula I according to any one of claims 1 to 5 or the photoresist composition according to claim 8 in photolithography.
10. The use according to claim 9, characterized in that: The photolithography is 365nm photolithography, 248nm photolithography, 193nm photolithography, extreme ultraviolet photolithography, nanoimprint photolithography or electron beam photolithography.