Composite carboxyl styrene butadiene latex for coated paper and preparation method thereof
By alkali activation treatment of seporin powder and reacting with other raw materials to form a composite carboxylic styrene butadiene latex, the problem of insufficient bonding strength and water resistance of carboxylic styrene butadiene latex in the prior art is solved, and the bonding performance of coated paper is improved and stability.
Patent Information
- Application Number
- CN202411178559.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing carboxylic styrene butadiene latex in coated paper production cannot meet market demand.
By alkali activation treatment of sepiolite powder and with raw materials such as vinyl silane coupling agent, sodium dodecyl sulfate, tert-dodecane thiol, butadiene, styrene, acrylic acid and N-hydroxyethyl acrylamide, etc. The reaction is carried out to form a composite carboxylic styrene butadiene latex, which improves its bonding and water resistance.
The bonding strength, mechanical stability, chemical stability and wet surface strength of the composite carboxylic styrene butadiene latex are improved, and its application performance in coated paper is enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of latex preparation, and in particular to a composite carboxyl styrene butadiene latex for coating paper and a preparation method thereof. Background Art
[0002] Latex is a colloidal emulsion formed by polymer particles dispersed in water. It can be directly used for surface coating, making films and adhesives, etc., and is widely used in daily life. Latex can be divided into two categories: natural latex and synthetic latex. The characteristics of natural latex are strong cohesion, high self-adhesion, good film-forming property, and adjustable viscosity. However, due to the low polarity of its macromolecular chain, it has poor adhesion to the adherend, especially the adherend with high polarity. Its aging resistance, oil resistance, chemical resistance, temperature resistance, and frost resistance are relatively poor.
[0003] Styrene butadiene latex (SBL) usually uses water molecules as solvent, has no volatile hazardous chemicals, can achieve zero formaldehyde release during the process of combining with wood base, and has become a substitute for traditional resins with advantages such as low cost, high strength and easy modification. Carboxyl styrene butadiene latex (XSBL) is a new ionic supramolecular hybrid network latex constructed by adding acrylic acid (AA) to the SBL chain. After the introduction of carboxyl groups, its elastic range, strength, compatibility with polymers and functional fillers, hydrocarbon resistance, and solvent resistance are all enhanced to a certain extent. After plasticization, it has good mechanical properties, elasticity and wear resistance and has attracted attention from the industry.
[0004] As one of the most important raw materials for paper coating, the papermaking industry has higher and higher quality requirements for latex. In the production process of coated paper, the performance requirements of latex are very high. It must have good rheological properties to obtain suitable construction viscosity and improve the gloss of the coated paper surface, and it must have good bonding strength to improve the surface strength of the coated paper. At the same time, the latex is also required to have good process adaptability, especially high stability (including mechanical stability and chemical stability). Carboxylated styrene butadiene latex is currently the most widely used latex in coated paper production, but the current carboxylated styrene butadiene latex still has problems with bonding strength, stability and water resistance that cannot meet market demand.
[0005] Chinese patent document CN201810703723.6 discloses a preparation method and application of modified carboxylated styrene butadiene latex. On the basis of carboxylated styrene butadiene latex, two monomers, ethylene glycol and maleic anhydride, are grafted thereto, and hydroxyl groups, ester groups, maleic anhydride and other groups are directly or indirectly grafted onto the macromolecular main chain of styrene butadiene latex, and unsaturated alkyd polyester is generated by condensation of maleic anhydride and ethylene glycol. A variety of polar groups are introduced into the macromolecular chain of carboxylated styrene butadiene latex, which greatly improves the intermolecular force and can greatly improve the bonding strength with highly polar adherend materials, but its water resistance still needs to be further improved. Summary of the invention
[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide a composite carboxylated styrene-butadiene latex for coating paper and a preparation method thereof.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme:
[0008] In a first aspect, the present invention provides a method for preparing a composite carboxylated styrene-butadiene latex for coated paper, comprising the following steps:
[0009] S1, adding sepiolite powder to an alkaline solution, heating and stirring, and then filtering, washing, and drying to obtain pretreated sepiolite powder;
[0010] S2, ultrasonically dispersing the pretreated sepiolite powder in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, heating and stirring to react, and then filtering, washing, and drying to obtain a modified sepiolite powder;
[0011] S3, adding modified sepiolite powder, sodium dodecyl sulfate and tert-dodecyl mercaptan to deionized water, stirring evenly, introducing nitrogen to expel air, then adding butadiene, styrene, acrylic acid and N-hydroxyethyl acrylamide, stirring and heating to 55-60° C., adding an initiator to react, and after the reaction is completed, obtaining a dispersion;
[0012] S4. Cool the dispersion to room temperature and perform physical degassing to obtain composite carboxylated styrene-butadiene latex.
[0013] Specifically, in step S1, the temperature of heating and stirring is 40-60° C., and the time of heating and stirring is 1-5 h.
[0014] Specifically, in step S2, the mass ratio of the pretreated sepiolite powder to the vinyl silane coupling agent is 5-10:1-2.
[0015] Specifically, in step S2, the temperature of the heating and stirring reaction is 50-65° C., and the time of the heating and stirring reaction is 2-3 h.
[0016] Specifically, in step S3, the mass ratio of modified sepiolite powder, sodium dodecyl sulfate, tert-dodecyl mercaptan, deionized water, butadiene, styrene, acrylic acid, N-hydroxyethyl acrylamide and initiator is 4-8:1-3:2-3:100-120:15-20:20-25:5-10:5-10:1-1.5.
[0017] Specifically, in step S3, the initiator is selected from persulfate.
[0018] Specifically, in step S3, the reaction time is 2-5 hours.
[0019] Specifically, in step S4, the physical degassing conditions are: degassing at -0.08 MPa to -0.1 MPa for 1-2 h.
[0020] In a second aspect, the present invention provides a composite carboxylated styrene-butadiene latex prepared by the above preparation method.
[0021] In a third aspect, the present invention also provides the use of the above-mentioned composite carboxyl styrene butadiene latex in paper surface sizing.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) The present invention first performs an alkali activation treatment on the sepiolite powder to dissolve some impurities and silicate components in the sepiolite, thereby making the structure of the sepiolite more open, thereby increasing its specific surface area and porosity. At the same time, the alkali activation treatment can also increase the hydroxyl content on the surface of the sepiolite, making it easier to react with the silane coupling agent.
[0024] (2) The present invention uses a silane coupling agent containing double bonds to modify sepiolite, introduces carbon-carbon double bonds into the surface of sepiolite, and then an addition reaction occurs between the double-bonded sepiolite and other raw material components, thereby increasing the bonding strength between sepiolite and other raw materials, thereby improving the bonding performance of carboxylated styrene butadiene latex; at the same time, the applicant also found that the effect of adding sepiolite powder is better than that of bentonite, which may be due to the fact that sepiolite powder has better adsorption properties, which enables sepiolite powder to provide better adhesion and stability in composite carboxylated styrene butadiene latex; and the fibrous crystal structure of sepiolite enables it to have good rheological properties in composite carboxylated styrene butadiene latex, which can improve the fluidity and thixotropy of the latex, that is, it has a higher viscosity when static, and the viscosity decreases when subjected to shear force. Although bentonite also has certain thixotropic properties, the performance is not as significant as that of sepiolite.
[0025] (3) The present invention adds N-hydroxyethyl acrylamide to the raw materials. The double bonds in the N-hydroxyethyl acrylamide undergo polymerization reaction with other double bonds in the raw materials. By introducing N-hydroxyethyl groups into the composite carboxy styrene butadiene latex, the N-hydroxyethyl groups can undergo self-crosslinking reaction when the composite latex is cured, thereby improving the water resistance of the composite carboxy styrene butadiene latex. When coating various types of paperboards, the wet surface strength of the paper can be improved, and the invention has good market application prospects. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.
[0027] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.
[0028] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0029] S1. Preparation of pretreated sepiolite powder
[0030] The sepiolite powder is added into an alkaline solution, heated and stirred, and then filtered, washed and dried to obtain the pretreated sepiolite powder.
[0031] In this step, the usage ratio of sepiolite powder and alkaline solution is 10-15g:100mL, for example, 10g:100mL, 11g:100mL, 12g:100mL, 13g:100mL, 14g:100mL, 15g:100mL can be selected, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Specifically, the alkaline solution is selected from NaOH solution or KOH solution, and the concentration of the alkaline solution is 0.5-2 mol / L. In some embodiments of the present invention, for example, 0.5 mol / L, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2.0 mol / L can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] In this step, the heating and stirring temperature is 40-60°C, for example, 40°C, 42°C, 45°C, 48°C, 50°C, 52°C, 55°C, 58°C, and 60°C can be selected; the heating and stirring time is 1-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, and 5h can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] In this step, the sepiolite powder is firstly subjected to an alkali activation treatment, which dissolves some impurities and silicate components in the sepiolite to make the structure of the sepiolite more open, thereby increasing its specific surface area and porosity. At the same time, the alkali activation treatment can also increase the hydroxyl content on the surface of the sepiolite, making it easier to react with the silane coupling agent.
[0035] S2. Preparation of modified sepiolite powder
[0036] The pretreated sepiolite powder is ultrasonically dispersed in an ethanol aqueous solution, and then a vinyl silane coupling agent is added thereto, heated and stirred for reaction, and then filtered, washed and dried to obtain a modified sepiolite powder.
[0037] In this step, the mass ratio of the pretreated sepiolite powder and the vinyl silane coupling agent is 5-10:1-2. In some embodiments of the present invention, for example, 5:1, 5:1.5, 5:2, 6:1, 6:2, 8:1, 8:2, 10:1, 10:1.5, 10:2 can be selected, but it is not limited to the listed values. Other values not listed in the numerical range are also applicable.
[0038] Specifically, the vinyl silane coupling agent is selected from any one of vinyl trimethoxy silane, vinyl triethoxy silane, methyl vinyl diethoxy silane, and vinyl triisopropoxy silane.
[0039] Specifically, the mass fraction of the ethanol aqueous solution is 60-80%, for example, 60%, 65%, 70%, 75%, 80% can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] In this step, the temperature of the heating and stirring reaction is 50-65°C. In some embodiments of the present invention, for example, 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 64°C, and 65°C can be selected; the time of the heating and stirring reaction is 2-3h, for example, 2h, 2.5h, and 3h can be selected, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] S3. Preparation of dispersion
[0042] Add modified sepiolite powder, sodium dodecyl sulfate and tert-dodecyl mercaptan into deionized water, stir evenly, introduce nitrogen to expel air, then add butadiene, styrene, acrylic acid and N-hydroxyethyl acrylamide, stir and heat to 55-60°C, add initiator to react, and after the reaction is completed, obtain a dispersion.
[0043] In this step, the mass ratio of modified sepiolite powder, sodium dodecyl sulfate, tert-dodecyl mercaptan, deionized water, butadiene, styrene, acrylic acid, N-hydroxyethyl acrylamide and initiator is 4-8:1-3:2-3:100-120:15-20:20-25:5-10:5-10:1-1.5.
[0044] Specifically, the initiator is selected from persulfates, for example, ammonium persulfate, potassium persulfate, and sodium persulfate.
[0045] Specifically, the reaction time is 2-5h. In some embodiments of the present invention, for example, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, and 5h can be selected, but are not limited to the listed values. Other values not listed within the numerical range are also applicable.
[0046] S4. Preparation of composite carboxylated styrene-butadiene latex
[0047] The dispersion is cooled to room temperature and physically degassed to obtain a composite carboxylated styrene-butadiene latex.
[0048] In this step, the physical degassing conditions are: degassing at -0.08MPa to -0.1MPa for 1-2h.
[0049] The present invention is further described below by means of specific examples. The particle size of the sepiolite powder used in the examples of the present invention is 2000 mesh.
[0050] Example 1
[0051] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0052] S1. Add 10 g of sepiolite powder to 100 mL of 1 mol / L NaOH solution, heat and stir at 50° C. for 3 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0053] S2, ultrasonically dispersing 8 g of pretreated sepiolite powder in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltriethoxysilane thereto, heating and stirring at 50° C. for 3 h, then filtering, washing, and drying to obtain modified sepiolite powder;
[0054] S3, adding 5g of modified sepiolite powder, 2g of sodium dodecyl sulfate and 2g of tert-dodecyl mercaptan to 100g of deionized water, stirring evenly, introducing nitrogen to exhaust the air, and then adding 15g of butadiene, 20g of styrene, 5g of acrylic acid and 5g of N-hydroxyethyl acrylamide thereto, stirring and heating to 60°C, adding 1g of initiator ammonium persulfate to react, and after the reaction is completed, a dispersion is obtained;
[0055] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0056] Example 2
[0057] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0058] S1. Add 10 g of sepiolite powder to 100 mL of 1 mol / L NaOH solution, heat and stir at 50° C. for 3 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0059] S2, ultrasonically dispersing 5 g of pretreated sepiolite powder in 100 mL of 80 wt% ethanol aqueous solution, then adding 1 g of vinyltrimethoxysilane thereto, heating and stirring at 65° C. for 2 h, then filtering, washing, and drying to obtain modified sepiolite powder;
[0060] S3, adding 4g of modified sepiolite powder, 1g of sodium dodecyl sulfate and 3g of tert-dodecyl mercaptan to 100g of deionized water, stirring evenly, introducing nitrogen to exhaust the air, and then adding 20g of butadiene, 20g of styrene, 6g of acrylic acid and 8g of N-hydroxyethyl acrylamide thereto, stirring and heating to 60°C, adding 1.2g of initiator ammonium persulfate to react, and after the reaction is completed, a dispersion is obtained;
[0061] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0062] Example 3
[0063] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0064] S1. Add 10 g of sepiolite powder into 100 mL of 1 mol / L NaOH solution, heat and stir at 40° C. for 5 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0065] S2, ultrasonically dispersing 10 g of pretreated sepiolite powder in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltrimethoxysilane thereto, heating and stirring at 65 ° C for 2 h, then filtering, washing and drying to obtain modified sepiolite powder;
[0066] S3, adding 8g of modified sepiolite powder, 2g of sodium dodecyl sulfate and 3g of tert-dodecyl mercaptan to 120g of deionized water, stirring evenly, introducing nitrogen to exhaust the air, and then adding 20g of butadiene, 25g of styrene, 8g of acrylic acid and 6g of N-hydroxyethyl acrylamide, stirring and heating to 60°C, adding 1.5g of initiator ammonium persulfate to react, and after the reaction is completed, a dispersion is obtained;
[0067] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0068] Example 4
[0069] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0070] S1. Add 10 g of sepiolite powder into 100 mL of 1 mol / L NaOH solution, heat and stir at 60° C. for 1 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0071] S2, ultrasonically dispersing 6 g of pretreated sepiolite powder in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltriethoxysilane thereto, heating and stirring at 65 ° C. for 2 h, then filtering, washing, and drying to obtain modified sepiolite powder;
[0072] S3, 6g of modified sepiolite powder, 3g of sodium dodecyl sulfate and 2g of tert-dodecyl mercaptan were added to 120g of deionized water, stirred evenly, nitrogen was introduced to exhaust the air, and then 20g of butadiene, 20g of styrene, 10g of acrylic acid and 10g of N-hydroxyethyl acrylamide were added thereto, stirred and heated to 60°C, 1g of initiator ammonium persulfate was added to react, and after the reaction was completed, a dispersion was obtained;
[0073] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0074] Comparative Example 1
[0075] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0076] S1. Add 10 g of sepiolite powder to 100 mL of 1 mol / L NaOH solution, heat and stir at 50° C. for 3 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0077] S2, 5g of pretreated sepiolite powder, 2g of sodium dodecyl sulfate and 2g of tert-dodecyl mercaptan were added to 100g of deionized water, stirred evenly, nitrogen was introduced to exhaust the air, and then 15g of butadiene, 20g of styrene, 5g of acrylic acid and 5g of N-hydroxyethyl acrylamide were added thereto, the temperature was raised to 60°C with stirring, and 1g of initiator ammonium persulfate was added to react. After the reaction was completed, a dispersion was obtained;
[0078] S3. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0079] Compared with Example 1, Comparative Example 1 does not perform modification treatment on the pretreated sepiolite powder.
[0080] Comparative Example 2
[0081] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0082] S1. Add 10 g of bentonite (with a particle size of 2000 mesh) into 100 mL of 1 mol / L NaOH solution, heat and stir at 50° C. for 3 h, and then filter, wash and dry to obtain pretreated bentonite;
[0083] S2, ultrasonically dispersing 8 g of pretreated bentonite in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltriethoxysilane thereto, heating and stirring at 50° C. for 3 h, then filtering, washing, and drying to obtain modified bentonite;
[0084] S3, 5g of modified bentonite, 2g of sodium dodecyl sulfate and 2g of tert-dodecyl mercaptan were added to 100g of deionized water, stirred evenly, nitrogen was introduced to exhaust the air, and then 15g of butadiene, 20g of styrene, 5g of acrylic acid and 5g of N-hydroxyethyl acrylamide were added thereto, stirred and heated to 60°C, 1g of initiator ammonium persulfate was added to react, and after the reaction was completed, a dispersion was obtained;
[0085] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0086] Compared with Example 1, in Comparative Example 2, the sepiolite powder was replaced with bentonite.
[0087] Comparative Example 3
[0088] A method for preparing a composite carboxylated styrene-butadiene latex for coating paper comprises the following steps:
[0089] S1. Add 10 g of sepiolite powder to 100 mL of 1 mol / L NaOH solution, heat and stir at 50° C. for 3 h, then filter, wash and dry to obtain pretreated sepiolite powder;
[0090] S2, ultrasonically dispersing 8 g of pretreated sepiolite powder in 100 mL of 80 wt% ethanol aqueous solution, then adding 2 g of vinyltriethoxysilane thereto, heating and stirring at 50° C. for 3 h, then filtering, washing, and drying to obtain modified sepiolite powder;
[0091] S3, adding 5g of modified sepiolite powder, 2g of sodium dodecyl sulfate and 2g of tert-dodecyl mercaptan to 100g of deionized water, stirring evenly, introducing nitrogen to exhaust the air, and then adding 15g of butadiene, 20g of styrene, 5g of acrylic acid and 5g of acrylamide thereto, stirring and heating to 60°C, adding 1g of initiator ammonium persulfate to react, and after the reaction is completed, a dispersion is obtained;
[0092] S4. Cool the dispersion to room temperature and degas at -0.08 MPa for 1 h to obtain composite carboxylated styrene-butadiene latex.
[0093] Compared with Example 1, Comparative Example 3 replaces N-hydroxyethyl acrylamide with acrylamide.
[0094] The composite carboxyl styrene butadiene latex prepared in Examples 1-4 and Comparative Examples 1-3 was subjected to performance tests, as follows:
[0095] Mechanical stability: According to SH / T 1151.1-2019 standard;
[0096] Chemical stability: According to SH / T 1608-2014 standard;
[0097] The test was performed 3 times and the results were averaged. The test results are shown in Table 1:
[0098] Table 1
[0099] Mechanical stability (%) Chemical stability (%) Example 1 0.007 0.003 Example 2 0.011 0.004 Example 3 0.006 0.006 Example 4 0.008 0.003 Comparative Example 1 0.163 0.079 Comparative Example 2 0.012 0.008 Comparative Example 3 0.008 0.006
[0100] The composite carboxylated styrene butadiene latex prepared in Examples 1-4 and Comparative Examples 1-3 was coated on the surface of paper, with a coating amount of 20 g / m 2 , and then tested after drying. The wet tensile strength of the paper was tested in accordance with the national standard GB / T 465.2-2008, and the dry tensile strength of the paper was tested in accordance with the national standard GB / T 12914-2018. The test was repeated 3 times and the average result was taken. The test results are shown in Table 2:
[0101] Table 2
[0102]
[0103] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A method for preparing a composite carboxylated styrene-butadiene latex for coating paper, characterized in that: The steps include: S1, adding sepiolite powder to an alkaline solution, heating and stirring, and then filtering, washing, and drying to obtain pretreated sepiolite powder; S2, ultrasonically dispersing the pretreated sepiolite powder in an ethanol aqueous solution, then adding a vinyl silane coupling agent thereto, heating and stirring to react, and then filtering, washing, and drying to obtain a modified sepiolite powder; S3, adding modified sepiolite powder, sodium dodecyl sulfate and tert-dodecyl mercaptan to deionized water, stirring evenly, introducing nitrogen to expel air, then adding butadiene, styrene, acrylic acid and N-hydroxyethyl acrylamide, stirring and heating to 55-60° C., adding an initiator to react, and after the reaction is completed, obtaining a dispersion; S4, cooling the dispersion to room temperature and performing physical degassing to obtain a composite carboxylated styrene-butadiene latex; Wherein, in step S1, the alkaline solution is selected from NaOH solution or KOH solution; In step S2, the mass ratio of the pretreated sepiolite powder to the vinyl silane coupling agent is 5-10:1-2; In step S3, the mass ratio of modified sepiolite powder, sodium dodecyl sulfate, tert-dodecyl mercaptan, deionized water, butadiene, styrene, acrylic acid, N-hydroxyethyl acrylamide and initiator is 4-8:1-3:2-3:100-120:15-20:20-25:5-10:5-10:1-1.5; The initiator is selected from persulfates.
2. The preparation method according to claim 1, characterized in that: In step S1, the temperature of heating and stirring is 40-60°C, and the time of heating and stirring is 1-5h.
3. The preparation method according to claim 1, characterized in that: In step S2, the temperature of the heating and stirring reaction is 50-65° C., and the time of the heating and stirring reaction is 2-3 h.
4. The preparation method according to claim 1, characterized in that: In step S3, the reaction time is 2-5 hours.
5. The preparation method according to claim 1, characterized in that: In step S4, the physical degassing conditions are: degassing at -0.08 MPa to -0.1 MPa for 1-2 h.
6. The composite carboxylated styrene-butadiene latex prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the composite carboxyl styrene butadiene latex as claimed in claim 6 in sizing the surface of paper.