A method for preparing magnesium-titanium type ultra-low-density ceramsite sand proppant
Through the preparation method of magnesium-titanium ultra-low density ceramic sand proppant, the problem of high density and high crushing rate of ceramic sand proppant is solved, and the effect of low density and high compressive strength is achieved. It is suitable for oil and natural gas underground Efficient support.
Patent Information
- Application Number
- CN202411194477.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The existing ceramic sand proppants have problems such as high density, high crushing rate and high production costs in the mining of deep oil and natural gas wells, and it is difficult to meet the needs of low density and high compressive strength.
The preparation method of magnesium-titanium ultra-low-density ceramic sand proppant is used to grind the powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash, and nanomagnesium oxide and nanoanatase are added. Titanium dioxide and nano-silica, combined with slurry of polyvinyl alcohol, sodium dodecyl sulfate, polyethylene glycol and dibutyl phthalate, are mixed and granulated, and are cut, dried, sieved and calcined. Magnesium-titanium-type ultra-low-density ceramic sand proppant was produced.
The density of ceramic sand proppant is reduced, the crushing rate is small, and the compressive strength is high, which reduces production costs and environmental pollution, and is suitable for efficient support underground oil and natural gas.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramsite sand proppant manufacturing, and in particular to a method for preparing a magnesium-titanium type ultra-low-density ceramsite sand proppant. Background Art
[0002] When deep wells are used for oil and gas exploitation, fracturing proppants are needed to keep the cracks formed after fracturing open so that oil and gas products can pass through smoothly, maintain high conductivity of the channel, and allow oil and gas to flow smoothly to increase production.
[0003] At present, the main fracturing proppants used in deep well exploitation of oil and natural gas in the market are quartz sand, ceramsite sand and resin-coated proppants. Quartz sand is suitable for fracturing in shallow well construction, and resin-coated proppants have the advantages of high sphericity, low breakage rate, strong corrosion resistance, and good conductivity, but they are expensive and have complex preparation processes. In the prior art, ceramsite sand is widely used as a fracturing proppant for oil. Due to various factors such as raw materials, content, and process, various types of ceramsite sand proppants currently exist, resulting in a series of problems such as high density, easy breakage, or high production cost.
[0004] Therefore, it is particularly important to develop products with low density, small breakage rate and high compressive strength for expanded clay sand proppants. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a method for preparing a magnesium-titanium type ultra-low density ceramsite sand proppant. The magnesium-titanium type ultra-low density ceramsite sand proppant obtained by the present invention has low density, small breakage rate and high compressive strength.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a magnesium-titanium type ultra-low density ceramsite sand proppant, comprising the following steps:
[0008] Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder;
[0009] Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder;
[0010] Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry;
[0011] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0012] Step S5: Screening and calcining the semi-finished ceramsite sand to obtain magnesium-titanium type ultra-low-density ceramsite sand proppant.
[0013] Preferably, in terms of mass fractions, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash.
[0014] For example, the mass fractions of the salt mud may be 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35.
[0015] For example, the mass fraction of the magnesium oxide may be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.
[0016] For example, the mass fraction of the titanium dioxide may be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or 16 parts.
[0017] For example, the mass fraction of bauxite may be 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or 21 parts.
[0018] For example, the mass fraction of the fly ash can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.
[0019] More preferably, the powder consists of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash in terms of mass.
[0020] Preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5-1.
[0021] More preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5.
[0022] Preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1.
[0023] More preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.
[0024] Preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1.
[0025] More preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5.
[0026] Preferably, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate in parts by mass.
[0027] More preferably, the slurry consists of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate in parts by mass.
[0028] In a second aspect, a magnesium-titanium type ultra-low density ceramsite sand proppant is provided, which is prepared by the preparation method described in the present invention.
[0029] Preferably, the preparation method comprises the following steps:
[0030] Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder;
[0031] Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder;
[0032] Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry;
[0033] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0034] Step S5: Screening and calcining the semi-finished ceramsite sand to obtain magnesium-titanium type ultra-low-density ceramsite sand proppant.
[0035] Preferably, in terms of mass fractions, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash.
[0036] For example, the mass fraction of the salt mud can be 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts or 35 parts.
[0037] For example, the mass fraction of the magnesium oxide may be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.
[0038] For example, the mass fraction of the titanium dioxide may be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or 16 parts.
[0039] For example, the mass fraction of bauxite may be 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or 21 parts.
[0040] For example, the mass fraction of the fly ash can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.
[0041] More preferably, the powder consists of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash in terms of mass.
[0042] Preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5-1.
[0043] More preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5.
[0044] Preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1.
[0045] More preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.
[0046] Preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1.
[0047] More preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5.
[0048] Preferably, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate in parts by mass.
[0049] More preferably, the slurry consists of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate in parts by mass.
[0050] In a third aspect, a fracturing proppant is provided, comprising the magnesium-titanium type ultra-low density ceramsite sand proppant as described in the present invention.
[0051] Preferably, the method for preparing the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0052] Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder;
[0053] Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder;
[0054] Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry;
[0055] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0056] Step S5: Screening and calcining the semi-finished ceramsite sand to obtain magnesium-titanium type ultra-low-density ceramsite sand proppant.
[0057] Preferably, in terms of mass fractions, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash.
[0058] For example, the mass fraction of the salt mud can be 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts or 35 parts.
[0059] For example, the mass fraction of the magnesium oxide may be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.
[0060] For example, the mass fraction of the titanium dioxide may be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or 16 parts.
[0061] For example, the mass fraction of bauxite may be 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or 21 parts.
[0062] For example, the mass fraction of the fly ash can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.
[0063] More preferably, the powder consists of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash in terms of mass.
[0064] Preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5-1.
[0065] More preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5.
[0066] Preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1.
[0067] More preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.
[0068] Preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1.
[0069] More preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5.
[0070] Preferably, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate in parts by mass.
[0071] More preferably, the slurry consists of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate in parts by mass.
[0072] In a fourth aspect, there is provided application of the magnesium-titanium type ultra-low density ceramsite sand proppant described in the present invention in oil production.
[0073] Preferably, the method for preparing the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0074] Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder;
[0075] Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder;
[0076] Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry;
[0077] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0078] Step S5: Screening and calcining the semi-finished ceramsite sand to obtain magnesium-titanium type ultra-low-density ceramsite sand proppant.
[0079] Preferably, in terms of mass fractions, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash.
[0080] For example, the mass fractions of the salt mud may be 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 or 35.
[0081] For example, the mass fraction of the magnesium oxide may be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.
[0082] For example, the mass fraction of the titanium dioxide may be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or 16 parts.
[0083] For example, the mass fraction of bauxite may be 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or 21 parts.
[0084] For example, the mass fraction of the fly ash can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.
[0085] More preferably, the powder consists of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash in terms of mass.
[0086] Preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5-1.
[0087] More preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5.
[0088] Preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1.
[0089] More preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.
[0090] Preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1.
[0091] More preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5.
[0092] Preferably, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate in parts by mass.
[0093] More preferably, the slurry consists of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate in parts by mass.
[0094] A fifth aspect provides the use of the magnesium-titanium type ultra-low density ceramsite sand proppant described in the present invention in natural gas well exploitation.
[0095] Preferably, the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0096] Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder;
[0097] Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder;
[0098] Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry;
[0099] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0100] Step S5: Screening and calcining the semi-finished ceramsite sand to obtain magnesium-titanium type ultra-low-density ceramsite sand proppant.
[0101] Preferably, step S4. cutting, drying and grinding the nano-mixed slurry to obtain nano-mixed powder; adding part of the nano-mixed powder into a granulator, and then spraying 5%-10% carboxymethyl cellulose solution into the granulator to form a mother core; after adding the nano-mixed powder, spraying high-mist water for granulation, repeating multiple times to obtain a semi-finished ceramsite sand product.
[0102] In the present invention, 5%-10% carboxymethyl cellulose solution is used to replace tap water, which is more conducive to the actual conversion of the semi-finished product from powder to granules.
[0103] Preferably, in terms of mass fractions, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash.
[0104] For example, the mass fraction of the salt mud can be 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts or 35 parts.
[0105] For example, the mass fraction of the magnesium oxide may be 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts.
[0106] For example, the mass fraction of the titanium dioxide may be 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or 16 parts.
[0107] For example, the mass fraction of bauxite may be 16 parts, 17 parts, 18 parts, 19 parts, 20 parts or 21 parts.
[0108] For example, the mass fraction of the fly ash can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.
[0109] More preferably, the powder consists of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash in terms of mass.
[0110] Preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5-1.
[0111] More preferably, the mass ratio of the magnesium oxide to the nano-magnesium oxide is 1:0.5.
[0112] Preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1.
[0113] More preferably, the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.
[0114] Preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1.
[0115] More preferably, the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5.
[0116] Preferably, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate in parts by mass.
[0117] More preferably, the slurry consists of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate in parts by mass.
[0118] Compared with the prior art, the beneficial effects of the present invention are:
[0119] The powder used in the preparation method of the magnesium-titanium ultra-low-density ceramsite sand proppant provided by the present invention is composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash. The raw material source is wide and can reduce environmental pollution. The ceramsite sand proppant prepared by the present invention not only has a small crushing rate, high compressive strength and ultra-low density. Furthermore, the present invention further improves the compressive strength of the ceramsite sand proppant prepared by using the powder of the specific mass fraction of the present invention by optimizing the mass fraction of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash in the powder, and further reduces the crushing rate of the ceramsite sand proppant prepared by using the ceramsite sand of the present invention; it also further reduces the density of the ceramsite sand proppant prepared by using the powder of the specific mass fraction of the present invention.
[0120] Adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide in nano form to the mixed powder can improve the compressive strength of the prepared ceramsite sand proppant; and by optimizing the mass ratio of magnesium oxide to nano magnesium oxide, the mass ratio of titanium dioxide to nano anatase titanium dioxide and the mass ratio of bauxite to nano silicon dioxide, the compressive strength of the ceramsite sand proppant can be better improved and the breakage rate of the ceramsite sand proppant prepared by the method of the present invention can be reduced.
[0121] In addition, the slurry composed of polyvinyl alcohol, sodium dodecyl sulfate, polyethylene glycol and dibutyl phthalate is added to the preparation process of ceramsite sand, which can reduce the friction and adhesion between the raw materials compared with other similar substances with similar properties; it is easier to mix the raw materials evenly; and at the same time, the mixed powder and nano-mixed powder of the present invention are combined to further improve the compressive strength of the ceramsite sand and reduce the breakage rate of the ceramsite sand proppant prepared by the method of the present invention. DETAILED DESCRIPTION
[0122] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0123] Example 1
[0124] This embodiment provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0125] Step S1. Grind a powder consisting of 25 parts of salt mud, 8 parts of magnesium oxide, 11 parts of titanium dioxide, 16 parts of bauxite and 20 parts of fly ash for 4 hours to obtain a mixed powder;
[0126] Step S2. 4 parts of nano magnesium oxide, 5.5 parts of nano anatase titanium dioxide and 8 parts of nano silicon dioxide are added to the mixed powder and ground for 5 hours to obtain a nano mixed powder;
[0127] Step S3. adding a slurry consisting of 0.2 parts of polyvinyl alcohol, 0.1 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.05 parts of dibutyl phthalate to the nano-mixed powder and grinding for 4 hours to obtain a nano-mixed slurry;
[0128] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0129] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0130] Example 2
[0131] This embodiment provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0132] Step S1. Grind a powder consisting of 35 parts of salt mud, 15 parts of magnesium oxide, 16 parts of titanium dioxide, 21 parts of bauxite and 30 parts of fly ash for 6 hours to obtain a mixed powder;
[0133] Step S2. 15 parts of nano-magnesium oxide, 16 parts of nano-anatase titanium dioxide and 21 parts of nano-silicon dioxide are added to the mixed powder and ground for 8 hours to obtain a nano-mixed powder;
[0134] Step S3. adding a slurry consisting of 0.5 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.1 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate to the nano-mixed powder and grinding for 6 hours to obtain a nano-mixed slurry;
[0135] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray high-mist water into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0136] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0137] Example 3
[0138] This embodiment provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0139] Step S1. Grind a powder consisting of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash for 5 hours to obtain a mixed powder;
[0140] Step S2. 5 parts of nano-magnesium oxide, 12 parts of nano-anatase titanium dioxide and 10 parts of nano-silicon dioxide are added to the mixed powder and ground for 6 hours to obtain a nano-mixed powder;
[0141] Step S3. adding a slurry consisting of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate to the nano-mixed powder and grinding for 5 hours to obtain a nano-mixed slurry;
[0142] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray 5%-10% carboxymethyl cellulose solution into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0143] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0144] Comparative Example 1
[0145] This comparative example provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0146] Step S1. Grind a powder consisting of 30 parts of salt mud, 10 parts of alumina, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash for 5 hours to obtain a mixed powder;
[0147] Step S2. 5 parts of nano-magnesium oxide, 12 parts of nano-anatase titanium dioxide and 10 parts of nano-silicon dioxide are added to the mixed powder and ground for 6 hours to obtain a nano-mixed powder;
[0148] Step S3. adding a slurry consisting of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate to the nano-mixed powder and grinding for 5 hours to obtain a nano-mixed slurry;
[0149] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray 5%-10% carboxymethyl cellulose solution into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0150] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0151] Comparative Example 2
[0152] This comparative example provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0153] Step S1. Grind a powder consisting of 30 parts of salt mud, 10 parts of magnesium oxide, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash for 5 hours to obtain a mixed powder;
[0154] Step S2. 11 parts of nano magnesium oxide, 12 parts of nano anatase titanium dioxide and 10 parts of nano silicon dioxide are added to the mixed powder and ground for 6 hours to obtain a nano mixed powder;
[0155] Step S3. adding a slurry consisting of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate to the nano-mixed powder and grinding for 5 hours to obtain a nano-mixed slurry;
[0156] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray 5%-10% carboxymethyl cellulose solution into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0157] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0158] Comparative Example 3
[0159] This comparative example provides a magnesium-titanium type ultra-low density ceramsite sand proppant, wherein the magnesium-titanium type ultra-low density ceramsite sand proppant is 30 / 50 mesh, and the preparation method of the magnesium-titanium type ultra-low density ceramsite sand proppant comprises the following steps:
[0160] Step S1. Grind a powder consisting of 30 parts of salt mud, 12 parts of titanium dioxide, 20 parts of bauxite and 22 parts of fly ash for 5 hours to obtain a mixed powder;
[0161] Step S2. 5 parts of nano-magnesium oxide, 12 parts of nano-anatase titanium dioxide and 10 parts of nano-silicon dioxide are added to the mixed powder and ground for 6 hours to obtain a nano-mixed powder;
[0162] Step S3. adding a slurry consisting of 0.3 parts of polyvinyl alcohol, 0.2 parts of sodium lauryl sulfate, 0.05 parts of polyethylene glycol and 0.1 parts of dibutyl phthalate to the nano-mixed powder and grinding for 5 hours to obtain a nano-mixed slurry;
[0163] Step S4. Cut, dry and grind the nano-mixed slurry to obtain a nano-mixed powder; add part of the nano-mixed powder to a granulator, and then spray 5%-10% carboxymethyl cellulose solution into the granulator to form a mother core; after adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain a semi-finished ceramsite sand;
[0164] Step S5. Screen and calcine the ceramsite sand semi-finished product to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; the ceramsite sand semi-finished product is screened using a 0.45-0.63 mm sieve; calcined by heating at a temperature of 100-800°C for 1-2 hours, then keeping warm at a temperature of 800°C for 1-2 hours, then heating at a temperature of 800-1200°C for 1-2 hours, and then calcining at a temperature of 1200-1400°C for 1-2 hours, and screening with a 0.3-0.6 mm sieve after calcination.
[0165] Experiment 1
[0166] The density of titanium-magnesium ultra-low-density ceramsite sand proppant was evaluated according to SY / T 5108-2014. The experimental results are shown in Table 1.
[0167] Table 1 Density test results of titanium-magnesium type ultra-low density ceramsite sand proppant
[0168]
[0169] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0170] A comparative example 1.1 is provided. Compared with Example 3, the difference of the comparative example 1.1 is that the salt mud of the present invention is replaced by red mud;
[0171] A comparative example 1.2 is provided. Compared with Example 3, the difference of the comparative example 1.2 is that the fly ash of the present invention is replaced with coal gangue;
[0172] Comparative Example 1.3 is provided. Compared with Example 3, the difference of Comparative Example 1.3 is that the dibutyl phthalate of the present invention is replaced by dioctyl adipate;
[0173] Comparative Example 1.4 is provided. Compared with Example 3, the difference of Comparative Example 1.4 is that the polyethylene glycol of the present invention is replaced by dioctyl adipate;
[0174] Comparative Example 1.5 is provided. Compared with Example 3, the difference of Comparative Example 1.5 is that the sodium lauryl sulfate of the present invention is replaced by sodium lauryl sulfonate;
[0175] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The density of the titanium-magnesium type ultra-low density ceramsite sand proppant prepared in Comparative Example 1.1, Comparative Example 1.2, Comparative Example 1.3, Comparative Example 1.4, and Comparative Example 1.5 was observed. The results were similar to those in the above Comparative Example 1.
[0176] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0177] A comparative example 2.1 is provided. Compared with Example 3, the difference of the comparative example 2.1 is that: the mass fraction of polyethylene glycol is adjusted to 0.2;
[0178] A comparative example 2.2 is provided. Compared with Example 3, the difference of the comparative example 2.2 is that: the mass fraction of polyvinyl alcohol is adjusted to 0.1;
[0179] A comparative example 2.3 is provided. Compared with Example 3, the difference of the comparative example 2.3 is that: the mass ratio of the magnesium oxide to the nano-magnesium oxide is 0.5:1;
[0180] A comparative example 2.4 is provided. Compared with Example 3, the difference of the comparative example 2.4 is that: the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.5;
[0181] A comparative example 2.5 is provided. Compared with Example 3, the difference of the comparative example 2.5 is that: the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.4;
[0182] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low-density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The density of the titanium-magnesium type ultra-low-density ceramsite sand proppant prepared in Comparative Example 2.1, Comparative Example 2.2, Comparative Example 2.3, Comparative Example 2.4, and Comparative Example 2.5 was observed. The results were similar to those in the above Comparative Example 2.
[0183] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0184] A comparative example 3.1 is provided. Compared with Example 3, the difference of the comparative example 3.1 is that: no salt mud is added;
[0185] A comparative example 3.2 is provided. Compared with Example 3, the difference of the comparative example 3.2 is that: magnesium oxide is not added;
[0186] A comparative example 3.3 is provided. Compared with Example 3, the difference of the comparative example 3.3 is that: no bauxite is added;
[0187] A comparative example 3.4 is provided. Compared with Example 3, the difference of the comparative example 3.4 is that: fly ash is not added;
[0188] A comparative example 3.5 is provided. Compared with Example 3, the difference of comparative example 3.5 is that no nano magnesium oxide is added.
[0189] A comparative example 3.6 is provided. Compared with Example 3, the difference of comparative example 3.6 is that no nano-anatase titanium dioxide or nano-silicon dioxide is added.
[0190] A comparative example 3.7 is provided. Compared with Example 3, the difference of comparative example 3.7 is that polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol or dibutyl phthalate is not added to the slurry.
[0191] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The density of the titanium-magnesium type ultra-low density ceramsite sand proppant prepared in Comparative Example 3.1, Comparative Example 3.2, Comparative Example 3.3, Comparative Example 3.4, Comparative Example 3.5, Comparative Example 3.6, and Comparative Example 3.7 was observed. The results were similar to those in the above Comparative Example 3.
[0192] As can be seen from Table 1, the method of the present invention can effectively reduce the density of the titanium-magnesium ultra-low-density ceramsite sand proppant, and the titanium-magnesium ultra-low-density ceramsite sand proppant prepared in Example 3 has the lowest density. The titanium-magnesium ultra-low-density ceramsite sand proppant prepared by the present invention has the lowest density while ensuring high strength, thereby reducing the difficulty of pumping, reducing the wear of ceramsite on equipment, and reducing the cost of fracturing. However, the density of the hydrophobic ultra-low-density ceramsite sand proppant prepared without the method of the present invention is relatively large, and cannot well meet the use requirements of oil and natural gas extraction.
[0193] Experiment 2
[0194] The compressive strength and crushing rate of magnesium-titanium ultra-low density ceramsite sand proppant were evaluated according to SY / T 5108-2014. The experimental results are shown in Table 2.
[0195] Table 2 Experimental results of magnesium-titanium ultra-low density ceramsite sand proppant
[0196]
[0197] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0198] A comparative example 1.1 is provided. Compared with Example 3, the difference of the comparative example 1.1 is that the salt mud of the present invention is replaced by red mud;
[0199] A comparative example 1.2 is provided. Compared with Example 3, the difference of the comparative example 1.2 is that the fly ash of the present invention is replaced with coal gangue;
[0200] Comparative Example 1.3 is provided. Compared with Example 3, the difference of Comparative Example 1.3 is that the dibutyl phthalate of the present invention is replaced by dioctyl adipate;
[0201] Comparative Example 1.4 is provided. Compared with Example 3, the difference of Comparative Example 1.4 is that the polyethylene glycol of the present invention is replaced by dioctyl adipate;
[0202] Comparative Example 1.5 is provided. Compared with Example 3, the difference of Comparative Example 1.5 is that the sodium lauryl sulfate of the present invention is replaced by sodium lauryl sulfonate;
[0203] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The crushing rate of the titanium-magnesium type ultra-low density ceramsite sand proppant prepared in Comparative Example 1.1, Comparative Example 1.2, Comparative Example 1.3, Comparative Example 1.4, and Comparative Example 1.5 was observed. The results were similar to those in the above Comparative Example 1.
[0204] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0205] A comparative example 2.1 is provided. Compared with Example 3, the difference of the comparative example 2.1 is that: the mass fraction of polyethylene glycol is adjusted to 0.2;
[0206] A comparative example 2.2 is provided. Compared with Example 3, the difference of the comparative example 2.2 is that: the mass fraction of polyvinyl alcohol is adjusted to 0.1;
[0207] A comparative example 2.3 is provided. Compared with Example 3, the difference of the comparative example 2.3 is that: the mass ratio of the magnesium oxide to the nano-magnesium oxide is 0.5:1;
[0208] A comparative example 2.4 is provided. Compared with Example 3, the difference of the comparative example 2.4 is that: the mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:1.5;
[0209] A comparative example 2.5 is provided. Compared with Example 3, the difference of the comparative example 2.5 is that: the mass ratio of the bauxite to the nano-silicon dioxide is 1:0.4;
[0210] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low-density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The crushing rate of the titanium-magnesium type ultra-low-density ceramsite sand proppant prepared in Comparative Example 2.1, Comparative Example 2.2, Comparative Example 2.3, Comparative Example 2.4, and Comparative Example 2.5 was observed. The results were similar to those in the above Comparative Example 2.
[0211] Similarly, in order to further illustrate the beneficial effects of the present invention, the following comparative examples are provided:
[0212] A comparative example 3.1 is provided. Compared with Example 3, the difference of the comparative example 3.1 is that: no salt mud is added;
[0213] A comparative example 3.2 is provided. Compared with Example 3, the difference of the comparative example 3.2 is that: magnesium oxide is not added;
[0214] A comparative example 3.3 is provided. Compared with Example 3, the difference of the comparative example 3.3 is that: no bauxite is added;
[0215] A comparative example 3.4 is provided. Compared with Example 3, the difference of the comparative example 3.4 is that: fly ash is not added;
[0216] A comparative example 3.5 is provided. Compared with Example 3, the difference of comparative example 3.5 is that no nano magnesium oxide is added.
[0217] A comparative example 3.6 is provided. Compared with Example 3, the difference of comparative example 3.6 is that no nano-anatase titanium dioxide or nano-silicon dioxide is added.
[0218] A comparative example 3.7 is provided. Compared with Example 3, the difference of comparative example 3.7 is that polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol or dibutyl phthalate is not added to the slurry.
[0219] Combined with the preparation method of the present invention, a titanium-magnesium type ultra-low density ceramsite sand proppant was prepared, and the test was carried out according to the test method in the effect verification. The crushing rate of the titanium-magnesium type ultra-low density ceramsite sand proppant prepared in Comparative Example 3.1, Comparative Example 3.2, Comparative Example 3.3, Comparative Example 3.4, Comparative Example 3.5, Comparative Example 3.6, and Comparative Example 3.7 was observed. The results are similar to those in the above Comparative Example 3.
[0220] As can be seen from Table 2, the magnesium-titanium ultra-low-density ceramsite sand proppant prepared by the method of the present invention has a small crushing rate at a crushing rate of 69 MPa, indicating that the magnesium-titanium ultra-low-density ceramsite sand proppant of the present invention has a high fracturing strength and can be well used for downhole support in oil fields, thereby increasing the production of oil and natural gas. However, the magnesium-titanium ultra-low-density ceramsite sand proppant not prepared by the method of the present invention has a large crushing rate at a crushing rate of 69 MPa, which cannot meet the support strength of downhole in oil fields.
[0221] It should be understood that the disclosed invention is not limited only to the specific method, scheme and material of description, because these all can change.It should also be understood that the terminology used herein is only for the purpose of describing specific embodiment scheme, rather than being intended to limit the scope of the present invention, and the scope of the present invention is only limited to the appended claims.
[0222] Those skilled in the art will also recognize, or be able to ascertain using no more than routine experimentation, many equivalents to the specific embodiments of the invention described herein. Such equivalents are also intended to be encompassed by the appended claims.
Claims
1. A method for preparing a magnesium-titanium type ultra-low density ceramsite sand proppant, characterized in that: The following steps are involved: Step S1. Grinding a powder composed of salt mud, magnesium oxide, titanium dioxide, bauxite and fly ash to obtain a mixed powder; Step S2. adding nano magnesium oxide, nano anatase titanium dioxide and nano silicon dioxide to the mixed powder and grinding them to obtain a nano mixed powder; Step S3. adding a slurry consisting of polyvinyl alcohol, sodium lauryl sulfate, polyethylene glycol and dibutyl phthalate to the nano-mixed powder and grinding the mixture to obtain a nano-mixed slurry; Step S4. Cutting, drying and grinding the nano-mixed slurry to obtain a nano-mixed powder; Add part of the nano-mixed powder into the granulator, and then spray high-mist water into the granulator to form a mother core; After adding the nano-mixed powder, spray high-mist water for granulation, repeat several times to obtain the semi-finished ceramsite sand; Step S5. Screening and calcining the semi-finished ceramsite sand to obtain a magnesium-titanium ultra-low-density ceramsite sand proppant; In terms of mass fraction, the powder consists of 25-35 parts of salt mud, 8-15 parts of magnesium oxide, 11-16 parts of titanium dioxide, 16-21 parts of bauxite and 20-30 parts of fly ash; The mass ratio of the magnesium oxide to the nano magnesium oxide is 1:0.5-1; The mass ratio of the titanium dioxide to the nano-anatase titanium dioxide is 1:0.5-1; The mass ratio of the bauxite to the nano-silicon dioxide is 1:0.5-1; In terms of weight percentage, the slurry consists of 0.2-0.5 parts of polyvinyl alcohol, 0.1-0.2 parts of sodium lauryl sulfate, 0.05-0.1 parts of polyethylene glycol and 0.05-0.1 parts of dibutyl phthalate.
2. A magnesium-titanium type ultra-low density ceramsite sand proppant, characterized in that: The method is prepared according to claim 1.
3. A fracturing proppant, characterized in that: It includes the magnesium-titanium type ultra-low-density ceramsite sand proppant as described in claim 2.
4. Use of the magnesium-titanium type ultra-low density ceramsite sand proppant according to claim 2 in oil production.
5. Use of the magnesium-titanium type ultra-low density ceramsite sand proppant according to claim 2 in natural gas well exploitation.