A copper / silver-based solid solution composite bump interconnection method and interconnection structure
By forming a silver-based solid solution film on the surface of the copper bump and performing hot press bonding, the problem of high temperature and high pressure required for copper-copper solid-state interconnection is solved, the plastic deformation capability of the copper bump is improved, the packaging quality is ensured and the chip is reduced damage.
Patent Information
- Application Number
- CN202411188988.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-28
AI Technical Summary
Copper-copper solid-state interconnects Due to the high yield strength and hardness of copper, they need to be bonded at higher temperatures and high pressures, resulting in cracks or fractures in the interconnect structure, which is difficult to ensure packaging quality and may damage the chip.
The interconnection method of copper/silver-based solid solution composite bumps is adopted. A silver-based solid solution film is formed on the surface of copper bumps by magnetron sputtering, and the thermal bonding is carried out at a lower temperature and pressure, and the silver-based solid solution film is used to bear it. Plastic deformation.
While meeting the packaging strength, the plastic deformation capability of copper bumps is improved, the risk of cracks or fractures at the interconnections is reduced, the packaging quality is ensured and chip damage is reduced.
Smart Images

Figure CN118712079B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic packaging, and in particular to an interconnection method and an interconnection structure of copper / silver-based solid solution composite bumps. Background Art
[0002] All-metal solid-state interconnects are widely used in the field of electronic packaging because they can avoid the generation of intermetallic compounds (IMC) in the interface, reduce interface thermal stress, and improve the reliability of the interconnect structure. At present, the materials of all-metal solid-state interconnects are mainly copper, nickel, gold or silver. Because copper has high strength, good conductivity, low cost and good processability, it is often used as a packaging material in the field of electronic packaging solid-state interconnects.
[0003] However, there are still some unresolved technical difficulties in copper-copper solid-state interconnection. Due to the high strength and hardness of copper and its poor plastic deformation ability, a bonding structure with good bonding can only be obtained under higher temperatures (>250°C) and higher pressures (>30MPa). High temperatures and high pressures can easily cause damage to the chip, so they need to be strictly avoided during the bonding process.
[0004] At present, most of the methods are to reduce the surface roughness of copper bumps and use chemical mechanical polishing (CMP) and other methods to make the bump surface extremely flat, so as to achieve copper-copper bump solid-state interconnection at lower temperature and pressure. However, this method usually requires extremely harsh process conditions and is difficult to apply on a large scale in industrial applications. Alternatively, low-temperature and low-pressure solid-state bonding of copper-copper bumps can be achieved by promoting atomic diffusion and rearrangement at the interconnection. However, this method has limited atomic diffusion free path, low interconnection strength, and difficulty in ensuring chip connection reliability. Summary of the invention
[0005] The invention provides an interconnection method and an interconnection structure of copper / silver-based solid solution composite bumps, which at least solve the problems that, when copper-copper bumps of a chip are currently bonded and interconnected, due to the large yield strength and hardness of copper, plastic deformation of the copper surface can only occur under conditions of high temperature and high pressure, resulting in cracks or fractures in the interconnection structure, making it difficult to ensure the packaging quality of the copper bumps, and the chip is easily damaged after being subjected to high temperature and high pressure.
[0006] In a first aspect, the present invention provides a method for interconnecting copper / silver-based solid solution composite bumps, comprising the steps of:
[0007] Step S1, cleaning and drying the copper bump chip;
[0008] Step S2, sputtering a silver-based solid solution film onto the surface of the copper bump using a magnetron sputtering device to obtain a copper / silver-based solid solution composite bump chip;
[0009] Step S3, cleaning and drying the copper / silver-based solid solution composite bump chip obtained in step S2;
[0010] Step S4, performing steps S1 to S3 on another copper bump chip to obtain another copper / silver-based solid solution composite bump chip, and then performing hot pressing bonding treatment on the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips to complete the interconnection of the two copper / silver-based solid solution composite bump chips.
[0011] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, step S1 specifically comprises: using a professional cleaning agent and cleaning equipment to clean the copper bump chip, and after cleaning, drying the moisture on the surface of the copper bump chip.
[0012] According to a method for interconnecting copper / silver-based solid solution composite bumps provided by the present invention, step S2 specifically comprises: installing a silver-based solid solution target material on the target material position of the magnetron sputtering device, and placing the copper bump chip in the sample chamber of the magnetron sputtering device; evacuating the sample chamber, and then introducing a working gas into the sample chamber, wherein the working gas bombards the silver-based solid solution target material, so that the silver-based solid solution target material is sputtered to the surface of the copper bump, so as to form the silver-based solid solution film on the surface of the copper bump.
[0013] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, the flow rate of the working gas bombarding the silver-based solid solution target material is 20 sccm~70 sccm, the pressure of the sample chamber is 0.2 Pa~0.65 Pa; the working gas is argon.
[0014] According to the interconnection method of the copper / silver-based solid solution composite bump provided by the present invention, the vacuum degree of the sample chamber is not less than 8×10 -4 Pa, the sputtering power of the sputtering power supply is 100W~150W, and the sputtering time is 50min~60min.
[0015] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, step S2 specifically comprises sputtering a 3 μm-5 μm thick silver-based solid solution film onto the surface of the copper bump.
[0016] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, step S3 specifically comprises: using a professional cleaning agent and cleaning equipment to clean the copper / silver-based solid solution composite bump chip; after cleaning, drying the moisture on the surface of the copper / silver-based solid solution composite bump chip.
[0017] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, in step S4, the temperature of hot pressing bonding is not higher than 250° C., the bonding pressure is lower than or equal to 30 MPa, and the bonding time is 30 min to 40 min.
[0018] According to a copper / silver-based solid solution composite bump interconnection method provided by the present invention, in step S4, the copper / silver-based solid solution composite bumps of two copper / silver-based solid solution composite bump chips are thermally pressed and bonded under vacuum or inert gas atmosphere.
[0019] In a second aspect, the present invention further provides an interconnection structure, comprising a first chip and a second chip, wherein the first chip and the second chip are each provided with a plurality of the copper bumps, and the plurality of the copper bumps on the first chip and the plurality of the copper bumps on the second chip are interconnected one-to-one using the interconnection method of the copper / silver-based solid solution composite bumps as described in any of the above items.
[0020] The present invention provides a copper / silver-based solid solution composite bump interconnection method and interconnection structure, wherein one of the copper bump chips to be connected is first cleaned and dried for standby, and then a silver-based solid solution film is sputtered onto the surface of the copper bump by a magnetron sputtering device to obtain a copper / silver-based solid solution composite bump chip, and then the copper / silver-based solid solution composite bump chip is cleaned and dried; then, the same steps are performed on another copper bump chip to be connected to obtain another copper / silver-based solid solution composite bump chip, and then the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips are subjected to hot pressing bonding, so that the interconnection of the two copper / silver-based solid solution composite bump chips can be completed. A layer of silver-based solid solution film with strong plastic deformation ability is made on the surface of the copper bump by the magnetron sputtering method, so that the silver-based solid solution film bears most of the plastic deformation in the bonding interconnection, thereby reducing the temperature and pressure required in the solid-state bonding process of the copper bump. Compared with the traditional pure copper bump interconnection, the present invention greatly improves the plastic deformation ability of the copper bump while meeting the packaging strength, and the interconnection is less likely to crack or break, thereby ensuring the packaging quality and reducing the degree of damage to the chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 The present invention provides a schematic flow diagram of a copper / silver-based solid solution composite bump interconnection method.
[0023] Figure 2 The present invention provides an array electron microscope image of copper / silver-based solid solution composite bumps in a copper / silver-based solid solution composite bump chip provided in an embodiment of the present invention.
[0024] Figure 3 It is a cross-sectional electron microscope image of a copper / silver-based solid solution composite bump in a copper / silver-based solid solution composite bump chip provided in an embodiment of the present invention.
[0025] Figure 4 It is an electron microscope image of the interconnection structure provided by an embodiment of the present invention.
[0026] Figure 5 It is a schematic diagram of the connection structure of the interconnection structure provided by an embodiment of the present invention.
[0027] Reference numerals:
[0028] 1. First chip; 11. Copper bump; 12. Silver-based solid solution film; 2. Second chip. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The features of the terms "first" and "second" in the specification and claims of the present invention may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.
[0031] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0032] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0033] Combine the following Figures 1 to 5 , through specific embodiments and application scenarios, an interconnection method and an interconnection structure of a copper / silver-based solid solution composite bump provided by an embodiment of the present invention are described in detail.
[0034] First, as Figure 1 As shown, the present invention provides a copper / silver-based solid solution composite bump interconnection method, comprising the steps of:
[0035] Step S1, cleaning and drying the copper bump chip.
[0036] Step S2, sputtering a silver-based solid solution film onto the surface of the copper bump using a magnetron sputtering device to obtain a copper / silver-based solid solution composite bump chip.
[0037] Step S3, cleaning and drying the copper / silver-based solid solution composite bump chip obtained in step S2.
[0038] Step S4, performing steps S1 to S3 on another copper bump chip to obtain another copper / silver-based solid solution composite bump chip; then performing a hot pressing bonding process on the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips to complete the interconnection of the two copper / silver-based solid solution composite bump chips.
[0039] The traditional way of interconnecting chips is to place two copper bump chips to be bonded under high temperature and high pressure to cause plastic deformation on the surface of the copper bumps, and then heat-press the two copper bumps together. However, when the chip is placed under high temperature and high pressure, its internal structure is easily damaged, which affects the communication and data transmission quality of the chip.
[0040] The interconnection method of the copper / silver-based solid solution composite bump provided by the present invention is to attach a layer of silver-based solid solution film on the surface of the copper bump. Compared with copper, the silver-based solid solution has a smaller yield strength and hardness. Therefore, in the interconnection process, the copper / silver-based solid solution composite bump chip only needs to be placed under a lower temperature and a lower pressure, and the two can be hot-pressed and bonded.
[0041] Specifically, the interconnection method of the copper / silver-based solid solution composite bump provided by the present invention, in step S1, first the copper bump chip is cleaned and dried. Cleaning and drying the copper bump chip is a very important step, which can ensure the good combination of the copper bump and the silver-based solid solution. The stains on the surface of the copper bump chip can be removed by using a professional cleaning agent and a professional cleaning equipment, and then the moisture on the surface of the copper bump chip is dried by a drying equipment for standby use.
[0042] Step S2, sputtering a silver-based solid solution film onto the surface of the copper bump using a magnetron sputtering device. The silver-based solid solution refers to a solid solution formed by silver as a solvent component and other metal or non-metal elements. In order to regulate the plastic deformation ability, electrical conductivity, hardness or corrosion performance of the silver-based solid solution, different types of solutes can be dissolved in pure silver. In the present invention, for example, indium element can be added to the silver-based solid solution to form a silver-indium solid solution. The silver-indium solid solution has high plastic deformation ability, excellent electrical conductivity and low yield strength. When preparing a silver-based solid solution target material, physical vapor deposition, chemical vapor deposition or solution method and other processes can be used to ensure that the required elements are evenly distributed in the lattice.
[0043] Magnetron sputtering equipment is a process equipment used for thin film deposition. It uses magnetic field and ion bombardment to release materials from the target surface and deposit them on the substrate to form a thin film. After the silver-based solid solution target is prepared, the silver-based solid solution target is placed in the magnetron sputtering equipment, and the silver-based solid solution is sputtered on the surface of the copper bump by the magnetron sputtering equipment to form a silver-based solid solution film, thereby obtaining a copper / silver-based solid solution composite bump chip.
[0044] Step S3, cleaning and drying the copper / silver-based solid solution composite bump chip obtained in step S2. The copper / silver-based solid solution composite bump chip needs to be cleaned with a special cleaning agent and equipment to remove dirt, grease or other impurities on the surface. After cleaning, the copper / silver-based solid solution composite bump chip is placed in an oven to dry the moisture on its surface.
[0045] Step S4, performing steps S1 to S3 on another copper bump chip to be interconnected, to obtain another copper / silver-based solid solution composite bump chip. Then, the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips are subjected to hot pressing bonding treatment to complete the interconnection of the two copper / silver-based solid solution composite bump chips. After the two copper / silver-based solid solution composite bump chips are prepared, the two copper / silver-based solid solution composite bump chips are hot pressed and bonded together using a hot pressing bonding device to complete the interconnection of the two copper / silver-based solid solution composite bump chips.
[0046] The present invention provides a copper / silver-based solid solution composite bump interconnection method, wherein one of the copper bump chips to be connected is first cleaned and dried for standby use, and then a silver-based solid solution film is sputtered onto the surface of the copper bump by a magnetron sputtering device to obtain a copper / silver-based solid solution composite bump chip, and then the obtained copper / silver-based solid solution composite bump chip is cleaned and dried. Next, the same steps are performed on another copper bump chip to be connected to obtain another copper / silver-based solid solution composite bump chip, and then the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips are subjected to hot pressing bonding treatment, so that the interconnection of the two copper / silver-based solid solution composite bump chips can be completed. A layer of silver-based solid solution with strong plastic deformation ability is made on the surface of the copper bump by the magnetron sputtering method, so that the silver-based solid solution bears most of the plastic deformation in the bonding interconnection, thereby reducing the temperature and pressure required for the solid-state bonding process of the copper bump. Compared with the traditional pure copper bump interconnection, the present invention greatly improves the plastic deformation ability of the copper bump surface while meeting the packaging strength, making the interconnection structure less prone to cracks or fractures, ensuring the packaging quality and reducing the possibility of chip damage.
[0047] Furthermore, step S1 is specifically as follows:
[0048] The copper bump chip is cleaned using a special cleaning agent and cleaning equipment. After cleaning, the moisture on the surface of the copper bump is dried.
[0049] First, the copper bump chip is cleaned using specialized cleaning agents and equipment to remove dirt, grease or other impurities on the surface. The cleaning process requires the use of appropriate chemicals and process parameters to ensure that the structure of the chip and the bump is not damaged.
[0050] The copper bump chip can be cleaned with acetone, alcohol and deionized water in sequence, with each cleaning time being 5 to 10 minutes.
[0051] After cleaning, place the chip in a drying device to ensure that moisture and cleaning agent residues are completely removed. The drying temperature should not be too high to avoid overheating and chip damage.
[0052] Step S2 specifically includes installing a silver-based solid solution target material on a target position of a magnetron sputtering device, and placing a copper bump chip in a sample chamber of the magnetron sputtering device; evacuating the sample chamber, and then introducing a working gas into the sample chamber, wherein the working gas bombards the silver-based solid solution target material, so that the silver-based solid solution target material is sputtered onto the surface of the copper bump chip to form a silver-based solid solution film on the surface of the copper bump.
[0053] The magnetron sputtering device has a sample chamber. The magnetron sputtering device is provided with a target mounting position and a substrate stage. The target mounting position and the substrate stage are arranged relative to each other. The sample chamber of the magnetron sputtering device is usually made of high vacuum sealed metal or ceramic material to ensure that the required high vacuum environment is formed in the sample chamber, which helps to prevent impurities such as oxygen and water vapor from having a negative impact on the deposited film, and is also conducive to improving the utilization rate of the silver-based solid solution target material and the quality of the silver-based solid solution film during the sputtering process.
[0054] During sputtering, the silver-based solid solution target is mounted on the target mounting position, and the copper bump chip is fixed on the substrate. Furthermore, the sample chamber is evacuated by a mechanical pump and a molecular pump in turn, and after the vacuum degree in the sample chamber meets the requirement, a working gas is introduced into the sample chamber; then, the bombardment energy and bombardment direction of the working gas on the silver-based solid solution target are controlled by applying a magnetic field. Under the bombardment of the working gas, the silver-based solid solution is sputtered to the surface of the copper bump, thereby forming a silver-based solid solution film on the surface of the copper bump.
[0055] In a specific embodiment, step S2 is specifically to sputter a 3 μm to 5 μm thick silver-based solid solution film onto the surface of the copper bump. The magnetic field is controlled so that the flow rate of the working gas bombarding the silver-based solid solution target is 20 sccm to 70 sccm, and the total pressure in the sample chamber is controlled to be 0.2 Pa to 0.65 Pa, ensuring that the working gas has sufficient bombardment intensity to ensure a better sputtering effect. The working gas is an inert gas. The working gas can be argon.
[0056] Furthermore, during the sputtering process, the vacuum degree of the sample chamber is not less than 8×10 -4 Pa. A DC power supply is used as the sputtering power supply of the magnetron sputtering equipment, and the sputtering power is 100W~150W. The sputtering time of sputtering a 3μm~5μm thick silver-based solid solution film on the surface of the copper bump is 50min~60min.
[0057] To ensure the best sputtering effect, preferably, the diameter of the copper bump is 30 μm, the thickness of the silver-based solid solution film is 3 μm, the working gas is argon, the flow rate of argon is 30 sccm, the total pressure in the sample chamber is 0.3 Pa, the sputtering power is 100 W, and the sputtering time is 60 min. After sputtering, a copper / silver-based solid solution composite bump chip is obtained.
[0058] Step S3 specifically includes cleaning the copper / silver-based solid solution composite bump chip obtained in step S2 using a special cleaning agent and cleaning equipment. After cleaning, the moisture on the surface of the copper / silver-based solid solution composite bump chip is dried.
[0059] After sputtering, the copper / silver-based solid solution composite bump chip is taken out of the sample chamber, and then the copper / silver-based solid solution composite bump chip is cleaned using a special cleaning agent and cleaning equipment to remove surface impurities. The cleaning process requires the use of appropriate chemicals and process parameters to ensure that the silver-based solid solution film on the copper bump surface is not damaged.
[0060] In some embodiments, acetone, alcohol and deionized water may be used to clean the copper / silver-based solid solution composite bump chip in sequence, and each cleaning time is 5 minutes to 10 minutes.
[0061] After cleaning, the copper / silver-based solid solution composite bump chip is placed in a drying device to ensure complete removal of moisture and cleaning agent residues.
[0062] Furthermore, in step S4, the temperature of hot pressing is not higher than 250°C, and the bonding pressure is lower than or equal to 30MPa to ensure the hot pressing bonding effect of the copper / silver-based solid solution composite bump chip. The bonding time is 30min~40min. Among them, a flip-chip bonding device can be used to align several copper / silver-based solid solution composite bumps on two copper / silver-based solid solution composite bump chips one by one and then hot pressing and bonding are performed in sequence. Preferably, the bonding time is 30 min.
[0063] In step S4, two copper / silver-based solid solution composite bump chips are subjected to hot pressing bonding treatment in a vacuum or inert gas atmosphere to prevent oxidation of the surface of the silver-based solid solution film during the bonding process and ensure the conductive performance of the silver-based solid solution film.
[0064] The following is an introduction in conjunction with specific embodiments. Example 1
[0065] The first step is to clean the copper bump chip with acetone, alcohol and deionized water in turn, with each cleaning time being 5 minutes to 10 minutes. Then put the chip into an oven to dry the moisture for later use.
[0066] In the second step, the copper bump chip is placed on the substrate table in the sample chamber of the magnetron sputtering equipment, and the silver-based solid solution target is installed on the target mounting rack in the sample chamber. The vacuum degree of the sample chamber is not less than 8×10 -4 Pa. The working gas is argon, and the flow rate of argon is 30 sccm. The total pressure in the sample chamber is 0.3Pa, the sputtering power is 100W, and the sputtering time is 60min. The thickness of the silver-based solid solution film is 3μm. The diameter of the copper bump is 30μm. After sputtering multiple copper bumps on the copper bump chip, the following is formed Figure 2 The copper / silver-based solid solution composite bump array is shown in FIG. The cross-sectional structure of a single copper / silver-based solid solution composite bump is shown in FIG. Figure 3 shown.
[0067] The third step is to clean the copper / silver-based solid solution composite bump chip with acetone, alcohol and deionized water in turn after sputtering. Each cleaning time is 5 to 10 minutes. Then put the chip into an oven to dry the moisture for later use.
[0068] The fourth step is to use a flip-chip bonding device to solid-state bond the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips under vacuum or inert gas atmosphere to form a Figure 4 The interconnection structure shown in FIG. 1 , wherein the hot pressing temperature is not higher than 250° C., the bonding pressure is lower than or equal to 30 MPa, and the bonding time is 30 min. Example 2
[0069] The copper / silver-based solid solution composite bump bonding chip with a silver-based solid solution film in Example 1 and the traditional copper bump bonding chip are respectively loaded on a push-pull force device. The push-pull force parameters of the push-pull force device are set to obtain the maximum push-pull force of the two chips respectively. Then, the bonding areas of the two chips are measured respectively. By dividing the maximum push-pull force by the bonding area, the shear strength of the two chips is calculated respectively.
[0070] The analysis results show that the shear strength of the chip with copper / silver-based solid solution composite bump bonding is significantly greater than the shear strength of the traditional copper bump bonding chip. The mechanical properties of the traditional copper bump bonding chip are greatly improved and the bonding strength can be guaranteed.
[0071] Second, as Figure 5 As shown, the present invention also provides an interconnection structure, including a first chip 1 and a second chip 2. A plurality of copper bumps 11 are provided on the first chip 1 and the second chip 2. The plurality of copper bumps 11 on the first chip 1 and the plurality of copper bumps 11 on the second chip 2 are interconnected one by one using the interconnection method of the copper / silver-based solid solution composite bumps as described above.
[0072] It is understandable that if Figure 5 As shown, a silver-based solid solution film 12 is sputtered on the end face of each copper bump 11. In this embodiment, the thickness of the silver-based solid solution film 12 can be 3μm. The copper bumps 11 on the multiple first chips 1 and the multiple copper bumps 11 on the multiple second chips 2 correspond one to one, and are interconnected using the interconnection method described above. Therefore, by sputtering the silver-based solid solution film 12 on the copper bump 11, while giving full play to the high thermal conductivity and electrical conductivity of copper, it is possible to avoid the disadvantages of excessively high bonding temperature requirements due to the high strength of copper, so that stable bonding of the copper bump 11 can be achieved when the temperature and pressure are low, and cracks or fractures are not easily generated at the interconnection of the copper bump 11. At the same time, lower temperature and pressure can reduce the degree of damage to the chip.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for interconnecting copper / silver-based solid solution composite bumps, characterized in that: Includes steps: Step S1, cleaning and drying the copper bump chip; Step S2, using a magnetron sputtering device to sputter a 3μm~5μm thick silver-based solid solution film onto the surface of the copper bump to obtain a copper / silver-based solid solution composite bump chip; wherein, a silver-based solid solution target is installed on the target position of the magnetron sputtering device, and the copper bump chip is placed in the sample chamber of the magnetron sputtering device; the sample chamber is evacuated, and then a working gas is introduced into the sample chamber, the working gas bombards the silver-based solid solution target, so that the silver-based solid solution target is sputtered onto the surface of the copper bump to form the silver-based solid solution film on the surface of the copper bump, the flow rate of the working gas bombarding the silver-based solid solution target is 20 sccm~70 sccm, and the sputtering power of the sputtering power supply is 100W~150W; the pressure of the sample chamber is 0.2 Pa~0.65 Pa; the working gas is argon; the vacuum degree of the sample chamber is not less than 8×10 -4 Pa, sputtering time is 50min~60min; Step S3, cleaning and drying the copper / silver-based solid solution composite bump chip obtained in step S2; Step S4, performing steps S1 to S3 on another copper bump chip to obtain another copper / silver-based solid solution composite bump chip, and then performing hot pressing bonding treatment on the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips to complete the interconnection of the two copper / silver-based solid solution composite bump chips; the temperature of the hot pressing bonding is not higher than 250° C., the bonding pressure is lower than or equal to 30 MPa, and the bonding time is 30 min to 40 min.
2. The interconnection method of the copper / silver-based solid solution composite bump according to claim 1, characterized in that: Step S1 specifically includes: using a professional cleaning agent and cleaning equipment to clean the copper bump chip, and after cleaning, drying the moisture on the surface of the copper bump chip.
3. The interconnection method of the copper / silver-based solid solution composite bump according to claim 1, characterized in that: Step S3 specifically includes: using a professional cleaning agent and cleaning equipment to clean the copper / silver-based solid solution composite bump chip; after cleaning, drying the moisture on the surface of the copper / silver-based solid solution composite bump chip.
4. The interconnection method of the copper / silver-based solid solution composite bump according to claim 1, characterized in that: In step S4, the copper / silver-based solid solution composite bumps of the two copper / silver-based solid solution composite bump chips are thermally pressed and bonded under vacuum or inert gas atmosphere.
5. An interconnection structure, characterized in that: It comprises a first chip and a second chip, wherein the first chip and the second chip are both provided with a plurality of copper bumps, and the plurality of copper bumps on the first chip and the plurality of copper bumps on the second chip are interconnected one by one using the interconnection method of copper / silver-based solid solution composite bumps as described in any one of claims 1 to 4.