A production process for battery positive electrode slurry dispersant

By preparing the composite dispersant, the problems of poor solid dispersion and low solid content of the positive electrode slurry of lithium-ion battery are solved, the viscosity and coating efficiency are improved, and the service life and performance of the battery are extended.

CN118712386BActive Publication Date: 2024-11-12SHANXI HAOBOSEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411171417.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

During the production process, the lithium-ion battery positive electrode slurry has problems such as poor solid dispersion, low solid content and large viscosity, resulting in low coating efficiency and increased production costs.

Method used

Using a production process of battery positive electrode slurry dispersant, through the synthesis of copolymers, initiators and polymers, a composite dispersant is prepared to improve the solid content and dispersion of active substances, improve the dispersion of conductive carbon black, and Sodium allylsulfonate enhances wetting properties and prevents agglomeration and precipitation.

Benefits of technology

It improves the solid dispersion and viscosity of the battery positive electrode slurry, increases the solid content, reduces production costs, and extends the service life and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712386B_ABST
    Figure CN118712386B_ABST
Patent Text Reader

Abstract

The present invention provides a production process of a battery positive electrode slurry dispersant, belonging to the technical field of battery preparation; the preparation process comprises the following steps: synthesis of copolymer; preparation of initiator; preparation of polycaprolactone monomer; synthesis of polymer; preparation of compound dispersant. The compound dispersant prepared by the present invention increases the solid content of active substances in the battery positive electrode slurry, and increases the dispersibility of solid materials in the battery positive electrode slurry. Good dispersibility leads to a decrease in slurry viscosity, and helps to improve battery performance and service life by improving the dispersibility of components such as active substances and conductive agents in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery preparation, and in particular to a production process of a battery positive electrode slurry dispersant. Background Art

[0002] Since the 1990s, the research and production of lithium-ion batteries have made significant progress, and their applications in various fields have become more and more extensive. At present, they have gradually replaced lead-acid batteries and nickel-cadmium batteries and become the mainstream of power lithium batteries. Especially in the field of new energy vehicles, the market demand for lithium batteries has grown rapidly. However, compared with other equipment, new energy vehicles have higher requirements for the energy density, cycle life and other performance of lithium batteries.

[0003] When the positive electrode of a lithium-ion battery is formed, lithium iron phosphate slurry needs to be coated on aluminum foil, so the properties of the lithium iron phosphate slurry are directly related to the coating of the positive electrode. At present, the positive electrode slurries of most domestic lithium-ion battery manufacturers are similar, mainly composed of lithium iron phosphate powder, conductive carbon black, adhesive and NMP. However, during the production process, there are the following problems: (1) The positive electrode active materials (such as lithium iron phosphate) and conductive carbon black of lithium-ion batteries are not well dispersed in NMP, the positive electrode slurry has a high viscosity and is easy to agglomerate and precipitate; (2) After the positive electrode slurry is made into a current collector, there are problems of surface cracking and powder loss; (3) When the solid content of the slurry is high, the positive electrode slurry has a high viscosity, the coating efficiency is low, and the coating effect is poor.

[0004] Therefore, in order to reduce the viscosity of the slurry, the solid content of the slurry will be reduced, resulting in a corresponding increase in the amount of solvent (NMP) used in the slurry production process. As NMP is a precious solvent, the production cost and subsequent use and recycling costs are increased accordingly. At the same time, the reduction in the solid content of the electrode active material also affects the performance of the positive electrode.

[0005] Based on the above problems, the purpose of the present invention is to provide a production process for a battery positive electrode slurry dispersant. The produced dispersant is applied to the battery positive electrode slurry to solve the problems of poor solid dispersibility, low solid content and high slurry viscosity in the existing lithium-ion battery positive electrode slurry. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a production process for a battery positive electrode slurry dispersant.

[0007] A production process for a battery positive electrode slurry dispersant comprises the following steps:

[0008] S1: Synthesis of copolymers

[0009] The copolymer is prepared by polymerizing methyl methacrylate, styrene, sodium allyl sulfonate, benzoyl peroxide and xylene;

[0010] S2: Preparation of initiator

[0011] A yellow solution is prepared by using a mixed solution of potassium phosphate and acetone, 2-mercaptoethanol and carbon disulfide, and the yellow solution is added with benzyl bromide, filtered and rotary evaporated, and then purified by silica gel column chromatography to obtain an initiator;

[0012] S3: Preparation of polycaprolactone monomer

[0013] The polycaprolactone monomer is prepared by reacting ε-caprolactone, an initiator, 1,8-diazabicycloundec-7-ene and a tetrahydrofuran solution;

[0014] S4: Synthesis of polymers

[0015] The polymer is prepared by reacting polycaprolactone monomer, acrylic acid, azobisisobutyronitrile and dimethylformamide;

[0016] S5: Preparation of compound dispersant

[0017] The compound dispersant is obtained by compounding the polymer and the copolymer.

[0018] Furthermore, the synthesis of the copolymer in step S1 specifically comprises the following steps:

[0019] S1.1: Dissolve 40-50 parts by weight of methyl methacrylate, 50-60 parts by weight of styrene, 10-12 parts by weight of sodium allyl sulfonate and 1-2 parts by weight of benzoyl peroxide in 10-20 parts by weight of xylene, purge with high-purity nitrogen, polymerize at 98-100° C. for 40-45 minutes, and immediately add 50-60 parts by weight of ethanol to stop the reaction to obtain a precipitate;

[0020] S1.2: dissolving the precipitate in 10-20 parts by weight of dichloromethane, then adding 30-40 parts by weight of anhydrous ethanol for precipitation, and filtering and collecting the solid;

[0021] S1.3: Repeat the dissolution-precipitation process of step S1.2 2-3 times with the obtained solid to obtain a pure copolymer, and dry the pure copolymer in a vacuum until constant weight to obtain a copolymer.

[0022] Furthermore, step S2 prepares an initiator, which specifically comprises the following steps:

[0023] S2.1: Dissolve 5-6 parts by weight of potassium phosphate in 40-50 parts by weight of acetone to obtain a mixed solution, add 2-3 parts by weight of 2-mercaptoethanol to the mixed solution, stir for 10-15 minutes, and then add 5-6 parts by weight of carbon disulfide to obtain a yellow solution;

[0024] S2.2: Stir the yellow solution for 10-15 minutes, quickly add 4-5 parts by weight of benzyl bromide, continue stirring for 10-15 minutes, filter to obtain a precipitate, wash the precipitate 2-3 times with 40-50 parts by weight of acetone, and then add it to a rotary evaporator to remove the solvent to obtain a yellow oil;

[0025] S2.3: The yellow oil was purified by silica gel column chromatography using a petroleum ether / ethyl acetate mixture as eluent to obtain an initiator.

[0026] Furthermore, the preparation of the polycaprolactone monomer in step S3 specifically comprises the following steps:

[0027] S3.1: In a dry Schlenk reactor, add 2-3 parts by weight of ε-caprolactone, 1-2 parts by weight of an initiator, 0.05-0.1 parts by weight of 1,8-diazabicycloundec-7-ene, and 10-12 parts by weight of a tetrahydrofuran solution, and perform a "freeze-pump" cycle operation 2-3 times to obtain a reaction product;

[0028] S3.2: After stirring the reaction product, 10-20 parts by weight of methanol is added, and the mixture is filtered to obtain a solid precipitate;

[0029] S3.3: The solid precipitate is vacuum dried at 40-50° C. for 20-24 hours to obtain a polycaprolactone monomer.

[0030] Furthermore, the synthesis of the polymer in step S4 specifically comprises the following steps:

[0031] S4.1: dissolving 2-3 parts by weight of polycaprolactone monomer, 3-4 parts by weight of acrylic acid and 0.075-0.08 parts by weight of azobisisobutyronitrile in 16-20 parts by weight of dimethylformamide, and subjecting the mixture to a "freeze-evacuate" cycle operation for 2-3 times, reacting the mixture at 80-85° C. for 10-12 hours to obtain a reactant;

[0032] S4.2: Add 10-12 parts by weight of diethyl ether to the reactant, filter, and obtain a precipitated product;

[0033] S4.3: The precipitated product is dried under vacuum at 60-65°C for 20-24 hours to obtain a polymer.

[0034] Furthermore, step S5 of preparing the compound dispersant specifically comprises the following steps:

[0035] S5.1: adding 0.05-0.07 parts by weight of the copolymer to 5-6 parts by weight of the methylpyrrolidone solution to completely dissolve the copolymer to obtain a mixed solution;

[0036] S5.2: Add 1-2 parts by weight of the mixed solution and 2-3 parts by weight of the polymer to 20-30 parts by weight of distilled water, and stir for 5-15 minutes to obtain a mixture;

[0037] S5.3: Add 2-3 parts by weight of a wetting agent and 10-20 parts by weight of distilled water to the mixture, and stir for 20-30 minutes to obtain a compound dispersant.

[0038] Furthermore, in step S2.3, the volume ratio of petroleum ether / ethyl acetate is (2-3):8.

[0039] Furthermore, in step S3.2, the stirring temperature is 60-65° C., and the stirring time is 20-24 hours.

[0040] Furthermore, in step S5.2, the temperature of the distilled water is 40-60°C.

[0041] Furthermore, in step S5.3, the wetting agent is dioctyl sodium sulfosuccinate.

[0042] Compared with the prior art, the present invention has at least the following beneficial effects:

[0043] 1. The composite dispersant prepared by the present invention increases the solid content of active substances in the battery positive electrode slurry, and improves the dispersibility of solid materials in the battery positive electrode slurry. Good dispersibility leads to a decrease in slurry viscosity, and helps to improve battery performance and service life by improving the dispersion of components such as active substances and conductive agents in water.

[0044] 2. The present invention forms a structure similar to the hydrophilic and hydrophobic ends of surfactants by copolymerization of methyl methacrylate and styrene. The hydrophobic end can increase the affinity for lipophilic conductive carbon black, and the polar group at the hydrophilic end has good adsorption and surface coating properties for positive electrode materials, thereby increasing the dispersibility of the copolymer to the positive electrode slurry, thereby improving the dispersibility of the compound dispersant to the positive electrode slurry.

[0045] 3. The present invention further greatly improves the wettability of the slurry by adding sodium allyl sulfonate, which can effectively prevent agglomeration and precipitation, reduce the viscosity of the slurry, increase the solid content, and reduce the problem of cracking caused by drying, volatilization and shrinkage of a large amount of NMP solvent.

[0046] 4. The present invention prepares an initiator and adds it to the synthesis of a polymer to initiate reversible addition-fragmentation chain transfer radical polymerization of acrylic monomers, thereby synthesizing a polymer. The compound dispersant obtained by compounding the polymer can increase the stability of the positive electrode slurry and further increase the dispersibility of the dispersant to the positive electrode slurry. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0048] Figure 1 The present invention is a flow chart of the production process of a battery positive electrode slurry dispersant used in an embodiment of the present invention. DETAILED DESCRIPTION

[0049] The following is a detailed description of the production process of a battery positive electrode slurry dispersant provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternative methods to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0050] Example 1: A production process for a battery positive electrode slurry dispersant, such as Figure 1 As shown, the following steps are included:

[0051] S1: Synthesis of copolymers

[0052] S1.1: 40 parts by weight of methyl methacrylate, 50 parts by weight of styrene, 10 parts by weight of sodium allyl sulfonate and 1 part by weight of benzoyl peroxide were dissolved in 10 parts by weight of xylene, purged with high-purity nitrogen, polymerized at 98° C. for 40 minutes, and immediately added with 50 parts by weight of ethanol to stop the reaction, to obtain a precipitate;

[0053] S1.2: dissolving the precipitate in 10 parts by weight of dichloromethane, then adding 30 parts by weight of anhydrous ethanol for precipitation, and filtering and collecting the solid;

[0054] S1.3: Repeat the dissolution-precipitation process of step S1.2 twice with the obtained solid to obtain a pure copolymer, and dry the pure copolymer in a vacuum until constant weight to obtain a copolymer;

[0055] S2: Preparation of initiator

[0056] S2.1: Dissolve 5 parts by weight of potassium phosphate in 40 parts by weight of acetone to obtain a mixed solution, add 2 parts by weight of 2-mercaptoethanol to the mixed solution, stir for 10 minutes, and then add 5 parts by weight of carbon disulfide to obtain a yellow solution;

[0057] S2.2: Stir the yellow solution for 10 minutes, quickly add 4 parts by weight of benzyl bromide, continue stirring for 10 minutes, filter to obtain a precipitate, wash the precipitate twice with 40 parts by weight of acetone, and then add it to a rotary evaporator to remove the solvent to obtain a yellow oil;

[0058] S2.3: The yellow oil was purified by silica gel column chromatography using a mixture of petroleum ether / ethyl acetate (volume ratio of 1:4) as an eluent to obtain an initiator;

[0059] S3: Preparation of polycaprolactone monomer

[0060] S3.1: In a dry Schlenk reactor, 2 parts by weight of ε-caprolactone, 1 part by weight of initiator, 0.05 parts by weight of 1,8-diazabicycloundec-7-ene, and 10 parts by weight of tetrahydrofuran solution are added, and a "freeze-pump" cycle operation is performed twice to obtain a reaction product;

[0061] S3.2: The reaction product was stirred at 60° C. for 20 hours, 10 parts by weight of methanol was added, and the mixture was filtered to obtain a solid precipitate;

[0062] S3.3: drying the solid precipitate under vacuum at 40° C. for 20 hours to obtain a polycaprolactone monomer;

[0063] S4: Synthesis of polymers

[0064] S4.1: 2 parts by weight of polycaprolactone monomer, 3 parts by weight of acrylic acid and 0.075 parts by weight of azobisisobutyronitrile are dissolved in 16 parts by weight of dimethylformamide, and subjected to a "freeze-evacuate" cycle operation twice, and reacted at 80° C. for 10 hours to obtain a reactant;

[0065] S4.2: Add 10 parts by weight of diethyl ether to the reactant, filter, and obtain a precipitated product;

[0066] S4.3: drying the precipitated product under vacuum at 60° C. for 20 hours to obtain a polymer;

[0067] S5: Preparation of compound dispersant

[0068] S5.1: adding 0.05 parts by weight of the copolymer to 5 parts by weight of methyl pyrrolidone solution to completely dissolve the copolymer to obtain a mixed solution;

[0069] S5.2: Add 1 part by weight of the mixed solution and 2 parts by weight of the polymer to 20 parts by weight of distilled water at a temperature of 40° C., and stir for 5 minutes to obtain a mixture;

[0070] S5.3: Add 2 parts by weight of dioctyl sodium sulfosuccinate and 10 parts by weight of distilled water to the mixture, and stir for 20 minutes to obtain a composite dispersant.

[0071] Example 2: A production process for a battery positive electrode slurry dispersant, such as Figure 1 As shown, the following steps are included:

[0072] S1: Synthesis of copolymers

[0073] S1.1: 50 parts by weight of methyl methacrylate, 60 parts by weight of styrene, 12 parts by weight of sodium allyl sulfonate and 2 parts by weight of benzoyl peroxide were dissolved in 20 parts by weight of xylene, purged with high-purity nitrogen, polymerized at 98° C. for 40 minutes, and immediately added with 60 parts by weight of ethanol to stop the reaction, to obtain a precipitate;

[0074] S1.2: dissolving the precipitate in 20 parts by weight of dichloromethane, then adding 40 parts by weight of anhydrous ethanol for precipitation, and filtering and collecting the solid;

[0075] S1.3: Repeat the dissolution-precipitation process of step S1.2 twice with the obtained solid to obtain a pure copolymer, and dry the pure copolymer in a vacuum until constant weight to obtain a copolymer;

[0076] S2: Preparation of initiator

[0077] S2.1: 6 parts by weight of potassium phosphate are dissolved in 50 parts by weight of acetone to obtain a mixed solution, 3 parts by weight of 2-mercaptoethanol are added to the mixed solution, and after stirring for 10 minutes, 6 parts by weight of carbon disulfide are added to obtain a yellow solution;

[0078] S2.2: Stir the yellow solution for 10 minutes, quickly add 5 parts by weight of benzyl bromide, continue stirring for 10 minutes, filter to obtain a precipitate, wash the precipitate twice with 50 parts by weight of acetone, and then add it to a rotary evaporator to remove the solvent to obtain a yellow oil;

[0079] S2.3: The yellow oil was purified by silica gel column chromatography using a mixture of petroleum ether / ethyl acetate (volume ratio of 3:8) as an eluent to obtain an initiator;

[0080] S3: Preparation of polycaprolactone monomer

[0081] S3.1: In a dry Schlenk reactor, 3 parts by weight of ε-caprolactone, 2 parts by weight of initiator, 0.1 parts by weight of 1,8-diazabicycloundec-7-ene, and 12 parts by weight of tetrahydrofuran solution are added, and a "freeze-pump" cycle operation is performed twice to obtain a reaction product;

[0082] S3.2: The reaction product was stirred at 60° C. for 20 hours, 20 parts by weight of methanol was added, and filtered to obtain a solid precipitate;

[0083] S3.3: drying the solid precipitate under vacuum at 40° C. for 20 hours to obtain a polycaprolactone monomer;

[0084] S4: Synthesis of polymers

[0085] S4.1: 3 parts by weight of polycaprolactone monomer, 4 parts by weight of acrylic acid and 0.08 parts by weight of azobisisobutyronitrile are dissolved in 20 parts by weight of dimethylformamide, and subjected to a "freeze-evacuate" cycle operation twice, and reacted at 80° C. for 10 hours to obtain a reactant;

[0086] S4.2: Add 12 parts by weight of diethyl ether to the reactant, filter, and obtain a precipitated product;

[0087] S4.3: drying the precipitated product under vacuum at 60° C. for 20 hours to obtain a polymer;

[0088] S5: Preparation of compound dispersant

[0089] S5.1: adding 0.07 parts by weight of the copolymer to 6 parts by weight of a methylpyrrolidone solution to completely dissolve the copolymer to obtain a mixed solution;

[0090] S5.2: Add 2 parts by weight of the mixed solution and 3 parts by weight of the polymer to 30 parts by weight of distilled water at a temperature of 40° C. and stir for 5 minutes to obtain a mixture;

[0091] S5.3: Add 3 parts by weight of dioctyl sodium sulfosuccinate and 20 parts by weight of distilled water into the mixture, and stir for 20 minutes to obtain a composite dispersant.

[0092] Example 3: A production process for a battery positive electrode slurry dispersant, such as Figure 1 As shown, the following steps are included:

[0093] S1: Synthesis of copolymers

[0094] S1.1: 40 parts by weight of methyl methacrylate, 50 parts by weight of styrene, 10 parts by weight of sodium allyl sulfonate and 1 part by weight of benzoyl peroxide are dissolved in 10 parts by weight of xylene, purged with high-purity nitrogen, polymerized at 100° C. for 45 minutes, and immediately 50 parts by weight of ethanol are added to stop the reaction to obtain a precipitate;

[0095] S1.2: dissolving the precipitate in 10 parts by weight of dichloromethane, then adding 30 parts by weight of anhydrous ethanol for precipitation, and filtering and collecting the solid;

[0096] S1.3: Repeat the dissolution-precipitation process of step S1.2 three times with the obtained solid to obtain a pure copolymer, and dry the pure copolymer in a vacuum until constant weight to obtain a copolymer;

[0097] S2: Preparation of initiator

[0098] S2.1: Dissolve 5 parts by weight of potassium phosphate in 40 parts by weight of acetone to obtain a mixed solution, add 2 parts by weight of 2-mercaptoethanol to the mixed solution, stir for 15 minutes, and then add 5 parts by weight of carbon disulfide to obtain a yellow solution;

[0099] S2.2: Stir the yellow solution for 15 minutes, quickly add 4 parts by weight of benzyl bromide, continue stirring for 15 minutes, filter to obtain a precipitate, wash the precipitate three times with 40 parts by weight of acetone, and then add it to a rotary evaporator to remove the solvent to obtain a yellow oil;

[0100] S2.3: The yellow oil was purified by silica gel column chromatography using a mixture of petroleum ether / ethyl acetate (volume ratio of 1:4) as an eluent to obtain an initiator;

[0101] S3: Preparation of polycaprolactone monomer

[0102] S3.1: In a dry Schlenk reactor, 2 parts by weight of ε-caprolactone, 1 part by weight of initiator, 0.05 parts by weight of 1,8-diazabicycloundec-7-ene, and 10 parts by weight of tetrahydrofuran solution were added, and a "freeze-pump" cycle operation was performed 3 times to obtain a reaction product;

[0103] S3.2: The reaction product was stirred at 65° C. for 24 hours, 10 parts by weight of methanol was added, and the mixture was filtered to obtain a solid precipitate;

[0104] S3.3: drying the solid precipitate under vacuum at 50° C. for 24 hours to obtain a polycaprolactone monomer;

[0105] S4: Synthesis of polymers

[0106] S4.1: 2 parts by weight of polycaprolactone monomer, 3 parts by weight of acrylic acid and 0.075 parts by weight of azobisisobutyronitrile are dissolved in 16 parts by weight of dimethylformamide, and subjected to a "freeze-evacuate" cycle operation 3 times, and reacted at 85° C. for 10 hours to obtain a reactant;

[0107] S4.2: Add 10 parts by weight of diethyl ether to the reactant, filter, and obtain a precipitated product;

[0108] S4.3: drying the precipitated product under vacuum at 65° C. for 24 hours to obtain a polymer;

[0109] S5: Preparation of compound dispersant

[0110] S5.1: adding 0.05 parts by weight of the copolymer to 5 parts by weight of methyl pyrrolidone solution to completely dissolve the copolymer to obtain a mixed solution;

[0111] S5.2: Add 1 part by weight of the mixed solution and 2 parts by weight of the polymer to 20 parts by weight of distilled water at a temperature of 60° C., and stir for 15 minutes to obtain a mixture;

[0112] S5.3: Add 2 parts by weight of dioctyl sodium sulfosuccinate and 10 parts by weight of distilled water to the mixture, and stir for 30 minutes to obtain a composite dispersant.

[0113] Comparative Example 1

[0114] Compared with Example 1, the difference of Comparative Example 1 is that Comparative Example 1 uses the copolymer synthesized in step S1 as a dispersant, and is recorded as Comparative Example 1.

[0115] Comparative Example 2

[0116] Compared with Example 1, the difference of Comparative Example 2 is that Comparative Example 2 uses the polymer synthesized in step S4 as a dispersant, and is recorded as Comparative Example 2.

[0117] The dispersants obtained from Examples 1-3 and Comparative Examples 1-2 were used in the following manner to prepare positive electrode slurries, which were recorded as Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2, and viscosity tests were performed on them.

[0118] A method for preparing a positive electrode slurry for a lithium ion battery comprises the following steps:

[0119] S1. The formula of the positive electrode slurry for lithium-ion batteries is lithium iron phosphate: conductive carbon black SP: polyvinylidene fluoride = 96:2:2, and the amount of NMP is calculated according to the design requirement of 70% solid content;

[0120] S2. The weighed NMP is added to the dispersion tank, and the weighed polyvinylidene fluoride is gradually added and dispersed until completely dissolved to form a transparent glue solution;

[0121] S3. The weighed conductive carbon black SP is gradually added to the glue solution in portions, dispersed and stirred evenly, and then the measured lithium iron phosphate is gradually added in portions and dispersed evenly;

[0122] S4. Finally, the dispersants obtained in Example 1-3 and Comparative Example 1-2 are added at the same solid content ratio, dispersed evenly, and the corresponding positive electrode slurry is obtained.

[0123] The positive electrode slurry without dispersant prepared according to the above positive electrode slurry preparation method was tested for viscosity, and the result was recorded as Comparative Example 3.

[0124] Please refer to Table 1 for the test results.

[0125] Table 1: Viscosity comparison table of Examples 1-3 and Comparative Examples 1-3

[0126]

[0127] It can be seen from the data of the embodiment and comparative example 3 in Table 1 that the viscosity of the slurry is greatly reduced by adding the dispersant prepared in the embodiment, which proves that the dispersant prepared in the embodiment has better dispersibility for solids. Under the same solid content conditions, low viscosity slurry means improved coating efficiency. Similarly, under the same existing construction viscosity conditions, the solid content of the slurry can be increased. It can be seen from the embodiment and comparative examples 1-2 that the compounded dispersant can reduce the slurry viscosity compared with comparative examples 1-2, thereby proving that the dispersant of the embodiment has better dispersibility than comparative examples 1-2.

[0128] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A production process for a battery positive electrode slurry dispersant, characterized in that: The steps include: S1: Synthesis of copolymers The copolymer is prepared by polymerizing methyl methacrylate, styrene, sodium allyl sulfonate, benzoyl peroxide and xylene; S2: Preparation of initiator A yellow solution is prepared by using a mixed solution of potassium phosphate and acetone, 2-mercaptoethanol and carbon disulfide, and the yellow solution is added with benzyl bromide, filtered and rotary evaporated, and then purified by silica gel column chromatography to obtain an initiator; S3: Preparation of polycaprolactone monomer The polycaprolactone monomer is prepared by reacting ε-caprolactone, an initiator, 1,8-diazabicycloundec-7-ene and a tetrahydrofuran solution; S4: Synthesis of polymers The polymer is prepared by reacting polycaprolactone monomer, acrylic acid, azobisisobutyronitrile and dimethylformamide; S5: Preparation of compound dispersant The compound dispersant is obtained by compounding the polymer and the copolymer.

2. The production process of a battery positive electrode slurry dispersant according to claim 1, characterized in that: Step S1: Synthesis of copolymer, specifically comprising the following steps: S1.1: Dissolve 40-50 parts by weight of methyl methacrylate, 50-60 parts by weight of styrene, 10-12 parts by weight of sodium allyl sulfonate and 1-2 parts by weight of benzoyl peroxide in 10-20 parts by weight of xylene, purge with high-purity nitrogen, polymerize at 98-100° C. for 40-45 minutes, and immediately add 50-60 parts by weight of ethanol to stop the reaction to obtain a precipitate; S1.2: dissolving the precipitate in 10-20 parts by weight of dichloromethane, then adding 30-40 parts by weight of anhydrous ethanol for precipitation, and filtering and collecting the solid; S1.3: Repeat the dissolution-precipitation process of step S1.2 2-3 times with the obtained solid to obtain a pure copolymer, and dry the pure copolymer in a vacuum until constant weight to obtain a copolymer.

3. The production process of a battery positive electrode slurry dispersant according to claim 2, characterized in that: Step S2 is preparing an initiator, which specifically comprises the following steps: S2.1: Dissolve 5-6 parts by weight of potassium phosphate in 40-50 parts by weight of acetone to obtain a mixed solution, add 2-3 parts by weight of 2-mercaptoethanol to the mixed solution, stir for 10-15 minutes, and then add 5-6 parts by weight of carbon disulfide to obtain a yellow solution; S2.2: Stir the yellow solution for 10-15 minutes, quickly add 4-5 parts by weight of benzyl bromide, continue stirring for 10-15 minutes, filter to obtain a precipitate, wash the precipitate 2-3 times with 40-50 parts by weight of acetone, and then add it to a rotary evaporator to remove the solvent to obtain a yellow oil; S2.3: The yellow oil was purified by silica gel column chromatography using a petroleum ether / ethyl acetate mixture as eluent to obtain an initiator.

4. The production process of a battery positive electrode slurry dispersant according to claim 3, characterized in that: Step S3: Preparation of polycaprolactone monomer, specifically comprising the following steps: S3.1: In a dry Schlenk reactor, add 2-3 parts by weight of ε-caprolactone, 1-2 parts by weight of initiator, 0.05-0.1 parts by weight of 1,8-diazabicycloundec-7-ene, and 10-12 parts by weight of tetrahydrofuran solution, and perform a "freeze-pump" cycle operation 2-3 times to obtain a reaction product; S3.2: After stirring the reaction product, 10-20 parts by weight of methanol is added, and the mixture is filtered to obtain a solid precipitate; S3.3: The solid precipitate is vacuum dried at 40-50° C. for 20-24 hours to obtain a polycaprolactone monomer.

5. The production process of a battery positive electrode slurry dispersant according to claim 4, characterized in that: Step S4: Synthesis of polymer, specifically comprising the following steps: S4.1: dissolving 2-3 parts by weight of polycaprolactone monomer, 3-4 parts by weight of acrylic acid and 0.075-0.08 parts by weight of azobisisobutyronitrile in 16-20 parts by weight of dimethylformamide, and subjecting the mixture to a "freeze-evacuate" cycle operation for 2-3 times, reacting the mixture at 80-85° C. for 10-12 hours to obtain a reactant; S4.2: Add 10-12 parts by weight of diethyl ether to the reactant, filter, and obtain a precipitated product; S4.3: The precipitated product is dried under vacuum at 60-65°C for 20-24 hours to obtain a polymer.

6. The production process of a battery positive electrode slurry dispersant according to claim 5, characterized in that: Step S5: preparation of a composite dispersant, specifically comprising the following steps: S5.1: adding 0.05-0.07 parts by weight of the copolymer to 5-6 parts by weight of the methylpyrrolidone solution to completely dissolve the copolymer to obtain a mixed solution; S5.2: Add 1-2 parts by weight of the mixed solution and 2-3 parts by weight of the polymer to 20-30 parts by weight of distilled water, and stir for 5-15 minutes to obtain a mixture; S5.3: Add 2-3 parts by weight of a wetting agent and 10-20 parts by weight of distilled water to the mixture, and stir for 20-30 minutes to obtain a compound dispersant.

7. The production process of a battery positive electrode slurry dispersant according to claim 3, characterized in that: In step S2.3, the volume ratio of petroleum ether / ethyl acetate is (2-3):

8.

8. The production process of a battery positive electrode slurry dispersant according to claim 4, characterized in that: In step S3.2, the stirring temperature is 60-65° C. and the stirring time is 20-24 hours.

9. The production process of a battery positive electrode slurry dispersant according to claim 6, characterized in that: The temperature of distilled water in step S5.2 is 40-60°C.

10. The production process of a battery positive electrode slurry dispersant according to claim 6, characterized in that: In step S5.3, the wetting agent is dioctyl sodium sulfosuccinate.