Battery coating and preparation method thereof

By using amorphous calcium carbonate and magnesium-doped low-cost lithium-ion battery separator coatings, the problem of performance degradation of traditional separators at high temperatures is solved, high-temperature stability and low-cost separator materials are achieved, and battery safety is improved. and cycle performance.

CN118712653APending Publication Date: 2024-09-27HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410928320.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Traditional lithium-ion battery separators are prone to shrinkage and reduced mechanical properties in high-temperature environments, and are difficult to meet the energy density and power density requirements of high-performance batteries. Moreover, ceramic coatings have high production costs, increased weight, and greater environmental hazards.

Method used

Amorphous calcium carbonate is used as the separator coating material, and magnesium is doped as a stabilizer. A low-cost and environmentally friendly lithium-ion battery separator coating is prepared through a simple process. The coating is composed of 20-50 nanoparticles and has a thickness of 0.5um-2um. , with excellent high temperature stability and thermal conductivity.

Benefits of technology

It significantly improves the safety and cycle performance of lithium-ion batteries, reduces manufacturing costs, avoids the weight increase and environmental hazards of ceramic coatings, and provides a low-cost, environmentally friendly separator solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_6
    Figure FT_6
  • Figure FT_2
    Figure FT_2
Patent Text Reader

Abstract

The invention discloses a battery coating and a preparation method thereof. The battery coating is composed of amorphous calcium carbonate, the amorphous calcium carbonate is doped with magnesium as an inorganic stabilizer, and the molar ratio of calcium to magnesium is 1-0.5. The preparation method comprises the following steps: (1) mixing a calcium salt solution or a mixed solution of calcium salt and magnesium salt with a carbonate solution, stirring for a certain time, then centrifugally collecting precipitates, washing the precipitates, and dispersing the precipitates in an alcohol-water solution to obtain an amorphous calcium carbonate dispersion liquid; and (2) coating the amorphous calcium carbonate dispersion liquid on the surface of a base membrane, and drying to form the membrane. Amorphous calcium carbonate is simple to synthesize and low in cost. Meanwhile, the chemical stability is good, and the cycle performance of the battery is facilitated; heat stability is good, and heat shrinkage is avoided; the mechanical property is excellent, and potential safety hazards caused by the fact that lithium dendrites penetrate through the diaphragm and the like are avoided. In conclusion, the amorphous calcium carbonate is a preferable material of a low-cost, non-toxic and harmless environment-friendly lithium ion battery diaphragm coating material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion battery materials, and in particular relates to a battery coating and a preparation method thereof. Background Art

[0002] In the field of lithium-ion battery technology, the separator plays a vital role as the key insulating layer between the positive and negative electrodes of the battery. It not only needs to effectively isolate the positive and negative electrodes to prevent short circuits, but also has to have good ion conductivity to ensure the efficiency of charge transfer inside the battery. With the widespread application of lithium-ion batteries in electric vehicles, portable electronic devices and other fields, the performance requirements for separators are also increasing. Although traditional polymer separators have certain ion conductivity and mechanical strength, they are prone to shrinkage and decreased mechanical properties under high temperature environments, resulting in battery performance degradation and even safety accidents. In addition, the pore size distribution and thickness of these separators are also difficult to meet the energy density and power density requirements of high-performance batteries.

[0003] To solve these problems, researchers began to explore new diaphragm materials and coating technologies. Among them, ceramic coated diaphragms have attracted attention due to their high temperature stability and excellent thermal conductivity. Ceramic coatings can form a protective layer on the polymer substrate, which can not only enhance the thermal stability of the diaphragm, but also maintain good ion conductivity. However, the manufacture of diaphragm ceramic coatings requires complex processes and high-purity raw materials, and the production cost is high; ceramic materials are usually heavier than polymers, so adding ceramic coatings to the diaphragm will increase the overall weight of the battery; moreover, during the production and recycling of ceramics, there will be heavy metals and chemical materials that cause harm to the environment. And the uniformity and adhesion of the coating need to be further optimized.

[0004] Therefore, the development of a low-cost and environmentally friendly lithium-ion battery separator material is of great significance to promote the sustainable development of electric vehicles and renewable energy storage technology. Summary of the invention

[0005] In view of the differences existing in the prior art, the present invention aims to provide a new type of lithium-ion battery separator coating material.

[0006] The above-mentioned object of the present invention is achieved by the following technical solutions: In a first aspect, the present invention provides a low-cost, environmentally friendly lithium-ion battery separator coating.

[0007] The low-cost and environment-friendly lithium-ion battery separator coating provided by the present invention is composed of amorphous calcium carbonate.

[0008] Furthermore, the amorphous calcium carbonate particles have a size of 20-50 nanometers.

[0009] Furthermore, the amorphous calcium carbonate is doped with magnesium as an inorganic stabilizer, and further, the molar ratio of calcium to magnesium in the amorphous calcium carbonate is 1-0.5.

[0010] Furthermore, the thickness of the lithium-ion battery separator coating may be 0.5um-2um.

[0011] Amorphous calcium carbonate is easy to synthesize, inexpensive, and has excellent mechanical properties and insulation properties. When used as a lithium-ion battery separator coating, the resulting coating separator not only has excellent high-temperature stability and thermal conductivity, but also reduces manufacturing costs while maintaining good ion conductivity. The technical solution of the present invention can significantly improve the safety and cycle performance of lithium-ion batteries, providing strong support for the further development of battery technology.

[0012] In a second aspect, the present invention provides a method for preparing the above-mentioned low-cost and environmentally friendly lithium-ion battery separator coating.

[0013] The method for preparing a low-cost, environmentally friendly lithium-ion battery separator coating provided by the present invention comprises the following steps: (1) mixing a calcium salt aqueous solution or a mixed aqueous solution of a calcium salt and a magnesium salt with a carbonate aqueous solution, stirring for a certain period of time, then collecting a precipitate by centrifugation, washing the precipitate and dispersing it in an alcohol aqueous solution to obtain an amorphous calcium carbonate dispersion; (2) coating the amorphous calcium carbonate dispersion on at least one side of the base film, and placing the base film coated with the amorphous calcium carbonate coating in a constant temperature and humidity chamber (10-20° C., relative humidity 30%-40%) to dry the base film.

[0014] In step (1) of the above method, the calcium salt is selected from at least one of calcium chloride and calcium nitrate; the magnesium salt is selected from at least one of magnesium chloride and magnesium nitrate; and the carbonate is selected from at least one of sodium carbonate and potassium carbonate.

[0015] In step (1) of the above method, the stirring time may be 0.5-5 minutes, specifically 5 minutes.

[0016] The operation of step (1) of the above method is carried out at 25°C-30°C.

[0017] In step (1) of the above method, the molar ratio of the calcium salt to the magnesium salt is 1-0.5, and the molar ratio of the calcium salt to the carbonate is 0.5-1.

[0018] In step (1) of the above method, the washing is performed by washing with anhydrous ethanol multiple times.

[0019] In step (1) of the above method, in the alcohol aqueous solution, the volume ratio of alcohol to water is 0.5-2, preferably the volume ratio of alcohol to water is 1. Furthermore, the alcohol may be ethanol.

[0020] In step (1) of the above method, the solid content of the amorphous calcium carbonate dispersion is 30%-40%.

[0021] In step (2) of the above method, the base film may be a polypropylene film.

[0022] In step (2) of the above method, the coating amount of the base film on one side is 0.5-2.5 ml of dispersion liquid / square centimeter.

[0023] In step (2) of the above method, the coating method can be spray coating or spin coating.

[0024] Furthermore, the spray coating machine equipment parameters used in the spray coating method are: the nozzle diameter of the spray gun is 50um, and the pressure is 0.3-0.8MPa; the spin coating machine equipment parameters used in the spin coating method are: first-stage rotation speed (1000-2000rpm), acceleration time (30s), and spin coating time (60s); second-stage rotation speed (2500-3500rpm), acceleration time (10s), and spin coating time (10s); the purpose of the second-stage acceleration is to remove excess amorphous calcium carbonate dispersion.

[0025] In a third aspect, the present invention provides a low-cost, environmentally friendly lithium-ion battery separator.

[0026] The low-cost and environment-friendly lithium-ion battery separator provided by the present invention comprises a base film and a separator coating composed of amorphous calcium carbonate as described in the first aspect of the present invention and coated on the surface of the base film.

[0027] Furthermore, the base film may be a polypropylene film.

[0028] In a fourth aspect, the present invention provides a lithium-ion battery.

[0029] The lithium-ion battery provided by the present invention comprises the battery separator described in the third aspect of the present invention.

[0030] In a fifth aspect, the present invention also provides the use of amorphous calcium carbonate or magnesium-doped amorphous calcium carbonate in the preparation of lithium-ion battery separator coatings.

[0031] The present invention has the following beneficial effects: As a kind of inorganic mineral, amorphous calcium carbonate is easy to synthesize and has low cost. At the same time, calcium carbonate is not easy to react with electrolyte components, has good chemical stability, and is beneficial to the cycle performance of the battery; the decomposition temperature is above 500 degrees, which is much higher than the thermal runaway temperature of lithium-ion batteries, has good thermal stability, and does not shrink when heated; it has excellent mechanical properties, can effectively improve the mechanical strength of the diaphragm, and avoid safety hazards such as lithium dendrites penetrating the diaphragm. In summary, amorphous calcium carbonate is a preferred low-cost, non-toxic, harmless, and environmentally friendly lithium-ion battery diaphragm coating material. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention is a flow chart of the preparation of the lithium ion battery separator; Figure 2 A scanning electron micrograph of the amorphous calcium carbonate prepared in Example 1; Figure 3 This is a scanning electron microscopic image of the coating surface after drying when the alcohol-water ratio is 0.5 in Example 3; Figure 4 This is a scanning electron microscopic image of the surface of the diaphragm coating after spraying amorphous calcium carbonate in Example 1; Figure 5 is a scanning electron microscopic image of the surface of the diaphragm coating after spin coating of amorphous calcium carbonate in Example 4; Figure 6 The graph is a comparison of the cycle performance of the battery assembled with the diaphragm base film and the diaphragm prepared in Example 1. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0034] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0035] Example 1: A method for preparing amorphous calcium carbonate as a lithium-ion battery separator coating material Synthetic amorphous calcium carbonate: Mix 10mL 0.1 mol / L calcium chloride solution and 2mL 0.5 mol / L magnesium chloride solution with 10mL 0.1 mol / L sodium carbonate solution, stir for 5 minutes, collect the precipitate by centrifugation, wash it with anhydrous ethanol for several times, and disperse the washed precipitate in an alcohol-water solution (ethanol / water = 1:1, v / v) to obtain an amorphous calcium carbonate dispersion with a solid content of 5%-30%. The solid content in the experiment was specifically 10%. Figure 1 Scanning electron microscopy images of the amorphous calcium carbonate showed that the particle size was about 20-50 nm.

[0036] Preparation of diaphragm coating: Spin or spray the amorphous calcium carbonate dispersion onto the surface of the diaphragm base film (polypropylene film), with a single-sided coating amount of 0.5-2.5 ml of dispersion per square centimeter (the specific experiment coating amount is 1 ml per square centimeter) The parameters of the spraying machine equipment are: the nozzle diameter of the spray gun is 50um, and the pressure is 0.3-0.8MPa; the spin coating setting parameters are: the first stage speed (1000-2000rpm), acceleration time (30s), spin coating time (60s); the second stage speed (2500-3500rpm), acceleration time (10s), spin coating time (10s); the spray coating setting parameters are: the nozzle diameter of the spray gun is 50um, and the pressure is 0.3-0.8MPa; finally, it is placed in a constant temperature and constant box for drying and film formation, and the coating thickness is 0.5um-2um. The spray coating method is used in Examples 1-3. Figure 3 The scanning electron micrograph in the figure shows that after spraying and drying, the amorphous calcium carbonate alcohol water dispersion forms a uniform film attached to the surface of the diaphragm base film, covering it completely.

[0037] Example 2: A method for preparing amorphous calcium carbonate as a lithium-ion battery separator coating material The preparation method is basically the same as that in Example 1, except that when synthesizing amorphous calcium carbonate, the alcohol-water ratio of the alcohol-water solution used is 2.

[0038] Example 3: A method for preparing amorphous calcium carbonate as a lithium-ion battery separator coating material The preparation method is basically the same as that of Example 1, except that when synthesizing amorphous calcium carbonate, the alcohol-water ratio of the alcohol-water solution used is 0.5. Figure 3 The scanning electron microscopic image shows that micron-sized crystalline calcium carbonate cubes are distributed on the surface of the base film, indicating that when the water content in the dispersion is high, amorphous calcium carbonate will crystallize to form micron-sized cubes, which cannot form a good diaphragm coating.

[0039] Example 4: A method for preparing amorphous calcium carbonate as a lithium-ion battery separator coating material The preparation method is basically the same as Example 1, except that: the coating method is spin coating; the parameters of the spin coating machine are: the first stage speed (1000-2000rpm), the specific speed is 1500rpm, the acceleration time (30s), the spin coating time (60s); the second stage speed (2500-3500rpm), the specific speed is 3000rpm, the acceleration time (10s), the spin coating time (10s); the purpose of the second stage acceleration is to remove excess amorphous calcium carbonate dispersion. Figure 5 The scanning electron microscopy image in the figure shows that the amorphous calcium carbonate does not completely cover the surface of the base film after spin coating, and the film-forming effect needs to be optimized.

[0040] In Example 2, the alcohol-water ratio is 2, the anhydrous ethanol content is high, and the evaporation is too fast during drying, which is not easy to form a film; in Example 3, the alcohol-water ratio is 0.5, and the water content is high, which will cause the amorphous calcium carbonate to undergo crystallization transformation, and the crystals will form cubic blocks with a size of micrometers, such as Figure 3 As shown, it cracks after drying and particles fall off.

[0041] Example 4 Spin coating film, the uniformity of the film surface needs to be improved, such as Figure 5 As shown, part of the base film surface is not covered with the coating, and the local mechanical and thermal stability are uneven, which will affect the battery cycle life and safety; the spray coating of Example 1 has better film forming properties and a smooth and uniform surface, such as Figure 4 shown.

[0042] The membrane-assembled lithium iron phosphate / graphite button lithium ion battery prepared in Example 1 was used as a comparison group. The same electrode surface density, electrolyte composition and other chemical systems, as well as the same assembly method and cycle test method were ensured. The button lithium ion battery was assembled using a diaphragm polypropylene-based membrane. The cycle comparison data for the first 20 cycles are as follows: Figure 6 As shown, the charge and discharge efficiency of the battery with a calcium carbonate coating is significantly higher than that of the battery assembled with a polypropylene-based membrane.

[0043] Based on the above embodiments, the most preferred alcohol-water ratio is 1, and spraying film formation can form a dense and uniform amorphous calcium carbonate coating on the surface of the polypropylene base film, which can significantly improve the safety and cycle performance of the battery, and is of great significance for promoting the sustainable development of electric vehicles and renewable energy storage technology.

[0044] The present invention has been described in detail above. It will be apparent to those skilled in the art that the present invention may be implemented in a wide range under equivalent parameters, concentrations and conditions without departing from the spirit and scope of the present invention and without the need for unnecessary experimentation. Although the present invention provides specific embodiments, it should be understood that further improvements may be made to the present invention. In short, according to the principles of the present invention, this application intends to include any changes, uses or improvements to the present invention, including changes made by conventional techniques known in the art that depart from the scope disclosed in this application. Applications of some of the basic features may be made within the scope of the following appended claims.

Claims

1. A lithium-ion battery separator coating composed of amorphous calcium carbonate.

2. The lithium ion battery separator coating according to claim 1, Features: The amorphous calcium carbonate particles have a size of 20-50 nanometers; And / or, the amorphous calcium carbonate is doped with magnesium as an inorganic stabilizer, and the molar ratio of calcium to magnesium in the amorphous calcium carbonate is 1-0.5; And / or, the thickness of the lithium-ion battery separator coating is 0.5um-2um.

3. The method for preparing the lithium ion battery separator coating according to claim 1 or 2, comprising the following steps: (1) mixing a calcium salt aqueous solution or a mixed aqueous solution of a calcium salt and a magnesium salt with a carbonate aqueous solution, stirring for a certain period of time, then collecting a precipitate by centrifugation, washing the precipitate and dispersing it in an alcohol aqueous solution to obtain an amorphous calcium carbonate dispersion; (2) coating the amorphous calcium carbonate dispersion on at least one side of the base film and drying it to form a film.

4. The preparation method according to claim 3, Features: In the step (1), the calcium salt is selected from at least one of calcium chloride and calcium nitrate; the magnesium salt is selected from at least one of magnesium chloride and magnesium nitrate; and the carbonate is selected from at least one of sodium carbonate and potassium carbonate.

5. The preparation method according to claim 3 or 4, Features: In the step (1), the stirring time is 0.5-5 minutes; And / or, the operation of step (1) is carried out at 25°C-30°C; And / or, in step (1), the molar ratio of the calcium salt to the magnesium salt is 1-0.5, and the molar ratio of the calcium salt to the carbonate is 0.5-1; And / or, in the step (1), the washing is performed multiple times with anhydrous ethanol.

6. The preparation method according to any one of claims 3 to 5, Features: In the step (1), the volume ratio of alcohol to water in the alcohol aqueous solution is 0.5-2, preferably the volume ratio of alcohol to water is 1; And / or, in step (1), the solid content of the amorphous calcium carbonate dispersion is 30%-40%.

7. The preparation method according to any one of claims 3 to 6, Features: In the step (2), the base film is a polypropylene film; And / or, in step (2), the coating amount on one side of the base film is 0.5-2.5 ml of dispersion liquid / cm2; And / or, in the step (2), the coating method is spray coating or spin coating; Furthermore, the spray coating machine equipment parameters used in the spray coating method are: the nozzle diameter of the spray gun is 50um, and the pressure is 0.3-0.8MPa; the spin coating machine equipment parameters used in the spin coating method are: the first stage rotation speed is 1000-2000rpm, the acceleration time is 30s, and the spin coating time is 60s; the second stage rotation speed is 2500-3500rpm, the acceleration time is 10s, and the spin coating time is 10s.

8. A lithium-ion battery separator, comprising a base film and the separator coating according to claim 1 or 2 coated on the surface of the base film.

9. A lithium ion battery comprising the lithium ion battery separator according to claim 8.

10. Use of amorphous calcium carbonate or magnesium-doped amorphous calcium carbonate in the preparation of lithium-ion battery separator coating; preferably, the molar ratio of calcium to magnesium in the magnesium-doped amorphous calcium carbonate is 1-0.5.

Citation Information

Cited By

  • Method and device for removing calcium ions in high-salinity wastewater by using electron beams and application of method and device

    CN120504418A

  • Calcium carbonate-based inorganic battery diaphragm and preparation method thereof

    CN121601954A