Acrylic acid-based hard tissue adhesive and preparation method thereof
By using bioabsorbable polymer microparticle pore-forming agents in acrylic-based hard tissue adhesives, an in-situ spatiotemporally controllable porous structure is formed, which solves the problems of poor osseointegration ability and high Young's modulus in the existing technology. It achieves mechanical properties and bone regeneration promotion effects that match cancellous bone.
Patent Information
- Application Number
- CN202410807369.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
Existing acrylic-based hard tissue adhesives have poor osseointegration capabilities and have a higher Young's modulus than cancellous bone, which easily causes fractures after implantation. Moreover, it is difficult to form a spatiotemporally controllable porous structure in situ with existing technology, and cannot Effectively promotes the rapid growth of endogenous cells and new bone.
It uses a hard tissue adhesive matrix composed of polymerizable monomers, polymer powders and polymerization initiators, combined with bioabsorbable polymer particulate pore-forming agents, and adjusts the degradation rate through light-initiated cross-linking to form an in-situ spatiotemporally controllable Porous structure, reduces Young's modulus and promotes bone regeneration.
The mechanical properties of the hard tissue adhesive are matched with the cancellous bone, forming a spatiotemporally controllable porous structure in situ, promoting the rapid growth of endogenous cells and new bone, and improving the osseointegration effect.
Smart Images

Figure CN118718072A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to medical materials, in particular to an acrylic acid-based hard tissue adhesive having an in-situ generated time-space controllable porous structure and a preparation method thereof. Background Art
[0002] Polymer-based hard tissue adhesives have been used in orthopedic / dental fields for more than 70 years, including fracture fixation, cone plasty, bone defect filling, and bone tumor treatment. Among them, acrylic-based hard tissue adhesives (such as polymethyl methacrylate (PMMA) bone cement) are the most widely used polymer-based hard tissue adhesives due to their excellent mechanical properties and shape plasticity, stable chemical structure, and acceptable biosafety. However, long-term clinical applications have also revealed that acrylic-based bone cement has poor bone integration ability, and its Young's modulus is much higher than that of cancellous bone, which is prone to cause fractures around implants.
[0003] The prior art uses a method combining freeze drying and free radical polymerization to prepare a composite material composed of water-soluble chitosan oligosaccharides (CSO) and PMMA. After immersion in water, CSO gradually dissolves from the composite material to obtain a porous PMMA with an appropriate compression modulus. However, this type of template method requires in vitro preforming, and the porous PMMA after forming does not have tissue adhesion and is difficult to fill irregular hard tissue defects, especially for cone plasty.
[0004] There is also a method of mixing PMMA bone cement with oxidized hyaluronic acid-carboxymethyl chitosan in situ cross-linked hydrogel to obtain PMMA / hydrogel hybrid cement. Compared with pure PMMA cement, PMMA / hydrogel hybrid cement exhibits a lower solidification temperature and elastic modulus, and a porous structure is obtained due to the degradation of the hydrogel. However, this method of directly mixing PMMA with degradable hydrogel can only obtain irregular pores that are uncontrollable in time and space, and the pore size of the pores cannot be controlled. In addition, the degradation of the degradable hydrogel takes time. Literature data show that PMMA / hydrogel hybrid cement will not appear until micropores appear after 14 days of in vitro degradation, which is not conducive to the rapid growth of endogenous cells.
[0005] Inorganic calcium salt particles coated with glutaraldehyde-crosslinked gelatin are also used as fillers and pore-forming agents for PMMA bone cement. The controllable particle size of the particles is conducive to the formation of a uniform microporous structure and promotes cell growth in the micropores. However, this type of particle leaching method can only obtain a spatially controllable pore structure, and because the degradation time of glutaraldehyde-crosslinked gelatin is long, it cannot form pores immediately at the initial stage of implantation, that is, it is difficult to control the time for the formation of micropores, which is not conducive to the initial endogenous cell growth and bone integration.
[0006] Therefore, there is an urgent need in the art for a hard tissue adhesive that can form a porous structure with controllable time and space in situ after bonding hard tissue, so as to achieve bone integration and rapid ingrowth of endogenous cells / new bone. Summary of the invention
[0007] The technical problem to be solved by the present invention is to provide an acrylic acid-based hard tissue adhesive and a preparation method thereof in view of the above-mentioned defects of the prior art.
[0008] In order to achieve the above object, the present invention provides an acrylic-based hard tissue adhesive, wherein the adhesive has an in-situ generated and spatiotemporally controllable porous structure, comprising:
[0009] A hard tissue adhesive matrix, comprising a polymerizable monomer, a polymer powder and a polymerization initiator, wherein the polymerizable monomer is polymerized into a polymer under the action of the polymerization initiator; and
[0010] The bioabsorbable polymer microparticle pore-forming agent is mixed in the hard tissue adhesive matrix and can adjust the degradation rate.
[0011] The above-mentioned acrylic-based hard tissue adhesive, wherein the polymerizable monomer is methacrylate, or a combination of methacrylate and a polymerizable monomer containing an acidic group;
[0012] The polymer powder is at least one selected from homopolymers of alkyl methacrylates, copolymers of alkyl methacrylates, copolymers of alkyl methacrylates and other polymerizable monomers, copolymers of alkyl methacrylates and alkylenedimethacrylates, and copolymers of alkyl methacrylates and diene monomers;
[0013] The polymerization initiator is dibenzoyl peroxide, tributyl boron or a partial oxide of tributyl boron.
[0014] The acrylic acid-based hard tissue adhesive mentioned above, wherein in the hard tissue adhesive matrix, the mass percentage of the polymerizable monomer is 20%-70%, the mass percentage of the polymer powder is 20%-70%, and the mass percentage of the polymerization initiator is 1%-20%.
[0015] The above-mentioned acrylic acid-based hard tissue adhesive, wherein the bioabsorbable polymer microparticle pore-forming agent comprises a soluble polymer, a biodegradable polymer and a photoinitiator, and the degradation rate is adjusted by adjusting the ratio of the soluble polymer and the biodegradable polymer;
[0016] The soluble polymer includes at least one of gelatin, alginic acid, hyaluronic acid, silk fibroin chitosan and carboxymethyl chitosan;
[0017] The biodegradable polymer comprises at least one of methacrylated gelatin, methacrylated alginic acid, methacrylated hyaluronic acid, methacrylated silk fibroin and methacrylated chitosan;
[0018] The photoinitiator is used for photocrosslinking of biodegradable polymers, including 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L) or lithium phenyl (2,4,6-trimethylbenzoyl) phosphate (LAP).
[0019] The above-mentioned acrylic acid-based hard tissue adhesive, wherein the bioabsorbable polymer microparticle pore-forming agent is prepared by mechanical crushing, emulsion stirring, electrostatic spraying, 3D printing or microfluidics; wherein the mass ratio of the soluble polymer to the biodegradable polymer is 1:10-10:1; and the mass ratio of the biodegradable polymer to the photoinitiator is 10:1-100:1.
[0020] The acrylic acid-based hard tissue adhesive mentioned above, wherein the average particle size of the bioabsorbable polymer microparticle pore-forming agent is 1-1000 μm; the soluble polymer completely dissolves within 72 hours, and the biodegradable polymer completely degrades within 3 months.
[0021] In order to better achieve the above-mentioned object, the present invention also provides a method for preparing an acrylic-based hard tissue adhesive, which comprises the following steps:
[0022] S100, preparing double network gel microparticles composed of soluble polymers and biodegradable polymers by mechanical crushing, emulsion stirring, electrostatic jetting, 3D printing or microfluidics, and cross-linking the biodegradable polymer network by photoinitiation to obtain a bioabsorbable polymer microparticle pore-forming agent with adjustable degradation rate;
[0023] S200, respectively weighing the components of the hard tissue adhesive matrix, including polymerizable monomers, polymer powder and polymerization initiator; and
[0024] S300, mixing the polymerizable monomer, polymer powder and polymerization initiator with the bioabsorbable polymer microparticle pore-forming agent to form a mixture, wherein the volume ratio of the hard tissue adhesive matrix to the bioabsorbable polymer microparticle pore-forming agent is 1:2-10:1.
[0025] The preparation method of the above-mentioned acrylic acid-based hard tissue adhesive, wherein the polymerizable monomer, polymer powder and polymerization initiator are mixed with the bioabsorbable polymer microparticle pore-forming agent to obtain an injectable slurry, and the slurry is injected by a syringe, applied by a brush or directly filled and implanted; the curing time of the injectable slurry after implantation is 1-20 minutes.
[0026] The preparation method of the above-mentioned acrylic-based hard tissue adhesive, wherein, after implantation, a spatiotemporally controllable porous structure is formed in situ in the acrylic-based hard tissue adhesive; the formation time of the porous structure is controlled by adjusting the type and mass ratio of the soluble polymer to the biodegradable polymer; the pore size of the porous structure is controlled by adjusting the particle size of the bioabsorbable polymer microparticle pore-forming agent; the porosity of the porous structure is controlled by adjusting the particle volume ratio of the hard tissue adhesive matrix to the bioabsorbable polymer microporogen.
[0027] The preparation method of the acrylic acid-based hard tissue adhesive, wherein the formation time of the porous structure is 24 hours to 3 months; the pore size of the porous structure is 1-1000 μm; the porosity of the porous structure is 10%-66.7%.
[0028] The technical effects of the present invention are:
[0029] The present invention combines soluble polymers and biodegradable polymers to prepare bioabsorbable polymer microparticles with adjustable degradation rate. As a pore-forming agent, the microparticles can be injected into the defect site in the body together with an acrylic acid-based hard tissue adhesive to reduce the Young's modulus of the acrylic acid-based hard tissue adhesive, and as the tissue regenerates, the polymer microparticles gradually dissolve / degrade and are absorbed by the body to make way for the regenerated tissue. By selecting different soluble polymers and biodegradable polymers and changing their ratio, the degradation behavior of the polymer microparticles is regulated, wherein the soluble polymer dissolves rapidly after implantation in the body, providing space for the rapid migration of endogenous cells into the adhesive; the biodegradable polymer can stably exist in the early stage of implantation, provide adhesion sites for cells migrating into the adhesive, and gradually degrade with tissue regeneration, and finally be absorbed by the body to make way for the new tissue, thereby achieving bone regeneration and three-dimensional bone integration inside the hard tissue adhesive.
[0030] In addition, the acrylic-based hard tissue adhesive of the present invention that generates in situ spatiotemporally controllable pore structures has multiple design capabilities. In practical applications, the appropriate types and proportions of soluble polymers and biodegradable polymers, as well as appropriate additives, can be selected according to the requirements of tissue regeneration rate to achieve the best defect repair effect.
[0031] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but is not intended to limit the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figures 1A-1C They are optical microscope images of GG-11-100, GG-11-200, and GG-11-400 droplets prepared by microfluidic technology in Example 1 of the present invention, respectively;
[0033] Figure 2A The spatiotemporal dynamic curves of the pores after PMMA-GG-11-100-M, PMMA-GG-11-200-M, and PMMA-GG-11-400-M in Example 5 of the present invention are immersed in the phosphate buffer solution in Example 8;
[0034] Figure 2B Spatiotemporal dynamic curves were generated for the pores of PMMA-GG-11-100-M, PMMA-GG-11-200-M, and PMMA-GG-11-400-M in Example 5 of the present invention after being immersed in the collagenase solution in Example 8;
[0035] Figure 2C Spatiotemporal dynamic curves were generated for the pores of PMMA-GG-11-200-L, PMMA-GG-11-200-M, and PMMA-GG-11-200-H in Examples 4-6 of the present invention after being immersed in the collagenase solution in Example 8;
[0036] Figure 3A This is a scanning electron microscope image of the pore structure of PMMA-GG-11-200-L in Example 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours;
[0037] Figure 3B This is a scanning electron microscope image of the pore structure of PMMA-GG-11-200-H in Example 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours;
[0038] Figure 3C This is a scanning electron microscope image of the pore structure of PMMA-GG-11-400-H in Example 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours;
[0039] Figure 4 The shear adhesion strength of PMMA-GG-11-200-M in Example 5 of the present invention and PMMA-N in Comparative Example 1 to fresh pig bones;
[0040] Figure 5A This is a micro-CT image of the rat skull defect in Example 10 repaired with PMMA-N in Comparative Example 1 of the present invention 8 weeks later;
[0041] Figure 5BThis is a micro-CT image of the rat skull defect repaired by PMMA-GG-11-200-M in Example 5 of the present invention 8 weeks after the repair. DETAILED DESCRIPTION
[0042] The structural principle and working principle of the present invention are described in detail below in conjunction with the accompanying drawings:
[0043] In this specification, the word "may" includes both the meaning of carrying out a certain treatment and the meaning of not carrying out a certain treatment. Unless otherwise specified, the degree of methacrylate esterification of methacrylated gelatin and methacrylated chitosan is 50%.
[0044] In view of the problem that the mechanical properties of acrylic-based hard tissue adhesives in the prior art do not match those of cancellous bone, and the lack of porous structure hinders the growth of endogenous cells and new bone, the present invention provides an acrylic-based hard tissue adhesive with an in-situ generated time-space controllable porous structure. The porous structure of the porous acrylic-based hard tissue adhesive with appropriate porosity can reduce its Young's modulus, so that its mechanical properties match those of cancellous bone, and at the same time provide space for new bone growth, so as to achieve bone integration in three-dimensional space rather than the two-dimensional surface of non-porous block adhesives. Among them, the "time" in the time-space controllable pore structure means that the time of in-situ generation of pores in the acrylic-based hard tissue adhesive is controllable, which can match the time of tissue regeneration; the "space" in the time-space controllable pore structure means that the pore size and porosity of the in-situ generated pores in the acrylic-based hard tissue adhesive are controllable, which can promote the growth of new blood vessels and new bone.
[0045] Different from the degradable gel particles or polyester particles commonly used in pore-making technology, the present invention combines soluble polymers and biodegradable polymers to prepare bioabsorbable polymer particles with adjustable degradation rate. As pore-making agents, they can be injected into the defect site in the body together with acrylic hard tissue adhesives to reduce the Young's modulus of acrylic hard tissue adhesives, and as the tissue regenerates, the polymer particles gradually dissolve / degrade and are absorbed by the body to make way for the regenerated tissue. By selecting different soluble polymers and biodegradable polymers and changing their ratio, the degradation behavior of the polymer particles can be regulated, wherein the soluble polymer quickly dissolves after implantation in the body, providing space for the rapid migration of endogenous cells into the adhesive; the biodegradable polymer can stably exist in the early stage of implantation, provide adhesion sites for cells migrating into the adhesive, and gradually degrade with tissue regeneration, and finally be absorbed by the body to make way for the new tissue, thereby achieving bone regeneration and three-dimensional bone integration inside the hard tissue adhesive.
[0046] The acrylic acid-based hard tissue adhesive of the present invention has an in-situ generated and spatiotemporally controllable porous structure, comprising: a hard tissue adhesive matrix, comprising a polymerizable monomer, a polymer powder and a polymerization initiator, wherein the polymerizable monomer is polymerized into a polymer under the action of the polymerization initiator; and a bioabsorbable polymer microparticle pore-forming agent, which is mixed in the hard tissue adhesive matrix and has an adjustable degradation rate. Among them, the polymerizable monomer is methacrylate, or a combination of methacrylate and a polymerizable monomer containing an acidic group; the polymer powder is at least one selected from homopolymers of alkyl methacrylates, copolymers between alkyl methacrylates, copolymers of alkyl methacrylates and other polymerizable monomers, copolymers of alkyl methacrylates and alkylenedimethacrylates, and copolymers of alkyl methacrylates and diene monomers; the polymerization initiator is dibenzoyl peroxide, tributyl boron or a partial oxide of tributyl boron. In the hard tissue adhesive matrix, the mass percentage of the polymerizable monomer is 20%-70%, the mass percentage of the polymer powder is 20%-70%, and the mass percentage of the polymerization initiator is 1%-20%.
[0047] The bioabsorbable polymer microparticles of the bioabsorbable polymer microparticle pore-forming agent include soluble polymers, biodegradable polymers and photoinitiators, and the degradation rate can be adjusted by adjusting the ratio of the soluble polymers and the biodegradable polymers; the soluble polymers include at least one of gelatin, alginate, hyaluronic acid, silk fibroin chitosan and carboxymethyl chitosan; the biodegradable polymers include at least one of methacrylated gelatin, methacrylated alginate, methacrylated hyaluronic acid, methacrylated silk fibroin and methacrylated chitosan; the photoinitiator is used for photocrosslinking of the biodegradable polymers, including 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L) or phenyl(2,4,6-trimethylbenzoyl)lithium phosphate (LAP).
[0048] In this embodiment, the polymer microparticles of the bioabsorbable polymer microparticle pore-forming agent can be prepared by mechanical crushing, emulsion stirring, electrostatic spraying, 3D printing or microfluidics; wherein the mass ratio of the soluble polymer to the biodegradable polymer is 1:10-10:1; the mass ratio of the biodegradable polymer to the photoinitiator is 10:1-100:1. The average particle size of the bioabsorbable polymer microparticle pore-forming agent is 1-1000 μm; the soluble polymer is completely dissolved within 72 hours, and the biodegradable polymer is completely degraded within 3 months.
[0049] The method for preparing the acrylic acid-based hard tissue adhesive of the present invention comprises the following steps:
[0050] Step S100, preparing double-network gel microparticles composed of soluble polymers and biodegradable polymers by mechanical crushing, emulsion stirring, electrostatic spraying, 3D printing or microfluidics, and cross-linking the biodegradable polymer network by photoinitiation to obtain bioabsorbable polymer microparticles with adjustable degradation rate; wherein the bioabsorbable polymer microparticles include soluble polymers, biodegradable polymers and photoinitiators, and the degradation rate is adjustable by adjusting the ratio of each component; the soluble polymer includes at least one of gelatin, alginate, hyaluronic acid, silk fibroin chitosan, and carboxymethyl chitosan; the biodegradable polymer network is cross-linked by photoinitiator to obtain bioabsorbable polymer microparticles with adjustable degradation rate; wherein the bioabsorbable polymer microparticles include soluble polymers, biodegradable polymers and photoinitiators, and the degradation rate is adjustable by adjusting the ratio of each component; the soluble polymer includes at least one of gelatin, alginate, hyaluronic acid, silk fibroin chitosan, and carboxymethyl chitosan; The photoinitiator comprises at least one of methacrylated gelatin, methacrylated alginate, methacrylated hyaluronic acid, methacrylated silk fibroin and methacrylated chitosan, preferably methacrylated gelatin and methacrylated chitosan; the photoinitiator comprises one of 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L) and phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (LAP), preferably the photoinitiator is LAP;
[0051] In this embodiment, the bioabsorbable polymer microparticles with adjustable degradation rate may further comprise additives accounting for 0-100% of the mass percentage of the polymer microparticles, wherein the additives are one or more of inorganic fillers, drugs, and protein growth factors; the mass ratio of the soluble polymer to the biodegradable polymer is 1:10-10:1, preferably 1:5-2:1; the mass ratio of the biodegradable polymer to the photoinitiator is 10:1-100:1, preferably 50:1; the average particle size of the bioabsorbable polymer microparticles is 1-1000 μm, preferably the average particle size of the microparticles is 20-500 μm; the soluble polymer in the microparticles is completely dissolved within 3 days, and the biodegradable polymer is completely degraded within 3 months;
[0052] Step S200, weighing the components of the hard tissue adhesive matrix respectively, including polymerizable monomers, polymer powders and polymerization initiators; wherein the polymerizable monomers are methacrylates, or a combination of methacrylates and polymerizable monomers containing acidic groups; the polymer powders are at least one polymer selected from homopolymers of alkyl methacrylates, copolymers between alkyl methacrylates, copolymers of alkyl methacrylates and other polymerizable monomers, copolymers of alkyl methacrylates and alkylenedimethacrylates, and copolymers of alkyl methacrylates and diene monomers; the polymerization initiators include dibenzoyl peroxide, tributyl boron, and partial oxides of tributyl boron; preferably, partial oxides of tributyl boron; wherein the mass percentage of the polymerizable monomers is 20%-70%, the mass percentage of the polymer powder is 20%-70%, and the mass percentage of the polymerization initiator is 1%-20%;
[0053] Step S300, mixing the components of the hard tissue adhesive matrix and the bioabsorbable polymer microparticle pore-forming agent in a container to form an injectable slurry state, wherein the volume ratio of the hard tissue adhesive matrix to the bioabsorbable polymer microparticles in the injectable slurry state is 1:2-10:1, preferably 1:1-5:1;
[0054] The components of the hard tissue adhesive matrix are mixed with the bioabsorbable polymer microparticle pore-forming agent to obtain an injectable slurry, which is injected by a syringe, applied by a brush, or directly filled and implanted into the body before the dough stage; the dough stage time after the injectable slurry is implanted, i.e., the curing time, is 1-20 minutes after mixing. After the hard tissue adhesive filled into the body is cured, an acrylic-based hard tissue adhesive with a spatiotemporally controllable pore structure is formed in situ due to the rapid dissolution of the soluble polymer and the slow degradation of the biodegradable polymer.
[0055] After implantation, a time-space controllable through-porous structure is formed in situ in the adhesive; the formation time of the porous structure is controlled by adjusting the type and mass ratio of the soluble polymer and the biodegradable polymer, which is 1 day to 3 months; the pore size of the porous structure is controlled by adjusting the particle size of the bioabsorbable polymer microporogen, which is 1-1000 μm; the porosity of the porous structure is controlled by adjusting the particle volume ratio of the hard tissue adhesive matrix and the bioabsorbable polymer microporogen, which is 10%-66.7%. That is, the formation time of the porous structure is 24 hours to 3 months; the pore size of the porous structure is 1-1000 μm; and the porosity of the porous structure is 10%-66.7%.
[0056] The acrylic-based hard tissue adhesive prepared by the above method has a low curing temperature (<45°C) and possesses mechanical properties similar to those of cancellous bone (Young's modulus <1GPa). It can also generate a spatiotemporally controllable porous structure in situ in vivo, promote the ingrowth of endogenous cells and new bone formation, achieve three-dimensional spatial bone integration, and avoid repair failure or even fracture due to stress mismatch and poor interface bone integration after implantation.
[0057] In addition, the acrylic-based hard tissue adhesive prepared by the above method is simple to operate and has the same application method as traditional PMMA bone cement. It can be injected by syringe, applied by brush or directly filled and implanted in the body. It is suitable for orthopedic fields including fracture fixation, cone plasty, bone defect filling, bone tumor treatment, etc.; it is also suitable for in vivo auxiliary fixation of orthopedic implants.
[0058] The present invention is further described below in conjunction with specific examples.
[0059] Example 1: Preparation of gelatin-based microparticle pore-forming agent with adjustable degradation rate
[0060] See also Figures 1A-1C , Figures 1A-1C These are optical microscope images of GG-11-100, GG-11-200, and GG-11-400 droplets prepared by microfluidic technology in Example 1 of the present invention. The preparation method is as follows:
[0061] 1) adding gelatin and methacrylated gelatin of different mass ratios of 2:1, 1:1, and 1:2 to different deionized waters, and continuing stirring for 30 minutes in a 40° C. water bath to obtain three aqueous solutions A, wherein the total mass fraction of gelatin and methacrylated gelatin in the three aqueous solutions A is 5%; for example, adding 5 g of gelatin and methacrylated gelatin of different mass ratios of 2:1, 1:1, and 1:2 to 95 g of different deionized waters, three aqueous solutions A in which the total mass fraction of gelatin and methacrylated gelatin is 5% can be obtained;
[0062] 2) adding photoinitiator LAP to three aqueous solutions A respectively, with the mass ratio of methacrylated gelatin to photoinitiator being 50:1, and oscillating and dissolving to obtain three corresponding aqueous solutions B;
[0063] 3) adding three aqueous solutions B into the microfluidic droplet preparation system respectively, and each aqueous solution B can obtain three kinds of microdroplets with average particle sizes of 100 μm, 200 μm and 400 μm respectively, and obtain corresponding gelatin-based gel particles by 365 nm ultraviolet cross-linking;
[0064] That is, three different aqueous solutions A are obtained respectively, and each aqueous solution A can correspond to a aqueous solution B, with a total of three aqueous solutions B; after the three aqueous solutions B are added to the microfluidic droplet preparation system respectively, each aqueous solution B can obtain three kinds of microdroplets with average particle sizes of 100μm, 200μm, and 400μm, respectively, and a total of 9 kinds of microdroplets are obtained, namely: microdroplets with particle sizes of 100μm, 200μm, and 400μm at a mass ratio of 2:1; microdroplets with particle sizes of 100μm, 200μm, and 400μm at a mass ratio of 1:1; microdroplets with particle sizes of 100μm, 200μm, and 400μm at a mass ratio of 1:2;
[0065] 4) Collect the gelatin-based gel particles by centrifugation, wash with deionized water for 3 times, and freeze-dry to obtain gelatin-based microparticle pore-forming agents. The gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to methacrylated gelatin of 2:1 are named GG-21-100, GG-21-200, and GG-21-400 according to their particle sizes; the gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to methacrylated gelatin of 1:1 are named GG-11-100, GG-11-200, and GG-11-400 according to their particle sizes; and the gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to methacrylated gelatin of 1:2 are named GG-12-100, GG-12-200, and GG-12-400 according to their particle sizes.
[0066] Example 2: Preparation of gelatin-based microparticle pore-forming agent with adjustable degradation rate using methacrylated gelatin (GelMA-80) with methacrylated degree of 80%
[0067] 1) adding gelatin and GelMA-80 in a mass ratio of 2:1, 1:1, and 1:2 to deionized water, respectively, and continuing stirring in a 40° C. water bath for 30 minutes to obtain three corresponding aqueous solutions A, wherein the total mass fraction of gelatin and methacrylated gelatin in the three aqueous solutions A is 5%;
[0068] 2) Adding photoinitiator LAP to three aqueous solutions A, the mass ratio of GelMA-80 to photoinitiator is 50:1, and shaking to dissolve to obtain the corresponding three aqueous solutions B;
[0069] 3) The three aqueous solutions B were added into the microfluidic droplet preparation system respectively, and each aqueous solution B could obtain three microdroplets with average particle sizes of 100 μm, 200 μm and 400 μm respectively, and the corresponding gelatin-based gel microparticles were obtained by 365 nm ultraviolet cross-linking; 4) The gelatin-based gel microparticles were collected by centrifugation, washed with deionized water for 3 times, and freeze-dried to obtain the gelatin-based microparticle pore-forming agent. Among them, the gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to GelMA-80 of 2:1 were named GG80-21-100, GG80-21-200, and GG-8021-400 according to their particle size; the gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to GelMA-80 of 1:1 were named GG80-11-100, GG80-11-200, and GG80-11-400 according to their particle size; and the gelatin-based microparticle pore-forming agents with a mass ratio of gelatin to GelMA-80 of 1:2 were named GG80-12-100, GG80-12-200, and GG80-12-400 according to their particle size.
[0070] Example 3: Preparation of Alginate-Gelatin Hybrid Microparticle Pore Forming Agent with Adjustable Degradation Rate
[0071] 1) adding alginic acid and methacrylated gelatin in a mass ratio of 2:1, 1:1, and 1:2 to deionized water, and continuing stirring for 30 minutes in a 40° C. water bath to obtain three corresponding aqueous solutions A, wherein the total mass fraction of gelatin and methacrylated gelatin in the three aqueous solutions A is 2%;
[0072] 2) adding photoinitiator LAP to three solutions A respectively, with the mass ratio of methacrylated gelatin to photoinitiator being 50:1, and shaking to dissolve to obtain three corresponding aqueous solutions B;
[0073] 3) The three aqueous solutions B were added into the microfluidic droplet preparation system respectively, and each aqueous solution B could obtain microdroplets with an average particle size of 200 μm, and alginate-gelatin hybrid gel particles were obtained by cross-linking with 365 nm ultraviolet light;
[0074] 4) Collecting the alginate-gelatin hybrid microparticles by centrifugation, washing with deionized water for 3 times, and freeze-drying to obtain alginate-gelatin hybrid microparticle pore-forming agents, wherein the mass ratio of alginate to methacrylated gelatin is 2:1, 1:1, and 1:2, respectively, and chitosan-based microparticle pore-forming agents AG-21-200, AG-11-200, and AG-12-200.
[0075] To test the degradation rate of the microparticle pore-forming agent of Examples 1-3, a 2U / mL collagenase solution was prepared using a phosphate buffer solution. The microparticle pore-forming agent prepared in Examples 1-4 was immersed in the collagenase solution or the phosphate buffer solution as a control, and placed in a constant temperature water bath shaking shaker at 37°C and 60rpm. The microparticles were taken out at 1, 12, and 24 hours, washed with cold water 3 times, freeze-dried, and weighed to calculate the degradation rate.
[0076] Example 4: Preparation of low-porosity PMMA hard tissue adhesive with in-situ generation of spatiotemporal controllable pore structure
[0077] 1) Weigh the components of the hard tissue adhesive matrix respectively: polymerizable monomer methacrylate, polymer powder polymethacrylate, and polymerization initiator butoxydibutyl boron, wherein the mass percentage of methacrylate is 30%, the mass percentage of polymethacrylate is 65%, and the mass percentage of butoxydibutyl boron is 5%;
[0078] 2) weighing the bioabsorbable polymer particles of Examples 1-3 accounting for 20% of the total volume of the hard tissue adhesive matrix;
[0079] 3) The bioabsorbable polymer particles and the hard tissue adhesive matrix components in Examples 1-3 are mixed in a precooled ceramic container (4° C.) to an injectable slurry state, and the slurry is sucked up with a syringe and then injected into a mold or a patient's body. Depending on the different bioresorbable polymer particles used, the PMMA hard tissue adhesives are named PMMA-GG-21-100-L, PMMA-GG-21-200-L, PMMA-GG-21-400-L, PMMA-GG-11-100-L, PMMA-GG-11-200-L, PMMA-GG-11-400-L, PMMA-GG-12-100-L, PMMA-GG-12-200-L, PMMA-GG-12-400-L, PMMA-AG-21-200-L, PMMA-AG-11-200-L, and PMMA-AG-12-200-L.
[0080] The following table shows the degradation percentages of GG-12-200, GG-11-200, GG-21-200, GG80-11-200 and AG-11-200 microparticle pore-forming agents prepared by microfluidic technology in Examples 1-4 of the present invention after being immersed in collagenase solution or phosphate buffer for 1, 12, and 24 hours.
[0081]
[0082] Example 5: Preparation of a mesoporous PMMA hard tissue adhesive with in-situ spatiotemporally controllable pore structure
[0083] 1) Weighing the components of the hard tissue adhesive matrix respectively, including: polymerizable monomer methacrylate, polymer powder polymethacrylate, and polymerization initiator butoxydibutyl boron; wherein the mass percentage of methacrylate is 30%, the mass percentage of polymethacrylate is 65%, and the mass percentage of butoxydibutyl boron is 5%;
[0084] 2) weighing the bioabsorbable polymer particles of Examples 1-3 accounting for 50% of the total volume of the hard tissue adhesive matrix;
[0085] 3) The bioabsorbable polymer particles and the hard tissue adhesive matrix components in Examples 1-3 are mixed in a precooled ceramic container (4° C.) to an injectable slurry state, and the slurry is sucked up with a syringe and then injected into a mold or a patient's body. Depending on the different bioresorbable polymer particles used, the PMMA hard tissue adhesives are named PMMA-GG-21-100-M, PMMA-GG-21-200-M, PMMA-GG-21-400-M, PMMA-GG-11-100-M, PMMA-GG-11-200-M, PMMA-GG-11-400-M, PMMA-GG-12-100-M, PMMA-GG-12-200-M, PMMA-GG-12-400-M, PMMA-AG-21-200-M, PMMA-AG-11-200-M, and PMMA-AG-12-200-M.
[0086] Example 6: Preparation of high-porosity PMMA hard tissue adhesive with in-situ generation of spatiotemporal controllable pore structure
[0087] 1) Weighing the components of the hard tissue adhesive matrix respectively, including: polymerizable monomer methacrylate, polymer powder polymethacrylate, and polymerization initiator butoxydibutyl boron; wherein the mass percentage of methacrylate is 30%, the mass percentage of polymethacrylate is 65%, and the mass percentage of butoxydibutyl boron is 5%;
[0088] 2) weighing the bioabsorbable polymer particles of Examples 1-3 accounting for 100% of the total volume of the hard tissue adhesive matrix;
[0089] 3) The bioabsorbable polymer particles and the hard tissue adhesive matrix components in Examples 1-3 are mixed in a precooled ceramic container (4° C.) to an injectable slurry state, and the slurry is sucked up with a syringe and then injected into a mold or a patient's body. Depending on the different bioresorbable polymer particles used, the PMMA hard tissue adhesives are named PMMA-GG-21-100-H, PMMA-GG-21-200-H, PMMA-GG-21-400-H, PMMA-GG-11-100-H, PMMA-GG-11-200-H, PMMA-GG-11-400-H, PMMA-GG-12-100-H, PMMA-GG-12-200-H, PMMA-GG-12-400-H, PMMA-AG-21-200-H, PMMA-AG-11-200-H, and PMMA-AG-12-200-H.
[0090] Comparative Example 1: Preparation of non-porous PMMA hard tissue adhesive
[0091] 1) Weighing the components of the hard tissue adhesive matrix respectively, including: polymerizable monomer methacrylate, polymer powder polymethacrylate, and polymerization initiator butoxydibutyl boron; wherein the mass percentage of methacrylate is 30%, the mass percentage of polymethacrylate is 65%, and the mass percentage of butoxydibutyl boron is 5%;
[0092] 2) Mix the components of the hard tissue adhesive matrix in a precooled ceramic container (4°C) to an injectable slurry state, use a syringe to absorb the slurry and inject it into the mold or the patient's body. The non-porous PMMA hard tissue adhesive is recorded as PMMA-N.
[0093] Example 7: Preparation of mesoporous PMMA / 4-META hard tissue adhesive with in-situ spatiotemporal controllable pore structure
[0094] 1) Weighing the components of the hard tissue adhesive matrix respectively, including: a mixture of polymerizable monomers methacrylic acid ester and 4-methacryloyloxyethyl trimellitic anhydride, a polymer powder polymethacrylic acid ester, and a polymerization initiator butoxydibutyl boron, wherein the mass percentage of methacrylic acid ester is 28%, the mass percentage of 4-methacryloyloxyethyl trimellitic anhydride is 2%, the mass percentage of polymethacrylic acid ester is 65%, and the mass percentage of butoxydibutyl boron is 5%;
[0095] 2) weighing the bioabsorbable polymer particles of Examples 1-3 accounting for 50% of the total volume of the hard tissue adhesive matrix;
[0096] 3) In a precooled ceramic container (4° C.), the bioabsorbable polymer particles and the components of the hard tissue adhesive matrix in Examples 1-3 are mixed to an injectable slurry state, and the slurry is sucked up with a syringe and injected into a mold or a patient's body. According to the different bioabsorbable polymer particles used, the PMMA hard tissue adhesives are named PMMA / 4-META-GG-21-100-M, PMMA / 4-META-GG-21-200-M, PMMA / 4-META-GG-21-400-M, PMMA / 4-META-GG-11-100-M, PMMA / 4-META-GG-11-200-M, PMMA / 4-META-GG-11-400-M, PMMA / 4-META-GG-12-100-M, PMMA / 4-META-GG-12-200-M, PMMA / 4-META-GG-12-400-M, PMMA / 4-META-GG-13-100-M, PMMA / 4-META-GG-13-200-M, PMMA / 4-META-GG-13-200-M, PMMA / 4-META-GG-13-300-M, PMMA / 4-META-GG-13-400-M, PMMA / 4-META-GG-14-100-M, PMMA / 4-META-GG-14-200-M, PMMA / 4-META-GG-14-300-M, PMMA / 4-META-GG-14-400-M, PMMA / 4-META-GG-15-100-M, PMMA / 4-META-GG-15-200-M, PMMA / 4-META-GG-15-3 PMMA / 4-META-GG-12-400-M, PMMA / 4-META-AG-21-200-M, PMMA / 4-META-AG-11-200-M, PMMA / 4-META-AG-12-200-M.
[0097] Example 8: In vitro simulation of the process of in situ generation of spatiotemporally controllable pore structures of hard tissue adhesives
[0098] See also Figure 2A-Figure 3C , Figure 2A The spatiotemporal dynamic curves of the pores after PMMA-GG-11-100-M, PMMA-GG-11-200-M, and PMMA-GG-11-400-M in Example 5 of the present invention are immersed in the phosphate buffer solution in Example 8; Figure 2B Spatiotemporal dynamic curves were generated for the pores of PMMA-GG-11-100-M, PMMA-GG-11-200-M, and PMMA-GG-11-400-M in Example 5 of the present invention after being immersed in the collagenase solution in Example 8; Figure 2C Spatiotemporal dynamic curves were generated for the pores of PMMA-GG-11-200-L, PMMA-GG-11-200-M, and PMMA-GG-11-200-H in Examples 4-6 of the present invention after being immersed in the collagenase solution in Example 8; Figure 3A This is a scanning electron microscope image of the pore structure of PMMA-GG-11-200-L in Example 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours; Figure 3B This is a scanning electron microscope image of the pore structure of PMMA-GG-11-200-H in Example 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours; Figure 3CThis is a scanning electron microscope image of the pore structure of PMMA-GG-11-400-H in Examples 4-6 of the present invention after being immersed in the collagenase solution in Example 8 for 24 hours.
[0099] A 2U / mL collagenase solution was prepared using a phosphate buffer solution. The hard tissue adhesive prepared using the mold in Examples 4-7 and Comparative Example 1 was immersed in the collagenase solution or the phosphate buffer solution as a control, and placed in a constant temperature water bath shaking shaker at 37°C and 60rpm. The hard tissue adhesive was taken out at 1, 3, 5, 7, 9, 12, 18, and 24 hours, washed with water 3 times, and then dried. The porosity of the hard tissue adhesive was tested using the mercury injection method.
[0100] Example 9: Adhesion strength of hard tissue adhesive with in-situ spatiotemporal controllable pore structure to pig bone
[0101] Fresh porcine cancellous bone blocks were sawn off from fresh porcine femurs. 50 μL of the hard tissue adhesive prepared in Examples 4-7 and Comparative Example 1 was injected onto the bone blocks, and the other block was bonded in an end-to-end and lap shear manner. After the bonded bone blocks were placed in a 37°C incubator overnight, a tensile mechanical test was performed, and the maximum stress of the bonded joint before failure was recorded. Figure 4 , Figure 4 Shear adhesion strength of PMMA-GG-11-200-M in Example 5 of the present invention and PMMA-N in Comparative Example 1 to fresh pig bones.
[0102] Example 10: In situ generation of a hard tissue adhesive with a spatiotemporally controllable pore structure for sealing and repairing critical skull defects in rats
[0103] SD rats were anesthetized by intraperitoneal injection. After the anesthesia took effect, the skull area was prepared, disinfected, and covered with a towel, and the rats were placed in a prone position. A 3 cm longitudinal incision was made on the rat skull, and the skin, subcutaneous tissue, and muscle-periosteum layer were cut and opened to expose the skull bone plate. Two circular defects with a diameter of 5 mm were made on both sides of the midcranial suture of the skull using a high-speed drill with a 5 mm outer diameter trephine. The hard tissue adhesive slurry prepared in Examples 4-7 and Comparative Example 1 was sucked with a syringe and injected into the skull defect. After the hard tissue adhesive was cured, the periosteum and skin were sutured. Two months after the operation, the rat skull was imaged using micro-CT. See Figure 5A and Figure 5B , Figure 5A This is a micro-CT image of the rat skull defect in Example 10 repaired with PMMA-N in Comparative Example 1 of the present invention 8 weeks later; Figure 5B This is a micro-CT image of the rat skull defect repaired by PMMA-GG-11-200-M in Example 5 of the present invention 8 weeks after the repair.
[0104] Example 11: In situ generation of hard tissue adhesive with spatiotemporal controllable pore structure for vertebroplasty in rats
[0105] SD rats were anesthetized by intraperitoneal injection, and after the anesthesia took effect, the surgical area was prepared, disinfected, and covered with a drape. After the diseased tissue in the vertebral body was removed using a high-speed drill, the hard tissue adhesive slurry prepared in Examples 4-7 and Comparative Example 1 was sucked with a syringe and injected into the vertebral body to stabilize the vertebral body and restore its function.
[0106] Example 12: In situ generation of a hard tissue adhesive with a spatiotemporally controllable pore structure for auxiliary implantation of titanium nails in rat femoral heads
[0107] SD rats were anesthetized by intraperitoneal injection. After the anesthesia took effect, the surgical area was prepared, disinfected, and covered with a drape. The femoral head of the rat was exposed by incising the skin and subcutaneous tissue, and a circular defect with a diameter of 4 mm was made in the femoral head using a high-speed drill with a 4 mm outer diameter trephine. The hard tissue adhesive slurry prepared in Example 4-7 was dipped in a brush and then smeared on the titanium nail surface by a pen accumulation method, and then the titanium nail was accurately implanted in the femoral head of the rat.
[0108] Generally speaking, chemically cross-linked gel microspheres degrade slowly and cannot be rapidly leached out of the implanted body; on the contrary, although microspheres made of soluble polymers can dissolve rapidly in body fluids, they cannot stably exist when compounded with hard tissue adhesives because they cannot be chemically cross-linked, that is, they have begun to dissolve during the curing process, significantly reducing the structural stability and adhesion ability of the hard tissue adhesive. The acrylic-based hard tissue adhesive with in-situ generation and spatiotemporally controllable pore structure of the present invention uses bioabsorbable polymer microparticles with adjustable degradation rate as pore-forming agents to achieve pore formation that is controllable in both time and space. A bioabsorbable polymer microparticle pore-forming agent with adjustable degradation rate is obtained by combining a soluble polymer and a biodegradable polymer. The biodegradable polymer is used to fix the soluble polymer to prevent the soluble polymer from dissolving during the curing process of the hard tissue adhesive. The pore size and porosity of the acrylic-based hard tissue adhesive depend on the particle size and addition amount of the microparticle pore-forming agent; and the mechanical properties of the hard tissue adhesive are regulated at the same time. Its pore formation rate depends on the type and proportion of the soluble polymer and the biodegradable polymer in the microparticle pore-forming agent. Since soluble polymers leach out through dissolution, a relatively fast process that is usually completed within 3 days, while biodegradable polymers leach out through degradation, a relatively slow process that can usually last up to 3 months, changing the ratio of the two can effectively control the spatiotemporal dynamics of in situ pore generation.
[0109] In addition, the biodegradable polymer is preferably a polymer that can provide cell adhesion sites and has biological activity, including methacrylated gelatin rich in RGD sequence and matrix metalloproteinase target sequence, antibacterial cationic polymer-methacrylated chitosan, etc. After the soluble polymer is dissolved and leached, the undegraded biodegradable polymer can provide adhesion sites for endogenous cells, promote their proliferation, migration and osteogenic differentiation, further promote bone integration, and accelerate tissue regeneration.
[0110] In addition, functional additives can be added to the bioabsorbable polymer microparticle pore-forming agent with adjustable degradation rate, including one or more of inorganic fillers, drugs, and protein growth factors, so as to give the hard tissue adhesive the functions of antibacterial, anti-inflammatory, bone formation promotion, angiogenesis promotion, medical imaging, etc.
[0111] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
[0112] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. An acrylic-based hard tissue adhesive, characterized in that: Porous structures with in-situ generation and controllable space and time, including: A hard tissue adhesive matrix, comprising a polymerizable monomer, a polymer powder and a polymerization initiator, wherein the polymerizable monomer is polymerized into a polymer under the action of the polymerization initiator; and The bioabsorbable polymer microparticle pore-forming agent is mixed in the hard tissue adhesive matrix and can adjust the degradation rate.
2. The acrylic-based hard tissue adhesive according to claim 1, characterized in that The polymerizable monomer is methacrylate, or a combination of methacrylate and a polymerizable monomer containing an acidic group; The polymer powder is at least one selected from homopolymers of alkyl methacrylates, copolymers of alkyl methacrylates, copolymers of alkyl methacrylates and other polymerizable monomers, copolymers of alkyl methacrylates and alkylenedimethacrylates, and copolymers of alkyl methacrylates and diene monomers; The polymerization initiator is dibenzoyl peroxide, tributyl boron or a partial oxide of tributyl boron.
3. The acrylic-based hard tissue adhesive according to claim 1 or 2, characterized in that: In the hard tissue adhesive matrix, the mass percentage of the polymerizable monomer is 20%-70%, the mass percentage of the polymer powder is 20%-70%, and the mass percentage of the polymerization initiator is 1%-20%.
4. The acrylic-based hard tissue adhesive according to claim 1, characterized in that The bioabsorbable polymer microparticle pore-forming agent comprises a soluble polymer, a biodegradable polymer and a photoinitiator, and the degradation rate is adjusted by adjusting the ratio of the soluble polymer and the biodegradable polymer; The soluble polymer includes at least one of gelatin, alginic acid, hyaluronic acid, silk fibroin chitosan and carboxymethyl chitosan; The biodegradable polymer comprises at least one of methacrylated gelatin, methacrylated alginic acid, methacrylated hyaluronic acid, methacrylated silk fibroin and methacrylated chitosan; The photoinitiator is used for photocrosslinking of biodegradable polymers, including 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), ethyl 2,4,6-trimethylbenzoylphenylphosphonate (TPO-L) or lithium phenyl (2,4,6-trimethylbenzoyl) phosphate (LAP).
5. The acrylic-based hard tissue adhesive according to claim 4, characterized in that The bioabsorbable polymer microparticle pore-forming agent prepares polymer microparticles by mechanical crushing, emulsion stirring, electrostatic spraying, 3D printing or microfluidics; wherein the mass ratio of the soluble polymer to the biodegradable polymer is 1:10-10:1; the mass ratio of the biodegradable polymer to the photoinitiator is 10:1-100:
1.
6. The acrylic-based hard tissue adhesive according to claim 4 or 5, characterized in that The average particle size of the bioabsorbable polymer microparticle pore-forming agent is 1-1000 μm; the soluble polymer is completely dissolved within 72 hours, and the biodegradable polymer is completely degraded within 3 months.
7. A method for preparing an acrylic acid-based hard tissue adhesive, characterized in that: The steps include: S100, preparing double network gel microparticles composed of soluble polymers and biodegradable polymers by mechanical crushing, emulsion stirring, electrostatic jetting, 3D printing or microfluidics, and cross-linking the biodegradable polymer network by photoinitiation to obtain a bioabsorbable polymer microparticle pore-forming agent with adjustable degradation rate; S200, respectively weighing the components of the hard tissue adhesive matrix, including polymerizable monomers, polymer powder and polymerization initiator; and S300, mixing the polymerizable monomer, polymer powder and polymerization initiator with the bioabsorbable polymer microparticle pore-forming agent to form a mixture, wherein the volume ratio of the hard tissue adhesive matrix to the bioabsorbable polymer microparticle pore-forming agent is 1:2-10:
1.
8. The method for preparing the acrylic acid-based hard tissue adhesive according to claim 7, characterized in that: The polymerizable monomer, polymer powder and polymerization initiator are mixed with the bioabsorbable polymer microparticle pore-forming agent to obtain an injectable slurry, which is injected by a syringe, applied by a brush or directly filled and implanted; the curing time of the injectable slurry after implantation is 1-20 minutes.
9. The method for preparing the acrylic acid-based hard tissue adhesive according to claim 7 or 8, characterized in that: After implantation, a spatiotemporally controllable porous structure is formed in situ in the acrylic-based hard tissue adhesive; the formation time of the porous structure is controlled by adjusting the type and mass ratio of the soluble polymer to the biodegradable polymer; the pore size of the porous structure is controlled by adjusting the particle size of the bioabsorbable polymer microparticle pore-forming agent; and the porosity of the porous structure is controlled by adjusting the particle volume ratio of the hard tissue adhesive matrix to the bioabsorbable polymer microporogen.