Modified filtering membrane as well as preparation method and application thereof

A modified filtration membrane is prepared through a composite material of metal organic framework and silk nanofibers, combined with polydopamine, which solves the problems of low efficiency and high cost of existing water treatment membranes in removing heavy metal ions, and achieves efficient removal and improvement of mechanical properties. promote.

CN118718754APending Publication Date: 2024-10-01SHANGHAI TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310322450.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing water treatment membranes have low efficiency in removing heavy metal ions, and are difficult to maintain high water flux and mechanical strength. At the same time, their preparation costs are high, which limits their application scenarios.

Method used

A composite material of metal organic framework and silk nanofibers is used to prepare a modified filter membrane through a self-assembly method, combined with polydopamine to improve adsorption capacity and mechanical properties.

Benefits of technology

The filtration effect of efficiently removing heavy metal ions and nanoparticles is achieved while maintaining high water flux and mechanical strength, reducing preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_29
    Figure SMS_29
  • Figure SMS_30
    Figure SMS_30
  • Figure SMS_31
    Figure SMS_31
Patent Text Reader

Abstract

The invention discloses a modified filtering membrane as well as a preparation method and application thereof. Specifically, the invention discloses a preparation method of a modified filtering membrane, which comprises the following steps: self-assembling a metal organic framework X and silk nano microfibers to prepare the modified filtering membrane, the metal organic framework X is a metal organic framework A or a metal organic framework B; the metal organic framework B is a metal organic framework compound formed by a metal organic framework A and a metal removing polymer; the metal organic framework A is MIL-100 (Fe), MIL-101 (Cr) or MIL-101 (Cr / Al). The preparation method of the modified filtering membrane is simple, high water flux can be kept during use, and the modified filtering membrane has a good filtering effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane separation, and in particular to a modified filtering membrane, a preparation method thereof and an application thereof. Background Art

[0002] A recent United Nations report predicts that the world could face a 40% water shortage in just 15 years. The high toxicity and ubiquity of cadmium, chromium, lead, arsenic, mercury, and uranium present in water make heavy metals in water one of the most concerning issues. These metals have no role in human homeostasis, can cause multi-organ damage, lead to birth defects, and are classified as carcinogens.

[0003] Water purification is mainly to filter out impurities from water, that is, to remove particulate matter from water by forcing water molecules to pass through porous media. Current technologies used to purify wastewater, such as chemical precipitation, adsorbent adsorption or membrane separation, are usually expensive, have poor ion specificity, are prone to scaling or produce a large amount of chemical sludge, so new methods for purifying wastewater are urgently needed. Water treatment membranes are an efficient and energy-saving means of removing heavy metal ions and molecular-level pollutants. In order to improve the purification efficiency of water treatment membranes, various new materials (e.g., polymers, biopolymers, inorganic nanomaterials or metal-organic framework materials) and novel manufacturing methods (e.g., block copolymer self-assembly, template synthesis, track etching technology, chemical vapor deposition or layer-by-layer assembly) have been developed. However, it remains a challenge to prepare low-cost water treatment membranes while maintaining mechanical strength and high purification performance.

[0004] In addition to layered inorganic nanomaterials, biomaterials have also been used to make water treatment membranes. Recent studies have shown that silk nanofibers can be used to make filtration membranes with high water flux and efficient separation performance for the separation of dyes, proteins and nanoparticles. However, similar to other biomaterial-based filtration systems, the original silk nanofiber membranes have small and non-adjustable pore sizes, and the water (and solvent) permeability decreases significantly with increasing membrane thickness, and the amount of molecules that can be purified is also limited. Despite their shortcomings, biomaterials have proven to be a useful option for the development of new water treatment membranes, in part because of their cost-saving, environmental and biocompatible advantages. However, the efficient and accurate removal of heavy metal ions remains a huge challenge. This problem can be solved to some extent by combining different materials within the same membrane. The existing technology (Shengjie, Ling, Zhao, et al. Design and function of biomimetic multilayer water purification membranes. [J]. Science advances, 2017.) has reported the use of a composite membrane of hydroxyapatite and silk nanofibers for water purification. When filtering heavy metals, a better filtering effect can only be achieved by making the heavy metals into the form of nanoparticles, and it is impossible to directly filter heavy metal ions (particle size less than 2 nm).

[0005] Metal-organic frameworks (MOFs) are a class of porous crystalline materials that have attracted widespread attention due to their unprecedented internal surface area, easy chemical tunability, and extraordinary ability to selectively adsorb a large number of guest species. In addition, amorphous polymers (such as polydopamine) composed of high-density metal-scavenging functional groups can be introduced as extrinsic porosity to obtain a high density of additional functions on the polymer backbone, thereby improving water treatment rates and adsorbent capacity. Polydopamine contains amine and catechol functional groups, which not only enable metal scavenging but also provide a way to adhere the polymer to the internal surface of MOF materials. By incorporating polydopamine into MOFs, the hydrophilic polydopamine can be inhibited from dispersing into water, so it is easy to separate after water treatment. However, MOFs and their polymer composites cannot be prepared into membranes by themselves, which greatly limits their application scenarios. The addition of flexible materials (polymers, silk nanofibers) can greatly improve the mechanical properties and usability of the membranes.

[0006] Therefore, exploring a simple and stable preparation method to obtain metal organic framework / polymer complexes and prepare modified silk nanofiber composite membranes to adsorb heavy metal ion pollutants while maintaining high water flux and recyclability will be the key to the application of silk nanofiber membranes in wastewater treatment. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the defect of insufficient types of water treatment membranes in the prior art and provide a new modified filtration membrane, a preparation method thereof and its application. The preparation method of the modified filtration membrane of the present invention is simple, and when used, it can maintain high water flux and has good filtration effect.

[0008] The present invention solves the above technical problems through the following methods.

[0009] The present invention provides a method for preparing a modified filtration membrane, which comprises the following steps:

[0010] The metal organic framework X and the silk nanofibers are self-assembled to prepare the modified filtration membrane;

[0011] The metal organic framework X is metal organic framework A or metal organic framework B;

[0012] The metal organic framework B is a metal organic framework complex formed by the metal organic framework A and a metal scavenging polymer;

[0013] The metal organic framework A is MIL-100 (Fe), MIL-101 (Cr) or MIL-101 (Cr / Al).

[0014] In one embodiment of the present invention, the silk nanofibers are prepared by the following method, which comprises the following steps: self-assembling silk fibroin to prepare silk nanofibers.

[0015] The MIL-100 (Fe), MIL-101 (Cr) or MIL-101 (Cr / Al) are all conventional in the art.

[0016] In one embodiment of the present invention, the mass ratio of the metal organic framework X to the silk nanofibers is (0.5-1.5):1, for example 1:1.

[0017] In one embodiment of the present invention, the metal organic framework X and the silk nanofibers are mixed in water and then self-assembled, and the mass concentration of the metal organic framework X in water is preferably 0.3-0.8 mg / ml, such as 0.5 mg / ml, and the mass concentration of the silk nanofibers in water is preferably 0.3-0.8 mg / ml, such as 0.5 mg / ml.

[0018] In one embodiment of the present invention, the metal organic framework X and the silk nanofibers are mixed in water and self-assembled by passing through a filter membrane. The filter membrane is preferably a polycarbonate filter membrane or a nylon filter membrane. The method of passing through the filter membrane is suction filtration. The pressure of the suction filtration is preferably 70-90 KPa, for example 80 KPa.

[0019] In one embodiment of the present invention, the method for preparing the modified filtration membrane comprises the following steps:

[0020] The mixed aqueous solution of metal organic framework X and silk nanofibers is filtered to achieve self-assembly, wherein the mass concentrations of metal organic framework X and silk nanofibers in the mixed aqueous solution are independently 0.3-0.8 mg / ml, for example, 0.5 mg / ml, the filter membrane of the "filtration" is a polycarbonate filter membrane or a nylon filter membrane, and the pressure of the "filtration" is 70-90 KPa, for example, 80 KPa.

[0021] In one embodiment of the present invention, the particle size of the metal organic framework X is 100-500 nm. Preferably, the average particle size of the metal organic framework is 400 nm.

[0022] In one embodiment of the present invention, the metal organic framework X is a regular octahedral crystal.

[0023] In the metal organic framework A, the MIL-100 (Fe), MIL-101 (Cr) or MIL-101 (Cr / Al) can be prepared by conventional preparation methods in the art.

[0024] For example, the MIL-100(Fe) is prepared by the following method, which comprises the following steps: 3+ The organic carboxylic acid is mixed with the organic carboxylic acid to undergo coordination reaction to prepare MIL-100(Fe), wherein the organic carboxylic acid is trimesic acid.

[0025] Preferably, the Fe 3+ The molar ratio of the amount of the trimesic acid is (1.5-5):1, for example, 2.25:1.

[0026] Preferably, the Fe 3+ It is provided by ferric chloride, ferric nitrate, a hydrate of ferric chloride or a hydrate of ferric nitrate, for example, provided by a hydrate of ferric chloride, and further provided by FeCl3·6H2O.

[0027] The MIL-101(Cr) can be prepared by the following method, which comprises the following steps: 3+ The organic carboxylic acid is mixed with the organic carboxylic acid to undergo coordination reaction to prepare MIL-101(Cr), wherein the organic carboxylic acid is terephthalic acid.

[0028] Preferably, the Cr 3+ The molar ratio of the amount of the phthalic acid is (0.8-3):1, for example 1:1.

[0029] Preferably, the Cr 3+ It is provided by chromium chloride, chromium nitrate, a hydrate of chromium chloride or a hydrate of chromium nitrate, for example, it is provided by a hydrate of chromium nitrate, and further provided by Cr(NO3)3·9H2O.

[0030] The MIL-101 (Cr / Al) can be prepared by the following method, which comprises the following steps: 3+ 、Al 3+ The organic carboxylic acid is mixed with terephthalic acid to produce a coordination reaction to prepare MIL-101 (Cr / Al). The organic carboxylic acid is terephthalic acid.

[0031] Preferably, the Cr 3+ With Al 3+ The ratio of the amount of substance is (1~2):1, for example 1.5:1.

[0032] Preferably, the Cr 3+ With Al 3+ The ratio of the total amount of the substance to the amount of the terephthalic acid is (0.8-3):1, for example, 1.5:1.

[0033] Preferably, the Cr 3+ It is provided by chromium chloride, chromium nitrate, a hydrate of chromium chloride or a hydrate of chromium nitrate, for example, it is provided by a hydrate of chromium nitrate, and further provided by Cr(NO3)3·9H2O.

[0034] Preferably, the Al 3+ It is provided by aluminum chloride, aluminum nitrate, a hydrate of aluminum chloride or a mixture of aluminum nitrates, for example, provided by a hydrate of aluminum nitrate, and further provided by Al(NO3)3·9H2O.

[0035] Any of the above coordination reactions can be carried out in water; preferably, the water is deionized water; preferably, the volume molar ratio of the water to the organic carboxylic acid is independently 1 to 10 L / mol, such as 1.5 to 7.5 L / mol.

[0036] Any of the above coordination reactions can be carried out in an autoclave, for example, in a polytetrafluoroethylene-lined autoclave.

[0037] The reaction temperature of any of the above coordination reactions may be independently 100 to 200°C, preferably 130 to 180°C.

[0038] The reaction time of any of the above coordination reactions can independently be 5 to 80 hours, preferably 8 to 72 hours.

[0039] In one embodiment of the present invention, in any of the above coordination reactions, the reaction temperature is 120-140° C., for example, 130° C.; and the reaction time is 70-80 h, for example, 72 h.

[0040] In one embodiment of the present invention, in any of the above coordination reactions, the reaction temperature is 170-190° C., for example, 180° C.; and the reaction time is 7-9 h, for example, 8 h.

[0041] After the coordination reaction is completed, post-treatment can be performed through the following steps, which include: cooling, collecting products, and washing.

[0042] Preferably, the temperature after cooling is 20-40°C, such as 25-30°C.

[0043] Preferably, the collected product is collected by centrifugation or filtration, for example, by centrifugation.

[0044] Preferably, the washing is washing with water and washing with methanol respectively, the number of washing with water is, for example, 3 times, and the number of washing with methanol is, for example, 3 times.

[0045] In one embodiment of the present invention, in the metal organic framework B, the metal scavenging polymer is located inside the metal organic framework A.

[0046] In one embodiment of the present invention, in the metal organic framework B, the loading amount of the metal scavenging polymer is 10% to 30%, for example, 18% to 22%, further for example, 18%, 21% or 22%, and the loading amount refers to the mass percentage of the metal scavenging polymer in the metal organic framework B.

[0047] In one embodiment of the present invention, in the metal organic framework B, the metal scavenging polymer is polydopamine, and its corresponding monomer is dopamine.

[0048] Preferably, the metal organic framework B is prepared by any one of the following methods:

[0049] Method 1: In a water-insoluble organic solvent, the metal organic framework A is mixed with an aqueous solution of a monomer salt corresponding to the metal scavenging polymer to prepare a metal organic framework composite;

[0050] Method 2: In an organic solvent, the metal organic framework A is mixed with monomers corresponding to the metal scavenging polymer to prepare a metal organic framework composite.

[0051] Preferably, when the metal organic framework A in the metal organic framework B is MIL-101 (Cr) or MIL-101 (Cr / Al), the preparation method of the metal organic framework B is method 1 described above.

[0052] Preferably, when the metal organic framework A in the metal organic framework B is MIL-100(Fe), the preparation method of the metal organic framework A is method 2 described above.

[0053] Preferably, the method 1 is to mix the metal organic framework A with the water-insoluble organic solvent, and then mix it with an aqueous solution of a monomer salt corresponding to the metal scavenging polymer to prepare a metal organic framework complex; preferably, the time for "mixing the metal organic framework A with the water-insoluble organic solvent" is 0.1 to 1 h, for example 0.5 h; preferably, the time for "mixing with an aqueous solution of a monomer salt corresponding to the metal scavenging polymer" is 0.5 to 2 h, for example 1 h.

[0054] Preferably, in the method 1 and the method 2, the metal organic framework is pre-dried, and the drying temperature may be 100-180°C, such as 130-150°C.

[0055] Preferably, in the method 1, the water-insoluble organic solvent is a hydrocarbon solvent, such as n-hexane.

[0056] Preferably, in the method 1, the volume mass ratio of the water-insoluble organic solvent to the metal organic framework A is 50-100 mL / g, for example 77 mL / g.

[0057] Preferably, in the method 1, the monomer salt is the hydrochloride salt of the monomer.

[0058] Preferably, in the method 1, the molar mass ratio of the monomer salt to the metal organic framework A is 0.5-5 mmol / g, preferably 0.9-3.6 mmol / g, for example 0.9 mmol / g, 1.8 mmol / g or 3.6 mmol / g.

[0059] Preferably, in the method 1, the volume ratio of the water-insoluble organic solvent to the aqueous solution of the monomer salt is (30-50):1, for example 44:1.

[0060] Preferably, in the method 1, the mixing time is 1 to 3 hours, preferably 1 hour.

[0061] In a certain embodiment of the present invention, the method 1 further comprises the following steps: collecting solids, mixing the solids with alcohol solvents, water and bases; preferably, the volume mass ratio of the alcohol solvent to the metal organic framework A is 3-10 ml / mg, for example 6.5 ml / mg; preferably, the volume ratio of the water to the alcohol solvent is (1.5-5):1, for example 2.25:1; preferably, the molar mass ratio of the base to the metal organic framework is 0.01-0.1 mmol / mg, for example 0.04-0.05 mmol / mg. Preferably, the mixing time is 5-12 hours, for example 8-10 hours, and further for example 9 hours.

[0062] Preferably, the “mixing the solid with an alcohol solvent, water and a base” means mixing the solid with an alcohol solvent and water, and then mixing with a base.

[0063] Preferably, the solid is collected by centrifugation.

[0064] Preferably, the alcohol solvent is ethanol.

[0065] Preferably, the base is ammonia, and the ammonia can be in the form of aqueous ammonia, such as aqueous ammonia with a mass fraction of 25% to 28%.

[0066] The method 1 can be post-processed by the following steps, which include: collecting the product and washing the product. Preferably, the method of collecting the product is centrifugation. Preferably, the washing liquid of the "washing" is a nitrogen-containing compound solvent and / or an alcohol solvent; the nitrogen-containing compound solvent can be DMF; the alcohol solvent can be methanol.

[0067] Preferably, in the second method, the "mixing" is carried out under an inert gas, such as nitrogen.

[0068] Preferably, in the second method, the organic solvent is an alcohol solvent, such as methanol.

[0069] Preferably, the second method is to mix the monomer corresponding to the metal scavenging polymer with the organic solvent, and then mix it with the metal organic framework to prepare the metal organic framework complex; preferably, the time of "mixing with the metal organic framework" is 20 to 30 hours, for example 25 hours.

[0070] Preferably, in the second method, the molar volume ratio of the monomer to the organic solvent is 0.01-0.05 mol / L, for example, 0.02 mol / L.

[0071] Preferably, in the second method, the molar mass ratio of the monomer to the metal organic framework is 1 to 10 mmol / g, such as 4 to 5 mmol / g.

[0072] In one embodiment of the present invention, in the method for preparing silk nanofibers, the silk fibroin self-assembles in water; preferably, the mass fraction of the silk fibroin in the water is 0.1% to 0.3%, for example, 0.1% to 0.2%; preferably, the water is deionized water.

[0073] In one embodiment of the present invention, the temperature for the self-assembly of the silk fibroin is 50-70°C, for example 60°C.

[0074] In one embodiment of the present invention, the self-assembly time of the silk fibroin is until silk nanofibers are formed, preferably 7 to 35 days, such as 25 to 31 days.

[0075] In one embodiment of the present invention, the silk fibroin is prepared by the following method, which comprises the following steps:

[0076] I: Under the action of alkali, the cocoons are degummed to obtain degummed silk fibers;

[0077] II: Dissolve the degummed silk fibers in (1) to prepare silk fibroin.

[0078] The silk cocoons used in the present invention are commonly used silk cocoons in the art, such as silk cocoons used in the textile industry to make silk fabrics, preferably tussah cocoons.

[0079] Preferably, in said I, said base is a bicarbonate of an alkali metal, such as sodium bicarbonate.

[0080] Preferably, in said I, said base participates in the reaction in the form of an aqueous solution, and the mass fraction of said aqueous solution may be 0.2% to 0.8%, for example 0.5%.

[0081] Preferably, in said I, the mass ratio of said silkworm cocoons to said alkali is (0.8-1.5):1, for example 1:1.

[0082] Preferably, in said I, the "degumming" time is 20 to 40 minutes, for example 30 minutes.

[0083] Preferably, in said I, the number of times of "degumming" is 1 to 3 times, for example, 2 times.

[0084] Preferably, in said I, the temperature of said "degumming" is 60-70°C, for example 60°C.

[0085] Preferably, in said step I, drying is performed after said "degumming", and then said step II is performed, and the drying temperature may be 50-70°C, for example 60°C.

[0086] Preferably, in said II, said "dissolving" reagent is an alkali metal halide, such as lithium bromide; preferably, said "dissolving" reagent is in the form of an aqueous solution, and the concentration of said aqueous solution may be 8 to 10 mol / L, such as 9.3 mol / L; preferably, the molar mass ratio of said "dissolving" reagent to said degummed silk fiber is 0.05 to 0.15 mmol / g, such as 0.093 mmol / g.

[0087] Preferably, in said II, the temperature of "dissolving" may be 50-70°C, for example 60°C.

[0088] Preferably, in said II, the time of "dissolving" is until there is no agglomeration or precipitation.

[0089] Preferably, in II, after the "dissolution", dialysis is performed, the dialysis reagent may be water (eg, deionized water), and the dialysis time may be 60 to 80 hours, for example, 72 hours.

[0090] The present invention also provides a modified filtration membrane prepared by the modified filtration membrane preparation method.

[0091] In one embodiment of the present invention, the thickness of the modified filtration membrane is 1 to 300 μm, such as 50 to 240 μm, and further such as 67 to 240 μm.

[0092] The present invention also provides a metal organic framework C, which is the metal organic framework B as described in any of the above schemes, wherein in the metal organic framework B, the metal organic framework A is MIL-101 (Cr) or MIL-101 (Cr / Al).

[0093] The present invention also provides a method for preparing a metal organic framework C, which is the above-mentioned method 1.

[0094] The present invention also provides an application of the modified filtration membrane or the metal organic framework C in the removal of organic dyes and the interception of nanoparticles or heavy metal ions.

[0095] Preferably, the organic dye is Eosin B, Orange G, Alcian Blue 8GX, Coomassie Brilliant Blue R, Coomassie Brilliant Blue G, Rhodamine B, Congo Red or Direct Red 81.

[0096] Preferably, the heavy metal ions are mercury ions, arsenic ions, lead ions, nickel ions, chromium ions or cadmium ions, such as Hg + 、As3+ , Pb 2+ 、Ni 2+ Cr 3+ or Cd 2+ , preferably Hg + 、As 3+ or Pb 2+ .

[0097] Preferably, the nanoparticles are platinum nanoparticles or gold nanoparticles.

[0098] Preferably, the particle size of the nanoparticles is 1-100 nm, preferably 3-100 nm, such as 3 nm or 13 nm.

[0099] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0100] The reagents and raw materials used in the present invention are commercially available.

[0101] The positive and progressive effects of the present invention are:

[0102] (1) The modified filtration membrane preparation method of the present invention is simple, the conditions are mild, and the raw materials are easily available.

[0103] (2) The modified filtration membrane of the present invention has good filtering effects on nanoparticles, organic dyes and heavy metal ions. DETAILED DESCRIPTION

[0104] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0105] In the following examples, TEM: transmission electron microscopy (TEM) images were acquired on a JEOL JEM 1400 field emission transmission electron microscope with a voltage set to 120 kV; SEM: scanning electron microscopy (SEM) images were acquired on a JEOL JSM 7800FPrime SEM; PXRD: powder X-ray diffraction patterns (PXRD) were acquired on a Bruker D8 ADVANCE diffractometer.

[0106] Example 1 MIL-101 (Cr) silk nanofiber composite membrane

[0107] (1) Preparation of MIL-101(Cr)

[0108] 1.57 g Cr(NO3)3·9H2O and 0.66 g terephthalic acid were dissolved in 60 mL deionized water. The mixture was added to a polytetrafluoroethylene-lined autoclave and heated in an oven at 180°C for 8 hours. After cooling to room temperature, the product MIL-101(Cr) was collected by centrifugation and washed three times with clean water and anhydrous methanol, respectively.

[0109] MIL-101(Cr) was prepared according to the above method. SEM images and TEM images showed that the product was a regular octahedral crystal with a particle size in the range of 100nm-500nm and an average particle size of 400nm. The powder X-ray diffraction pattern was consistent with the fitted MIL-101(Cr), confirming that MIL-101(Cr) was well prepared.

[0110] (2) Preparation of silk nanofibers

[0111] Silk cocoons (20 g, purchased from Jiuheng Silk Market, Nanxun, Zhejiang Province, China) were boiled in 4L of 0.5% sodium bicarbonate aqueous solution (20 g of sodium bicarbonate dissolved in 4000 g of water to obtain a 0.5% sodium bicarbonate aqueous solution) for half an hour at 60°C, and the temperature was repeated once, and then the degummed silk fibers were washed with deionized water and then dried in an oven at 60°C overnight. 5 g of degummed silk fibers were placed in 0.05L of 9.3M lithium bromide aqueous solution and dissolved in a 60°C water bath until there was no agglomeration and precipitation. The solution was cooled to room temperature and dialyzed with deionized water. After dialysis for 72 hours, a silk fibroin solution with a mass fraction of ~2% was obtained. The concentration of the obtained silk fibroin solution was adjusted to 0.1-0.2% by mass with deionized water, and incubated at 60°C for about 1 month to obtain a silk nanofiber aqueous solution, which was observed to be polarized under a polarizer (a polarizer is a polarizer conventionally used in the art), indicating that silk nanofibers were prepared. Under polarized light, the silk nanofibers exist in a nematic phase.

[0112] (3) Preparation of MIL-101(Cr) silk nanofiber composite membrane

[0113] A 0.5 mg / mL MIL-101(Cr) / silk nanofiber aqueous solution (equal volumes of 1 mg / mL MIL-101(Cr) aqueous solution and 1 mg / mL silk nanofiber aqueous solution mixed) is passed through a nylon membrane or a polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve membrane self-assembly, thereby obtaining a modified silk nanofiber composite membrane on the nylon membrane or the polycarbonate membrane, and thus obtaining the target sewage purification membrane.

[0114] Using the composite membrane preparation method described in the present invention, composite membranes of different thicknesses were prepared by adjusting the volume of the MIL-101(Cr) / silk nanofiber aqueous solution, and it was found that there was a linear relationship between the membrane thickness and the solution volume, which was: ΔH=32.25V-20.58 (ΔH: μm, V: mL, where ΔH is the membrane thickness, and V is the volume of the aqueous solution for preparing the composite membrane). The diameter of the composite membrane corresponding to this linear relationship is 15 mm.

[0115] Example 2 Silk nanofiber composite membrane

[0116] (1) Complex of MIL-101(Cr) and polydopamine Preparation

[0117] 130 mg of MIL-101(Cr) powder prepared in Example 1 was heated at 130°C under vacuum overnight. Then 10 mL of n-hexane was added to MIL-101(Cr). After stirring for 0.5 h, 0.228 mL of dopamine hydrochloride aqueous solution of different concentrations (0.513 M, 1.026 M and 2.052 M) was added and stirred for 1 h to prepare different composites, respectively. and Then the supernatant was poured out, and the solid was centrifuged and 20 mL of ethanol, 45 mL of deionized water and 375 μL of ammonia water were added to the solid and stirred for 9 h. The product was collected by centrifugation and washed three times with DMF and anhydrous methanol respectively.

[0118] The infrared spectrum shows the characteristic peaks of primary and secondary amines, the selected area electron diffraction spectrum shows that the N element is evenly distributed in the composite, and the TEM shows that the obtained There is no polymer layer on the surface, indicating that polydopamine is mainly attached to the inside of MIL-101(Cr). TGA shows The PDA loading in the and The amounts of polydopamine loaded were 21% and 22% respectively, indicating that MIL-101(Cr) can only load 22% polydopamine at most.

[0119] The above method is used to prepare metal organic framework materials and polymer composites. The preparation conditions are mild and safe, without special high temperature and high pressure, and the experimental raw materials are simple and easy to obtain. The obtained metal organic framework materials and polymer composites have a relatively regular morphology and a medium size (100nm-500nm), which can provide a good foundation for subsequent reactions;

[0120] (2) Preparation of Silk Nanofiber Composite Membrane

[0121] 0.5 mg / mL Silk nanofiber aqueous solution (equal volume of 1 mg / mL The aqueous solution and 1 mg / mL of the silk nanofiber aqueous solution are mixed) and passed through a nylon membrane or a polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the nylon membrane or the polycarbonate membrane, and thus obtaining the target sewage purification membrane. The preparation of the silk nanofiber is the same as in Example 1.

[0122] Example 3 MIL-101 (Cr / Al) silk nanofiber composite membrane

[0123] (1) Preparation of MIL-101 (Cr / Al)

[0124] 1.44 g Cr(NO3)3·9H2O, 0.9 g Al(NO3)3·9H2O and 0.66 g terephthalic acid were dissolved in 60 mL deionized water. The mixture was added to a polytetrafluoroethylene-lined autoclave and heated in an oven at 180°C for 8 hours. After cooling to room temperature, the product MIL-101 (Cr / Al) was collected by centrifugation and washed three times with clean water and anhydrous methanol, respectively.

[0125] MIL-101(Cr / Al) was prepared according to the above method. SEM images showed that the product was a regular octahedral crystal with a size of about 400 nm.

[0126] (2) Preparation of MIL-101 (Cr / Al) silk nanofiber composite membrane

[0127] A 0.5 mg / mL MIL-101 (Cr / Al) / silk nanofiber aqueous solution (equal volumes of 1 mg / mL MIL-101 (Cr / Al) aqueous solution and 1 mg / mL silk nanofiber aqueous solution mixed) was passed through a nylon membrane or polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the nylon membrane or polycarbonate membrane, and thus obtaining the target sewage purification membrane. The preparation of silk nanofibers is the same as in Example 1.

[0128] Example 4 Silk nanofiber composite membrane

[0129] (1) Composite of MIL-101(Cr / Al) and polydopamine Preparation

[0130] 130 mg of MIL-101 (Cr / Al) powder obtained in Example 3 was heated at 130°C under vacuum overnight. Then 10 mL of n-hexane was added to MIL-101 (Cr / Al). After stirring for 0.5 h, 0.228 mL of dopamine hydrochloride aqueous solution of different concentrations (0.513 M, 1.026 M and 2.052 M) was added and stirred for 1 h to prepare different composites, respectively. and Then pour out the supernatant and centrifuge to leave the solid. Add 20 mL of ethanol, 45 mL of deionized water and 375 μL of ammonia water to the solid and stir for 9 h. Collect the product by centrifugation and wash it three times with DMF and anhydrous methanol respectively.

[0131] SEM shows the There is no polymer layer on the surface, indicating that polydopamine is mainly attached to the inside of MIL-101(Cr / Al).

[0132] (2) Preparation of Silk Nanofiber Composite Membrane

[0133] 0.5 mg / mL Silk nanofiber aqueous solution (equal volume of 1 mg / mL The aqueous solution and 1 mg / mL of the silk nanofiber aqueous solution are mixed) and passed through a nylon membrane or a polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the nylon membrane or the polycarbonate membrane, and thus obtaining the target sewage purification membrane. The preparation of the silk nanofiber is the same as in Example 1.

[0134] Example 5 MIL-100 (Fe) silk nanofiber composite membrane

[0135] (1) Preparation of MIL-100(Fe)

[0136] 9.72 g FeCl3·6H2O and 3.36 g H3BTC (trichemic acid) were dissolved in 120 mL deionized water. The mixture was added to a polytetrafluoroethylene-lined autoclave and heated in an oven at 130°C for 72 hours. After cooling to room temperature, the product MIL-100 (Fe) was collected by centrifugation and washed three times with clean water and anhydrous methanol, respectively.

[0137] (2) Preparation of MIL-100(Fe) silk nanofiber composite membrane

[0138] will contain 0.5mg mL -1The aqueous solution of silk nanofibers and MIL-100 (Fe) particles is passed through a polycarbonate filter membrane or a nylon membrane on a vacuum filtration device to realize self-assembly of a composite membrane, thereby obtaining a modified silk nanofiber composite membrane on the polycarbonate filter membrane or the nylon membrane.

[0139] The preparation of silk nanofibers is the same as in Example 1.

[0140] Example 6 Silk nanofiber composite membrane

[0141] (1) Preparation of free dopamine

[0142] Add 20 mL of anhydrous tetrahydrofuran and 20 mL of anhydrous methanol to a three-necked flask, add 2 g of dopamine hydrochloride under nitrogen purge, then slowly add 0.136 g of CaCl2 in small amounts over 5 minutes, stir at room temperature for 48 hours under nitrogen protection. Wash the obtained product with tetrahydrofuran 5 times.

[0143] (2) Complex of MIL-100(Fe) and polydopamine Preparation

[0144] 2g of MIL-100 (Fe) was activated in a 150°C vacuum oven overnight. After activation, the reaction vessel was cooled to room temperature, and then nitrogen was passed through the sample for 10 minutes, and 400mL of 0.02M dopamine in methanol solution was added under nitrogen purge. After about 1 hour, the orange powder turned dark purple, indicating polymerization. The reaction was stirred at room temperature for 24 hours under nitrogen protection. After completion, the reaction mixture was vacuum filtered and washed with a large amount of methanol and water.

[0145] (3) Preparation of Silk Nanofiber Composite Membrane

[0146] 0.5 mg / mL Silk nanofiber aqueous solution (equal volume of 1 mg / mL The aqueous solution and 1 mg / mL of the silk nanofiber aqueous solution are mixed) and passed through a nylon membrane or a polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the nylon membrane or the polycarbonate membrane, and thus obtaining the target sewage purification membrane. The preparation of the silk nanofiber is the same as in Example 1.

[0147] Comparative Example 1 Silk Nanofiber Membrane

[0148] A 1 mg / mL silk nanofiber aqueous solution was passed through a nylon membrane or a polycarbonate membrane used as a filter in a vacuum filtration device at a fixed pressure of 80 KPa to achieve membrane self-assembly, thereby obtaining a silk nanofiber membrane on the nylon membrane or the polycarbonate membrane. The preparation of the silk nanofibers was the same as in Example 1.

[0149] Effect test example: Testing the filtration performance of different composite membranes

[0150] A: Water flux test method:

[0151] The filtration effect test was carried out on a solvent filter (where a nylon membrane was used as the base membrane, the diameter was 25 mm, and the inner diameter of the funnel top was 15 mm).

[0152] The aqueous solution of the metal organic framework and the silk nanofibers is passed through a base membrane used as a filter in a solvent filter at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the base membrane.

[0153] Also at a fixed pressure of 80 KPa, 10 mL of deionized water was filtered through the modified silk nano-microfiber composite membrane on the substrate membrane in the solvent filter, and the filtration time was recorded.

[0154] Water flux (L h -1 m -2 bar -1 ) is calculated as follows:

[0155]

[0156] V is the volume of the filtered solution (here 10 mL), T is the measured filtration time (h), and S is the effective membrane filtration area (m 2 ), ΔP is the pressure across the membrane (here 0.8 bar).

[0157] B: Testing methods for filtering effects of different substances: various particles, dyes and heavy metal ions, etc.:

[0158] The filtration effect test was carried out on a solvent filter (where a polycarbonate membrane was used as the base membrane, the diameter was 25 mm, and the inner diameter of the funnel top was 15 mm).

[0159] The aqueous solution of the metal organic framework and the silk nanofibers is passed through a base membrane used as a filter in a solvent filter at a fixed pressure of 80 KPa to achieve self-assembly of the membrane, thereby obtaining a modified silk nanofiber composite membrane on the base membrane.

[0160] Preparation of pollutant solutions: Prepare aqueous solutions of dyes with specific concentrations (Table 1) with deionized water, dilute the corresponding standard solutions with deionized water to prepare 1 ppm aqueous solutions of various heavy metal ions, and dilute 1 mg ml with deionized water. -1 Nanoparticle solutions of specific concentrations were prepared (Table 1).

[0161] At a fixed pressure of 80KPa, 10mL of pollutant solution was passed through the modified silk nanofiber composite membrane on the substrate membrane to evaluate the filtration effect of the membrane. The concentrations of dye and nanoparticle aqueous solution before and after filtration were obtained by testing the OD (optical density) value using a multifunctional microplate reader, and the concentrations of heavy metal ion aqueous solution before and after filtration were obtained by testing the element concentration using ICP-OES. The calculation formula for the interception rate (R, %) is:

[0162]

[0163] Among them C f and C p are the concentrations of the compound in the feed and filtrate, respectively.

[0164] 1. Water flux performance

[0165] The water flux of the 1 μm thick MIL-101 (Cr) silk nanofiber composite membrane in Example 1 was as high as 3249 L h -1 m -2 bar -1 The water flux of the 67μm thick MIL-101(Cr) silk nanofiber composite membrane is 200.75L / m 2 Even if the thickness of the MIL-101(Cr) silk nanofiber composite membrane increases to 230 μm, its water flux remains at 70 L h -1 m -2 bar -1 .

[0166] 2. Filtration performance

[0167] (1) The filtration effect of the 240 μm thick MIL-101 (Cr) silk nanofiber composite membrane on dyes and nanoparticles in Example 1 is shown in Table 1

[0168] Table 1

[0169]

[0170]

[0171] As shown in Table 1, whether it is gold nanoparticles with a diameter of 13nm or platinum nanoparticles with a diameter of 3nm, the retention rate of the MIL-101(Cr) silk nanofiber composite membrane is 100%. For the filtration of dyes, the MIL-101(Cr) silk nanofiber composite membrane achieved a retention rate of 99.5% for 240μM orange G and a retention rate of 99.1% for 199μM Coomassie Brilliant Blue R. This shows that the composite membrane of the present invention (the MIL-101(Cr) silk nanofiber composite membrane in Example 1, the MIL-101(Cr) silk nanofiber composite membrane in Example 2) has good performance in the filtration of dyes. Silk nanofiber composite membranes or other embodiments of composite membranes) can effectively remove substances larger than 3nm by size exclusion. Common nanoparticle pollutants in water, such as bacteria, viruses and inorganic nanoparticles, are much larger than this scale, so they can all be filtered by the composite membrane.

[0172] (2) Heavy metal ion filtration performance is shown in Table 2 (the thickness of the following filter membrane is 67 μm)

[0173] Table 2

[0174]

[0175] As shown in Table 2, the composite membrane of the present invention can effectively remove mercury, arsenic and lead. The silk nanofiber composite membrane can remove chromium and cadmium with rejection rates of 9.3% and 5.1%, respectively.

Claims

1. A method for preparing a modified filtration membrane, comprising the following steps: The metal organic framework X and the silk nanofibers are self-assembled to prepare the modified filtration membrane; The metal organic framework X is metal organic framework A or metal organic framework B; The metal organic framework B is a metal organic framework complex formed by the metal organic framework A and a metal scavenging polymer; The metal organic framework A is MIL-100 (Fe), MIL-101 (Cr) or MIL-101 (Cr / Al).

2. The method for preparing the modified filtration membrane according to claim 1, It is characterized in that It meets one or more of the following conditions: (1) The mass ratio of the metal organic framework X to the silk nanofibers is (0.5-1.5):1, for example 1:1; (2) The metal organic framework X and the silk nanofibers are mixed in water and then self-assembled, wherein the mass concentration of the metal organic framework X in water is preferably 0.3-0.8 mg / ml, for example 0.5 mg / ml, and the mass concentration of the silk nanofibers in water is preferably 0.3-0.8 mg / ml, for example 0.5 mg / ml; (3) The silk nanofibers are prepared by the following method, which comprises the following steps: self-assembling silk fibroin to prepare silk nanofibers; (4) The particle size of the metal organic framework X is 100-500 nm, preferably, the average particle size of the metal organic framework is 400 nm; (5) The metal organic framework X is a regular octahedral crystal; (6) In the metal organic framework B, the metal scavenging polymer is located inside the metal organic framework A; (7) In the metal organic framework B, the loading amount of the metal scavenging polymer is 10% to 30%, such as 18% to 22%, and further such as 18%, 21% or 22%; (8) In the metal organic framework B, the metal scavenging polymer is polydopamine, and its corresponding monomer is dopamine.

3. The method for preparing the modified filtration membrane according to claim 2, It is characterized in that It meets one or more of the following conditions: (1) The metal organic framework X and the silk nanofibers are mixed in water and self-assembled by passing through a filter membrane, wherein the filter membrane is preferably a polycarbonate filter membrane or a nylon filter membrane, and the method of passing through the filter membrane is suction filtration, and the pressure of the suction filtration is preferably 70-90 KPa, for example 80 KPa; (2) In the method for preparing the silk nanofibers, the silk fibroin is self-assembled in water; preferably, the mass fraction of the silk fibroin in the water is 0.1% to 0.3%, such as 0.1% to 0.2%; preferably, the water is deionized water; (3) In the method for preparing the silk nanofibers, the temperature at which the silk fibroin is self-assembled is 50 to 70° C., for example, 60° C.; (4) In the method for preparing the silk nanofibers, the time for the silk fibroin to self-assemble is 7 to 35 days, for example, 25 to 31 days; (5) The metal organic framework B is prepared by any one of the following methods: Method 1: In a water-insoluble organic solvent, the metal organic framework A is mixed with an aqueous solution of a monomer salt corresponding to the metal scavenging polymer to prepare a metal organic framework composite; Method 2: In an organic solvent, the metal organic framework A is mixed with monomers corresponding to the metal scavenging polymer to prepare a metal organic framework composite.

4. The method for preparing the modified filtration membrane according to claim 3, It is characterized in that It meets one or more of the following conditions: (1) In the method for preparing the silk nanofibers, the silk fibroin is prepared by the following method, which comprises the following steps: I: Under the action of alkali, the cocoons are degummed to obtain degummed silk fibers; II: dissolving the degummed silk fibers in (1) to prepare silk fibroin; (2) In the method for preparing the metal organic framework B, the first method is to mix the metal organic framework A with the water-insoluble organic solvent, and then mix it with the aqueous solution of the monomer salt corresponding to the metal scavenging polymer to prepare the metal organic framework complex; preferably, the time for "mixing the metal organic framework A with the water-insoluble organic solvent" is 0.1 to 1 hour, for example 0.5 hours; preferably, the time for "mixing with the aqueous solution of the monomer salt corresponding to the metal scavenging polymer" is 0.5 to 2 hours, for example 1 hour; (3) In the method for preparing the metal organic framework B, in the method 1 and the method 2, the metal organic framework A is dried in advance, and the drying temperature may be 100 to 180° C., for example, 130 to 150° C.; (4) In the method for preparing the metal organic framework B, in the method 1, the water-insoluble organic solvent is a hydrocarbon solvent, such as n-hexane; (5) In the method for preparing the metal organic framework B, in the method 1, the volume mass ratio of the water-insoluble organic solvent to the metal organic framework A is 50 to 100 mL / g, for example 77 mL / g; (6) In the method for preparing the metal organic framework B, in the method 1, the monomer salt is the hydrochloride salt of the monomer; (7) In the method for preparing the metal organic framework B, in the method 1, the molar mass ratio of the monomer salt to the metal organic framework A is 0.5 to 5 mmol / g, preferably 0.9 to 3.6 mmol / g, for example 0.9 mmol / g, 1.8 mmol / g or 3.6 mmol / g; (8) In the method for preparing the metal organic framework B, in the method 1, the volume ratio of the water-insoluble organic solvent to the aqueous solution of the monomer salt is (30-50):1, for example 44:1; (9) In the method for preparing the metal organic framework B, in the method 1, the mixing time is 1 to 3 hours, preferably 1 hour; (10) In the method for preparing the metal organic framework B, the method 1 further comprises the following steps: collecting solids, mixing the solids with an alcohol solvent, water and a base, for example, collecting solids, mixing the solids with an alcohol solvent and water, and then mixing with a base; Preferably, the volume mass ratio of the alcohol solvent to the metal organic framework A is 3 to 10 ml / mg, for example 6.5 ml / mg; preferably, the volume ratio of the water to the alcohol solvent is (1.5 to 5): 1, for example 2.25: 1; preferably, the molar mass ratio of the base to the metal organic framework is 0.01 to 0.1 mmol / mg, for example 0.04 to 0.05 mmol / mg; preferably, the mixing time is 5 to 12 h, for example 8 to 10 h, and further for example 9 h; Preferably, the alcohol solvent is ethanol; preferably, the base is ammonia, and the ammonia is in the form of aqueous ammonia, preferably in the form of aqueous ammonia with a mass fraction of 25% to 28%; (11) In the method for preparing the metal organic framework B described above, in the second method, the "mixing" is carried out under an inert gas, for example, under the action of nitrogen; (12) In the method for preparing the metal organic framework B, in the method 2, the organic solvent is an alcohol solvent, such as methanol; (13) In the method for preparing the metal organic framework B, the second method is to mix the monomer corresponding to the metal scavenging polymer with the organic solvent, and then mix it with the metal organic framework to prepare the metal organic framework composite; preferably, the time of "mixing with the metal organic framework" is 20 to 30 hours, for example 25 hours; (14) In the method for preparing the metal organic framework B, in the method 2, the molar volume ratio of the monomer to the organic solvent is 0.01 to 0.05 mol / L, for example 0.02 mol / L; (15) In the method for preparing the metal organic framework B described in method 2, the molar mass ratio of the monomer to the metal organic framework A is 1 to 10 mmol / g, for example, 4 to 5 mmol / g.

5. The method for preparing the modified filtration membrane according to claim 4, It is characterized in that It meets one or more of the following conditions: (1) In the method for preparing silk fibroin, in said I, the base is a bicarbonate of an alkali metal, such as sodium bicarbonate; (2) In the method for preparing silk fibroin, in said I, the base is reacted in the form of an aqueous solution, and the mass fraction of the aqueous solution may be 0.2% to 0.8%, for example 0.5%; (3) In the method for preparing silk fibroin, in said I, the mass ratio of the silkworm cocoon to the alkali is (0.8-1.5):1, for example, 1:1; (4) In the method for preparing silk fibroin, in the step I, the degumming time is 20 to 40 minutes, for example, 30 minutes; (5) In the method for preparing silk fibroin, in the step I, the number of "degumming" is 1 to 3 times, for example, 2 times; (6) In the method for preparing silk fibroin, in said step I, the temperature of "degumming" is 60-70°C, for example 60°C; (7) In the method for preparing silk fibroin, in II, the "dissolving" reagent is an alkali metal halide, such as lithium bromide; preferably, the "dissolving" reagent is in the form of an aqueous solution, and the concentration of the aqueous solution can be 8-10 mol / L, such as 9.3 mol / L; preferably, the molar mass ratio of the "dissolving" reagent to the degummed silk fiber is 0.05-0.15 mmol / g, such as 0.093 mmol / g; (8) In the method for preparing silk fibroin, in II, the temperature of "dissolving" can be 50-70°C, for example, 60°C; (9) In the method for preparing silk fibroin, in II, after the "dissolution", dialysis is performed, the dialysis reagent may be water, and the dialysis time may be 60 to 80 hours, for example 72 hours; (10) The MIL-100(Fe) is prepared by the following method, which comprises the following steps: 3+ Mixing with an organic carboxylic acid to undergo coordination reaction to prepare MIL-100(Fe), wherein the organic carboxylic acid is trimesic acid; (11) The MIL-101(Cr) is prepared by the following method, which comprises the following steps: 3+ Mixing with an organic carboxylic acid to undergo coordination reaction to prepare MIL-101(Cr), wherein the organic carboxylic acid is terephthalic acid; (12) The MIL-101 (Cr / Al) is prepared by the following method, which comprises the following steps: 3 + 、Al 3+ The organic carboxylic acid is mixed with terephthalic acid to produce a coordination reaction to prepare MIL-101 (Cr / Al). The organic carboxylic acid is terephthalic acid.

6. The method for preparing the modified filtration membrane according to claim 5, It is characterized in that It meets one or more of the following conditions: (1) In the preparation method of MIL-100(Fe), the Fe 3+ The molar ratio of the trimesic acid is (1.5-5):1, for example 2.25:1; (2) In the preparation method of MIL-100(Fe), the Fe 3+ It is provided by ferric chloride, ferric nitrate, hydrate of ferric chloride or hydrate of ferric nitrate, for example, provided by hydrate of ferric chloride, further provided by FeCl 3 6H 2 O provides; (3) In the preparation method of MIL-101(Cr), the Cr 3+ The molar ratio of the terephthalic acid is (0.8-3):1, for example 1:1; (4) In the preparation method of MIL-101(Cr), the Cr 3+ It is provided by chromium chloride, chromium nitrate, chromium chloride hydrate or chromium nitrate hydrate, for example, provided by chromium nitrate hydrate, further provided by Cr(NO 3 ) 3 9H 2 O provides; (5) In the preparation method of MIL-101 (Cr / Al), the Cr 3+ With Al 3+ The ratio of the amount of substance is (1-2):1, for example 1.5:1; (6) In the preparation method of MIL-101 (Cr / Al), the Cr 3+ With Al 3+ The ratio of the total amount of the substance to the amount of the terephthalic acid is (0.8-3):1, for example, 1.5:1; (7) In the preparation method of MIL-101 (Cr / Al), the Cr 3+ It is provided by chromium chloride, chromium nitrate, chromium chloride hydrate or chromium nitrate hydrate, for example, provided by chromium nitrate hydrate, further provided by Cr(NO 3 ) 3 9H 2 O provides; (8) In the preparation method of MIL-101 (Cr / Al), the Al 3+ It is provided by aluminum chloride, aluminum nitrate, a hydrate of aluminum chloride or a mixture of aluminum nitrates, for example, provided by a hydrate of aluminum nitrate, and further provided by Al(NO 3 ) 3 9H 2 O provides; (9) In the preparation methods of MIL-100(Fe), MIL-101(Cr) and MIL-101(Cr / Al), the coordination reaction is carried out in water; preferably, the water is deionized water; preferably, the volume molar ratio of the water to the organic carboxylic acid is independently 1 to 10 L / mol, for example 1.5 to 7.5 L / mol; (10) In the preparation methods of MIL-100(Fe), MIL-101(Cr) and MIL-101(Cr / Al), the reaction temperature of the coordination reaction is independently 100 to 200°C, preferably 130 to 180°C; (11) In the preparation methods of MIL-100(Fe), MIL-101(Cr) and MIL-101(Cr / Al), the reaction time of the coordination reaction is independently 5 to 80 hours, preferably 8 to 72 hours.

7. The method for preparing the modified filtration membrane according to claim 6, It is characterized in that In the preparation methods of MIL-100(Fe), MIL-101(Cr) and MIL-101(Cr / Al), in the coordination reaction, the reaction temperature is 120-140°C, for example, 130°C, and the reaction time is 70-80h, for example, 72h; Alternatively, the reaction temperature is 170-190° C., for example 180° C.; the reaction time is 7-9 h, for example 8 h.

8. A method for preparing a modified filtration membrane according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: filtering a mixed aqueous solution of a metal organic framework X and silk nanofibers to achieve self-assembly, wherein the mass concentrations of the metal organic framework X and the silk nanofibers in the mixed aqueous solution are independently 0.3-0.8 mg / ml, for example, 0.5 mg / ml, the filter membrane of the "filtration" is a polycarbonate filter membrane or a nylon filter membrane, and the pressure of the "filtration" is 70-90 KPa, for example, 80 KPa.

9. A modified filtration membrane, prepared according to the method for preparing a modified filtration membrane according to any one of claims 1 to 8; Preferably, the thickness of the modified filtration membrane is 1 to 300 μm, such as 50 to 240 μm, and further such as 67 to 240 μm.

10. A metal organic framework C, which is the metal organic framework B according to any one of claims 1 to 8, wherein in the metal organic framework B, the metal organic framework A is MIL-101 (Cr) or MIL-101 (Cr / Al).

11. A method for preparing the metal organic framework C as claimed in claim 10, It is characterized in that It is method 1 as claimed in claim 3 or 4.

12. Use of the modified filtration membrane according to claim 9 or the metal organic framework C according to claim 10 in organic dye removal, nanoparticle or heavy metal ion interception; Preferably, the organic dye is Eosin B, Orange G, Alcian Blue 8GX, Coomassie Brilliant Blue R, Coomassie Brilliant Blue G, Rhodamine B, Congo Red or Direct Red 81; Preferably, the heavy metal ions are mercury ions, arsenic ions, lead ions, nickel ions, chromium ions or cadmium ions, such as Hg + 、As 3+ , Pb 2+ 、Ni 2+ Cr 3+ or Cd 2+ , preferably Hg + 、As 3+ or Pb 2+ ; Preferably, the nanoparticles are platinum nanoparticles or gold nanoparticles; Preferably, the particle size of the nanoparticles is 1-100 nm, preferably 3-100 nm, such as 3 nm or 13 nm.