Biomass adsorbent, preparation method thereof and application of biomass adsorbent in field of neodymium iron boron waste recovery

Through the adsorption, elution and desorption steps of the modified biomass adsorbent, the problems of complex processes and large loss of organic solvents in NdFeB recovery technology are solved, and high-purity separation of iron, praseodymium, neodymium and cobalt is efficiently recovered and simplified. Streamline the process and reduce costs.

CN118719006APending Publication Date: 2024-10-01LIAONING UNIVERSITY OF PETROLEUM AND CHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410955723.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing NdFeB recycling technology has a complicated process and a large loss of organic solvents, making it difficult to effectively recover valuable elements in NdFeB waste.

Method used

The modified biomass adsorbent is used to separate and recover iron, praseodymium, neodymium and cobalt through adsorption, elution and desorption steps, and the combination of modified cellulose and extraction agent is used to efficiently separate NdFeB waste.

Benefits of technology

Efficient recovery of NdFeB waste is achieved, with a purity greater than 99.9% and a recovery rate greater than 98%. The process is simple, the reagent consumption is small, and the biomass adsorbent can be reused, reducing the cost of separation and purification.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a biomass adsorbent, a preparation method thereof and application of the biomass adsorbent in the field of neodymium iron boron waste recovery, and the preparation method of the biomass adsorbent comprises the following steps: biomass modification: biomass is crushed, water, hydrogen peroxide and sodium hydroxide are added, and after heating digestion, modified cellulose is obtained, and modified biomass is obtained; mixing the modified biomass, an extracting agent and a dispersing agent, heating and redistilling, and evaporating and drying to obtain the biomass adsorbent. The invention further discloses application of the biomass adsorbent in the field of neodymium iron boron waste recovery. The biomass adsorbent prepared by the method is good in stability, and metal ions in a solution can be separated and recycled by utilizing different adsorption properties of the biomass adsorbent on the metal ions. The method for recycling the neodymium iron boron waste by adopting the biomass adsorbent has the advantages of simplicity in operation and low cost, and effective recycling of iron, praseodymium neodymium and cobalt can be realized only through adsorption, leaching and desorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to hydrometallurgical technology, and in particular to a biomass adsorbent, a preparation method thereof and application thereof in the field of NdFeB waste recovery. Background Art

[0002] There have been many studies on the preparation of biomass adsorbents and their use for the adsorption of organic matter. Chinese patent CN202211406880.3 discloses a biomass adsorbent and a method for its preparation, and the modified biomass is used for the adsorption of amino-containing antibiotics such as pefloxacin, ciprofloxacin, norfloxacin, and other amino-containing organic matter. Chinese patent CN201610626952.3 discloses a modified biomass adsorbent and a method for its preparation for the removal of NO in eutrophic water. However, the biomass adsorbents prepared in these patents are all used for the adsorption of organic matter, and the adsorption and separation of metal ions are not involved.

[0003] NdFeB magnets and SmCo magnets are two important rare earth permanent magnet materials. During the production and use process, about 30% of waste is generated, of which about 30% rare earth elements are contained. During the service process of permanent magnet materials, the materials will also fail due to oxidation and other reasons. They have great recycling potential. Chinese patent CN202010186548.5 invented a NdFeB waste resource recovery system and recovery method. Through the setting of the acid leaching liquid spray pyrolysis unit, the effective separation of iron and rare earth metals is realized, and the iron and rare earth metals are recovered separately, and the amount of hydrochloric acid used and the discharge of hydrochloric acid are reduced. Chinese patent CN202210307758.4 invented a full-cycle recycling preparation process for NdFeB waste magnetic steel. Through waste treatment, hydrogen crushing, mixing, air flow grinding, mixed powder cooling treatment, magnetic field forming, discharge plasma sintering, magnetic field aging heat treatment and other steps, the full-cycle recycling of waste magnetic steel is realized.

[0004] In summary, in the current field, the wet recovery methods of valuable elements in NdFeB have problems of complex processes and large organic solvent losses to varying degrees, and NdFeB recovery technology still needs further exploration and improvement. Summary of the invention

[0005] The purpose of the present invention is to propose a method for preparing a biomass adsorbent in view of the problems of complicated processes and large organic solvent loss in the current NdFeB recovery methods. The biomass adsorbent prepared by the method has good stability and can separate and recover metal ions in the solution by utilizing its different adsorption properties for metal ions. The use of the biomass adsorbent of the present invention to recover NdFeB waste has the advantages of simple operation and low cost. The effective recovery of iron, praseodymium, neodymium and cobalt can be achieved only through adsorption, elution and desorption.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a biomass adsorbent, comprising the following steps:

[0007] Step 1: modifying the biomass: crushing the biomass, adding water, hydrogen peroxide, and sodium hydroxide, heating and digesting to obtain modified cellulose, thereby obtaining the modified biomass;

[0008] Step 2: The modified biomass, the extractant and the dispersant are mixed, heated and refluxed, and then evaporated and dried to obtain the biomass adsorbent.

[0009] Furthermore, the biomass is crushed to a particle size of 1 to 100 meshes, preferably 10 to 50 meshes, more preferably 10 to 30 meshes.

[0010] Furthermore, the weight ratio of the biomass, water, hydrogen peroxide and sodium hydroxide is 1:2-10:0:05-0.5:0.1-1. The preferred weight ratio is 1:2-5:0:1-0.3:0.2-0.5.

[0011] Furthermore, the heating digestion temperature is 50-100°C, and the duration is 0.5-5 hours. Preferably, the heating digestion temperature is 70-90°C, and the duration is 1-3 hours.

[0012] Furthermore, the biomass is a mixture of one or more of straw, coconut shell and tree branches.

[0013] Furthermore, the extractant in step 2 is a mixture of one or more of di(2-ethylhexyl)phosphoric acid, 2-ethylhexylphosphonic acid mono-(2-ethylhexyl) ester and di(2,4,4-trimethylpentyl)phosphonic acid.

[0014] Furthermore, the dispersant in step 2 is alcohol and / or alkane.

[0015] Furthermore, the carbon chain length of the alcohol is C1-C10.

[0016] Furthermore, the alkane carbon chain length is C5-C10.

[0017] Furthermore, the weight ratio of the modified biomass, the extractant and the dispersant is 1:0.05-0.5:0.5-5. The preferred weight ratio is 1:0.1-0.4:1-3.

[0018] Furthermore, the heating reflux reaction temperature varies according to different types of dispersants, and is based on the observation of droplet reflux; the reflux time is 0.5 to 10 hours, and the preferred reflux time is 3 to 5 hours.

[0019] Furthermore, the evaporation drying temperature is 40-80°C, and the duration is 0.5-10 hours. Preferably, the evaporation drying temperature is 50-60°C, and the duration is 3-5 hours.

[0020] Another object of the present invention is to disclose a biomass adsorbent prepared by the above method.

[0021] Another object of the present invention is to disclose the use of a biomass adsorbent in the field of NdFeB waste recovery.

[0022] Furthermore, the method for recovering NdFeB waste using the biomass adsorbent comprises the following steps:

[0023] S1. Leaching the NdFeB waste with acid, and adjusting the acidity of the NdFeB leaching solution to control its pH value to 2.5 to 4.5 to obtain a NdFeB leaching solution;

[0024] S2. The NdFeB leaching solution is sequentially passed through a plurality of containers (including but not limited to separation columns) containing biomass adsorbents for stepwise adsorption to obtain biomass adsorbents loaded with iron, praseodymium, neodymium and cobalt, respectively;

[0025] S3. The biomass adsorbent loaded with iron, praseodymium, neodymium and cobalt is respectively eluted and desorbed to obtain a desorption solution containing iron, praseodymium, neodymium and cobalt. The purity of iron, praseodymium, neodymium and cobalt in the desorption solution containing iron, praseodymium, neodymium and cobalt is greater than or equal to 99.9%.

[0026] Furthermore, before the S2 biomass adsorbent is loaded into the container, it is saponified using a saponifying agent.

[0027] Furthermore, the saponifying agent used in the saponification is one or a mixture of ammonia water and sodium hydroxide.

[0028] Furthermore, the concentration of the saponifier is 4 to 13 mol / L, preferably 5 to 10 mol / L.

[0029] Furthermore, the amount of the saponifier is determined according to the amount of the extractant in the biomass adsorbent, and the molar ratio of the extractant to the saponifier is 1:0.1-0.8, preferably 1:0.2-0.6. Saponification can enhance the extraction performance of the biomass adsorbent for metal ions in the NdFeB leachate, thereby increasing the adsorption amount of the biomass adsorbent for metal ions.

[0030] Furthermore, the NdFeB leaching solution is obtained by acid leaching of abandoned NdFeB waste materials; the acid in S1 is a mixture of one or more of nitric acid, hydrochloric acid and sulfuric acid, and the acid concentration is 1 to 10 mol / L, preferably 2 to 6 mol / L.

[0031] Furthermore, the mass ratio of the amount of metal ion substance to the amount of acid in the NdFeB waste described in S1 is 1:1.0-4.0, and the preferred mass ratio is 2:2.5-3.5.

[0032] Furthermore, the acidity of the S1 leaching solution is adjusted by adding NdFeB waste.

[0033] Furthermore, the pH value of the NdFeB leaching solution in S1 is 3-4.

[0034] Furthermore, S2 passes the NdFeB leachate through three separation columns containing the same biomass adsorbent; passes the NdFeB leachate through the 1# container to obtain the 1# effluent, and monitors the iron content in the 1# effluent to be 0.01-1 g / L. When the iron content of the 1# effluent reaches a limit value, the feeding is stopped, and the 1# container is washed and desorbed. After desorption, the 1# container can be reused. The effluent No. 1 flows through the No. 2 container to obtain the No. 2 effluent. The content of Pr and Nd in the No. 2 effluent is monitored to be 0.01-1 g / L. When the content of Pr and Nd in the No. 2 effluent reaches the limit value, the feeding is stopped, and the No. 2 container is washed and desorbed. After desorption, the No. 2 container can be reused. The effluent No. 2 flows through the No. 3 container to obtain the No. 3 effluent. The content of Co in the No. 3 effluent is monitored to be 0.01-1 g / L. When the content of Co in the No. 3 effluent reaches the limit value, the feeding is stopped, and the No. 3 container is washed and desorbed. After desorption, the No. 3 container can be reused. The biomass adsorbent preferentially adsorbs iron, then Pr and Nd, and finally cobalt.

[0035] Furthermore, the adsorption endpoint of S3 is: the concentration of iron in the adsorption tail liquid flowing out of the 1# separation column, the concentration of praseodymium and neodymium in the adsorption tail liquid flowing out of the 2# separation column, and the concentration of cobalt in the adsorption tail liquid flowing out of the 3# separation column reach 0.01 to 1 g / L, preferably 0.1 g / L.

[0036] Furthermore, the eluting agent used for eluting in S3 is a low-concentration acid; the concentration of the low-concentration acid is 0.01-0.5 mol / L, preferably 0.1-0.3 mol / L; the low-concentration acid is a mixture of one or more of nitric acid, hydrochloric acid and sulfuric acid.

[0037] Furthermore, in S3, the ratio (volume ratio) of the biomass adsorbent to the eluent is 1:0.1-1, preferably 1:0.2-0.5.

[0038] Furthermore, the desorbent for desorption in S3 is a high-concentration acid; the concentration of the high-concentration acid is 0.5-6 mol / L, preferably 1-5 mol / L; the high-concentration acid is one or more of nitric acid, hydrochloric acid, and sulfuric acid.

[0039] Furthermore, in the desorption process described in S3, the ratio (volume ratio) of the biomass adsorbent to the desorbent is 1:0.1 to 2, preferably 1:0.5 to 1.5.

[0040] The biomass adsorbent of the present invention, its preparation method and its use in the field of NdFeB waste recovery have the following advantages compared with the prior art:

[0041] 1) The present invention provides a biomass adsorbent, in which an extractant is in-situ bonded to the modified biomass, and the extractant is tightly bonded to the polymer fiber skeleton of the modified biomass, is not easy to fall off, and has good stability.

[0042] 2) The biomass source of the present invention is widely available, cheap and easy to obtain, and compared with conventional resins, does not consume precious organic reagents.

[0043] 3) The present invention also provides the use of the biomass adsorbent in the field of NdFeB waste recovery. The biomass adsorbent of the present invention is used to separate and purify the NdFeB leachate. The separation and recovery of iron, praseodymium, neodymium and cobalt in the leachate can be achieved through only three steps of adsorption, elution and desorption. The process flow is simple, the reagent consumption is small, and the biomass adsorbent can be reused after desorption, further reducing the cost of separation and purification. The experimental results show that the purity of praseodymium, neodymium, iron and cobalt in the NdFeB waste leachate after separation by the present invention is greater than 99.9%, and the recovery rate is greater than 98%. DETAILED DESCRIPTION

[0044] The invention provides a biomass adsorbent, which comprises modifying biomass to obtain modified biomass, then mixing the modified biomass, an extractant and a dispersant, heating and reflux, and then evaporating and drying to obtain the biomass adsorbent.

[0045] In the present invention, the biomass includes a mixture of one or more materials that can provide cellulose, such as straw, coconut shell, branches, etc., mixed in any proportion; the extractant includes one or more of di(2-ethylhexyl)phosphoric acid, 2-ethylhexylphosphonic acid mono-(2-ethylhexyl) ester and di(2,4,4-trimethylpentyl)phosphonic acid; the dispersant is a mixture of one or more of alcohols (whose carbon chain length is C1-C10) and alkanes (whose carbon chain length is C5-C10) mixed in any proportion. In the present invention, the biomass adsorbent is prepared by suspension polymerization, which will be described in detail in the preparation method section later.

[0046] The present invention also provides a method for preparing the biomass adsorbent described in the above scheme, comprising the following steps:

[0047] (1) Modifying biomass: crushing the biomass, adding water, hydrogen peroxide, and sodium hydroxide, and heating and digesting to obtain modified cellulose, thereby obtaining modified biomass.

[0048] In the present invention, preferably, the biomass is crushed to a particle size of 1 to 100 mesh; preferably, the weight ratio of the biomass: water: hydrogen peroxide: sodium hydroxide is 1:2 to 10:0:05 to 0.5:0.1 to 1; preferably, the temperature of the heating digestion is 50 to 100°C, and the duration is 0.5 to 5 hours.

[0049] (2) Synthesis of biomass adsorbent: The modified biomass is mixed with an extractant and a dispersant, heated and refluxed, and then evaporated and dried to obtain the biomass adsorbent.

[0050] In the present invention, the weight ratio of biomass: extractant: dispersant is 1:0.05-0.5:0.5-5, more preferably 1:0.1-0.4:1-3.

[0051] In the present invention, the heating reflux reaction temperature varies according to different types of dispersants, and is based on the observation of droplet reflux; the reflux time is 0.5 to 10 hours.

[0052] In the present invention, the evaporation drying temperature is 40 to 80° C. and the duration is 0.5 to 10 hours.

[0053] The present invention also provides a method for recycling NdFeB waste, comprising the following steps:

[0054] Acid leaching is used to extract NdFeB waste to obtain NdFeB leaching solution; the acidity of the NdFeB leaching solution is adjusted to control the pH value thereof to be 2.5-4.5.

[0055] The biomass adsorbent is used to perform step-by-step adsorption on the NdFeB-containing leaching solution to obtain biomass adsorbents loaded with iron, praseodymium, neodymium and cobalt respectively; the biomass adsorbent is the biomass adsorbent described in the above scheme or the biomass adsorbent prepared by the preparation method described in the above scheme.

[0056] The biomass adsorbent loaded with iron, praseodymium, neodymium and cobalt is sequentially eluted and desorbed to obtain a desorption solution containing iron, praseodymium, neodymium and cobalt; the purity of iron, praseodymium, neodymium and cobalt in the desorption solution containing iron, praseodymium, neodymium and cobalt is greater than or equal to 99.9%.

[0057] In a specific embodiment of the present invention, the adsorption method is preferably dynamic adsorption; the present invention preferably loads the biomass adsorbent into three separation columns respectively to obtain 1#, 2#, and III# separation columns, and then passes the NdFeB leachate through the 1# separation column to obtain 1# effluent; the 1# effluent enters the 2# separation column for adsorption exchange to obtain 2# effluent; the 2# effluent enters the 3# separation column for adsorption exchange to obtain 3# effluent; the end point of the adsorption is preferably: the concentration of iron in the adsorption tail liquid flowing out of the 1# separation column, the concentration of praseodymium and neodymium in the adsorption tail liquid flowing out of the 2# separation column, and the concentration of cobalt in the adsorption tail liquid flowing out of the 3# separation column reach 0.01-1g / L, more preferably 0.1g / L.

[0058] After obtaining the biomass adsorbent loaded with iron, praseodymium, neodymium and cobalt, the present invention respectively performs elution and desorption on the biomass adsorbent loaded with iron, praseodymium, neodymium and cobalt to obtain desorption solutions containing iron, praseodymium, neodymium and cobalt, respectively; the purity of iron, praseodymium, neodymium and cobalt in the desorption solutions containing iron, praseodymium, neodymium and cobalt is greater than or equal to 99.9%. In the present invention, the elution agent for elution is a low-concentration acid; the concentration of the low-concentration acid is preferably 0.01-0.5 mol / L, more preferably 0.1-0.3 mol / L; the low-concentration acid is preferably one or more of hydrochloric acid, sulfuric acid and nitric acid. In a specific embodiment of the present invention, it is preferred to elute the above-mentioned low-concentration acid through the separation column after adsorption; the present invention removes the unadsorbed neodymium iron boron leaching solution on the surface of the biomass adsorbent by elution, and can remove some impurity ions at the same time. The eluent obtained by elution contains some iron, praseodymium, neodymium and cobalt elements. In the present invention, the eluent is preferably used as a raw material solution to continue the adsorption step.

[0059] After elution, the present invention desorbs the washed biomass adsorbent (i.e., 1#, 2#, 3# separation columns), and the desorbent for desorption is preferably a high-concentration acid; the concentration of the high-concentration acid is preferably 0.5-6 mol / L, more preferably 1-5 mol / L; the high-concentration acid is preferably one or more of hydrochloric acid, sulfuric acid, and nitric acid, more preferably hydrochloric acid; in a specific embodiment of the present invention, it is preferred to directly flow the desorbent through the washed separation column for desorption, and the end point of the desorption is preferably based on the concentration of iron, praseodymium, neodymium and cobalt in the outflowing desorption liquid being less than 0.1 g / L. After desorption is completed, the desorbed biomass adsorbent is preferably saponified with conventional ammonia water and then reused.

[0060] The present invention adopts a biomass adsorbent to separate the iron, praseodymium, neodymium and cobalt elements in the NdFeB leachate, and desorption solutions containing iron, praseodymium, neodymium and cobalt can be obtained respectively only through adsorption, elution and desorption, and the process flow is simple and the reagent consumption is small; moreover, the extractant in the biomass adsorbent is fixed in the cellulose in a chemical bonding manner and is not easy to fall off, and the biomass adsorbent can be reused after desorption, thereby reducing the cost of separation and purification.

[0061] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0062] Example 1

[0063] This embodiment discloses a biomass adsorbent, a preparation method thereof, and its use in the field of NdFeB waste recovery, as follows:

[0064] (1) The orange stalks were dried in an oven at 105°C for 2 hours, and then crushed to 30 mesh after cooling. 1000 g of orange stalk powder, 1000 ml of water, 200 g of sodium hydroxide, and 200 ml of hydrogen peroxide were added to a 5 L reactor in sequence, heated to 90°C in a water bath under mechanical stirring, reacted for 2 hours, filtered, rinsed with water until neutral, and dried at 100°C for 2 hours to obtain 560 g of modified biomass.

[0065] 560 g of modified biomass, 200 ml of P507 and 1000 ml of n-heptane were added into a 5 L reactor, refluxed at 60° C. for 2 hours, and then dried at 60° C. for 10 hours to obtain a total of 740 g of biomass adsorbent.

[0066] (2) Take 2000g of NdFeB waste, add 10L of 0.5mol / L dilute HCl solution, stir at 100°C for 6 hours, filter, add solid NaOH to the filtrate to adjust the acidity of the solution to pH=3.0, and obtain 8100ml of NdFeB leaching solution. The iron content in the leaching solution is 3.27g / L, the praseodymium-neodymium content is 1.05g / L, and the cobalt content is 0.72g / L.

[0067] (3) Take 200 g of the biomass adsorbent synthesized in (1), add 20 ml of 10 mol / L ammonia water for saponification; then take 50 g, 50 g, and 20 g of the saponified biomass adsorbent and load them into columns 1#, 2#, and 3#, respectively.

[0068] (4) The NdFeB leachate obtained in step (2) is passed through the 1# column prepared in step (3) at a flow rate of 5 mL / min by a plunger pump, and the iron concentration in the effluent is monitored every 5 minutes. When the iron concentration in the effluent reaches 0.1 g / L, the addition of NdFeB leachate is stopped, and an iron-loaded separation column and 260 ml of iron removal adsorption liquid are obtained respectively. 50 ml of 0.1 mol / L dilute HCl solution is added to the iron-loaded separation column as an eluent at a flow rate of 3 mL / min to obtain an iron-loaded separation column after elution; 50 ml of 5 mol / L HCl solution is added to the iron-loaded separation column as an eluent at a flow rate of 3 mL / min to obtain a desorbed separation column and an iron desorption liquid (iron content is 16.8 g / L, purity is 99.92%). The desorbed separation column can be reused after saponification. Repeat the above steps to prepare 780 ml of iron removal adsorption liquid in total.

[0069] (5) The iron removal adsorption liquid obtained in step (4) is passed through the 2# column prepared in step (3) at a flow rate of 5 mL / min using a plunger pump, and the praseodymium-neodymium concentration in the effluent is monitored by sampling every 5 minutes. When the praseodymium-neodymium concentration in the effluent reaches 0.01 g / L, the addition of the iron removal adsorption liquid is stopped, and a praseodymium-neodymium-loaded separation column and 760 ml of the praseodymium-neodymium removal adsorption liquid are obtained respectively. 50 ml of 0.1 mol / L dilute HCl solution is added as eluent to the praseodymium-neodymium-loaded separation column at a flow rate of 3 mL / min to obtain a washed praseodymium-neodymium-loaded separation column; 50 ml of 5 mol / L HCl solution is added as eluent to the washed iron-loaded separation column at a flow rate of 3 mL / min to obtain a desorbed separation column and a praseodymium-neodymium desorption liquid (the praseodymium-neodymium content is 15.31 g / L and the purity is 99.95%), and the desorbed separation column can be reused after saponification.

[0070] (6) The praseodymium-neodymium removal adsorption liquid obtained in step (5) is passed through the 3# column prepared in step (3) by a plunger pump at a flow rate of 3 mL / min, and the cobalt concentration in the effluent is monitored every 5 minutes. When the cobalt concentration in the effluent reaches 0.01 g / L, the addition of the praseodymium-neodymium removal adsorption liquid is stopped, and a cobalt-loaded separation column and 710 ml of the cobalt-removal adsorption liquid are obtained respectively. 20 ml of a 0.05 mol / L dilute HCl solution is added to the cobalt-loaded separation column as an eluent at a flow rate of 3 mL / min to obtain a praseodymium-loaded neodymium separation column after elution; 20 ml of a 5 mol / L HCl solution is added to the iron-loaded separation column as an eluent at a flow rate of 3 mL / min to obtain a desorbed separation column and a cobalt desorption liquid (cobalt content is 21.06 g / L, purity is 99.93%), and the desorbed separation column can be reused after saponification.

[0071] Example 2

[0072] The biomass adsorbent and its preparation method disclosed in this embodiment are the same as those in Example 1, except that the method of using the biomass adsorbent to recover NdFeB waste is as follows:

[0073] According to the separation steps of Example 1, the biomass adsorbent column after desorption and ammonia saponification in Example 1 was used, and the flow rates of columns 1#, 2#, and 3# were adjusted to 10 ml / min, 10 ml / min, and 5 ml / min, respectively. The penetration point of metal ions in the effluent was adjusted to iron: 0.05 ml / min, 0.05 ml / min, and 0.05 ml / min, respectively. 648 ml of iron removal adsorption liquid, 606 ml of praseodymium-neodymium removal adsorption liquid, and 594 ml of cobalt removal adsorption liquid were obtained; iron desorption liquid (iron content of 14.62 g / L, purity of 99.90%), praseodymium-neodymium desorption liquid (praseodymium-neodymium content of 14.47 g / L, purity of 99.93%), and cobalt desorption liquid (cobalt content of 20.64 g / L, purity of 99.94%) were obtained.

[0074] Example 3

[0075] The biomass adsorbent and its preparation method disclosed in this embodiment are the same as those in Example 1, except that the biomass adsorbent is used to recover NdFeB waste, as follows:

[0076] (1) The method for preparing the NdFeB leachate in Example 1 was adopted, and the leaching acid was adjusted to 0.5 mol / L nitric acid to obtain a total of 8050 ml of NdFeB leachate. The iron content in the leachate was 2.84 g / L, the praseodymium-neodymium content was 1.13 g / L, and the cobalt content was 0.68 g / L.

[0077] (2) Using the method for separating the NdFeB leachate in Example 1, 250 g of the biomass adsorbent prepared in Example 1 was taken, 70 ml of 5.0 mol / L ammonia water was added for saponification, and filtered; then 100 g, 100 g, and 50 g of the saponified biomass adsorbent were taken and loaded into columns 1#, 2#, and 3#, respectively.

[0078] (3) The NdFeB leachate obtained in step (1) is passed through the 1# column prepared in step (2) at a flow rate of 5 mL / min by a plunger pump, and the iron concentration in the effluent is monitored every 5 minutes. When the iron concentration in the effluent reaches 0.01 g / L, the addition of NdFeB leachate is stopped, and an iron-loaded separation column and 480 ml of iron removal adsorption liquid are obtained respectively. 50 ml of 0.05 mol / L dilute nitric acid solution is added to the iron-loaded separation column at a flow rate of 3 mL / min as an eluent to obtain an iron-loaded separation column after elution; 100 ml of 6 mol / L nitric acid solution is added to the iron-loaded separation column after elution as an eluent at a flow rate of 5 mL / min to obtain a separation column after desorption and an iron desorption liquid (iron content is 13.27 g / L, purity is 99.94%). The separation column after desorption can be reused after saponification. Repeat the above steps to prepare 1340 ml of iron removal adsorption liquid in total.

[0079] (4) The iron removal adsorption liquid obtained in step (3) is passed through the 2# column prepared in step (2) at a flow rate of 10 mL / min using a plunger pump, and the praseodymium-neodymium concentration in the effluent is monitored every 5 minutes. When the praseodymium-neodymium concentration in the effluent reaches 0.01 g / L, the addition of the iron removal adsorption liquid is stopped, and a praseodymium-neodymium-loaded separation column and 1260 ml of the praseodymium-neodymium removal adsorption liquid are obtained respectively. 100 ml of 0.1 mol / L dilute nitric acid solution is added as an eluent to the praseodymium-neodymium-loaded separation column at a flow rate of 5 mL / min to obtain a washed praseodymium-neodymium-loaded separation column; 100 ml of 5 mol / L nitric acid solution is added as an eluent to the praseodymium-neodymium-loaded separation column at a flow rate of 2 mL / min to obtain a desorbed separation column and a praseodymium-neodymium desorption solution (the praseodymium-neodymium content is 13.36 g / L and the purity is 99.96%), and the desorbed separation column can be reused after saponification.

[0080] (5) The praseodymium-neodymium removal adsorption liquid obtained in step (4) is passed through the 3# column prepared in step (3) at a flow rate of 10 mL / min by a plunger pump, and the cobalt concentration in the effluent is monitored every 5 minutes. When the cobalt concentration in the effluent reaches 0.01 g / L, the addition of the praseodymium-neodymium removal adsorption liquid is stopped, and a loaded cobalt separation column and 1180 ml of the cobalt removal adsorption liquid are obtained respectively. 50 ml of 0.01 mol / L dilute nitric acid solution is added to the loaded cobalt separation column as an eluent at a flow rate of 2 mL / min to obtain a washed loaded cobalt separation column; 50 ml of 5 mol / L nitric acid solution is added to the washed loaded cobalt separation column as an eluent at a flow rate of 2 mL / min to obtain a desorbed separation column and a cobalt desorption liquid (cobalt content is 18.21 g / L, purity is 99.95%), and the desorbed separation column can be reused after saponification.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a biomass adsorbent, characterized in that: The following steps are involved: Step 1: modifying the biomass: crushing the biomass, adding water, hydrogen peroxide, and sodium hydroxide, heating and digesting to obtain modified cellulose, thereby obtaining the modified biomass; Step 2: The modified biomass, the extractant and the dispersant are mixed, heated and refluxed, and then evaporated and dried to obtain the biomass adsorbent.

2. The method for preparing the biomass adsorbent according to claim 1, characterized in that: The weight ratio of the biomass, water, hydrogen peroxide and sodium hydroxide in step 1 is 1:2-10:0:05-0.5:0.1-1.

3. The method for preparing the biomass adsorbent according to claim 2, characterized in that: The temperature of the heating digestion in step 1 is 50-100° C., and the duration is 0.5-5 hours.

4. The method for preparing the biomass adsorbent according to claim 1, characterized in that: The extractant in step 2 is a mixture of one or more of di(2-ethylhexyl)phosphoric acid, 2-ethylhexylphosphonic acid mono-(2-ethylhexyl) ester and di(2,4,4-trimethylpentyl)phosphonic acid.

5. The method for preparing the biomass adsorbent according to claim 1, characterized in that: In step 2, the weight ratio of the modified biomass, the extractant and the dispersant is 1:0.05-0.5:0.5-5.

6. The method for preparing the biomass adsorbent according to claim 1, characterized in that: The reflux time in step 2 is 0.5 to 10 hours; the evaporation drying temperature is 40 to 80° C. and the time is 0.5 to 10 hours.

7. A biomass adsorbent, characterized in that: Prepared by any one of the methods of claims 1 to 6.

8. Use of the biomass adsorbent according to claim 7 in the field of NdFeB waste recovery.

9. The use according to claim 8, characterized in that: The method for recovering NdFeB waste using the biomass adsorbent comprises the following steps: S1. Leaching the NdFeB waste with acid, and adjusting the acidity of the NdFeB leaching solution to control its pH value to 2.5 to 4.5 to obtain a NdFeB leaching solution; S2. The NdFeB leachate is sequentially passed through a plurality of containers containing biomass adsorbents for step-by-step adsorption to obtain biomass adsorbents loaded with iron, praseodymium, neodymium and cobalt; S3. The biomass adsorbent loaded with iron, praseodymium, neodymium and cobalt is respectively eluted and desorbed to obtain a desorption liquid containing iron, praseodymium, neodymium and cobalt.

10. The use according to claim 9, characterized in that: S1: the acid is a mixture of one or more of nitric acid, hydrochloric acid and sulfuric acid, and the acid concentration is 1 to 10 mol / L; And / or, the eluting agent in S3 is a low-concentration acid; the concentration of the low-concentration acid is 0.01-1 mol / L; the low-concentration acid is a mixture of one or more of nitric acid, hydrochloric acid and sulfuric acid; And / or, the desorbent for desorption in S3 is a high-concentration acid; the concentration of the high-concentration acid is 0.5-6 mol / L; the high-concentration acid is one or more of nitric acid, hydrochloric acid, and sulfuric acid.