Catalyst for synthesis of vinylene carbonate and continuous synthesis method of vinylene carbonate

By using a carrier and a catalyst of active components to perform a gas-phase catalytic dehydrochlorination reaction of vinylene carbonate in a tubular reactor, the problems of high cost and low efficiency in the production of vinylene carbonate in the existing technology are solved, and high purity is achieved and high-efficiency vinylene carbonate production.

CN118719040APending Publication Date: 2024-10-01CHONGQING MINHENG TECH CO LTD

Patent Information

Application Number
CN202410691213.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The industrial production of vinylene carbonate in the existing technology has problems of high cost, low yield and pollution. Especially in the catalytic dehydrochlorination process using chlorinated vinyl carbonate as raw material, it is difficult to achieve high purity and high efficiency production.

Method used

The catalyst is prepared by excessive impregnation method using a carrier such as spherical γ-alumina, spherical silica or HY-5 and active components such as zinc chloride, magnesium chloride and additives such as magnesium hydroxide. The gas-phase catalytic dehydrochlorination reaction is carried out in the reactor to realize the continuous synthesis of vinylene carbonate.

Benefits of technology

The conversion rate of chloroethylene carbonate and the selectivity of vinylene carbonate are improved, high purity (99.996%) and high yield (65-70%) are achieved, the process flow is simplified, and the economic and time costs are reduced. and reduce pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719040A_ABST
    Figure CN118719040A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of synthesis of vinylene carbonate, and particularly relates to a catalyst for synthesis of vinylene carbonate, the catalyst comprises a carrier, an active component and an auxiliary agent, the carrier is one of spherical gamma-aluminum oxide, spherical silicon dioxide, HY-5 and HZSM-5, and the auxiliary agent is one of spherical gamma-aluminum oxide, spherical silicon dioxide, HY-5 and HZSM-5. The active component is at least one of zinc chloride, lithium chloride, nickel chloride, ferric chloride, copper chloride, cuprous chloride and magnesium chloride, and the additive is one of magnesium hydroxide, calcium hydroxide and potassium hydroxide; the dosage of the active component is 5-20% of the sum of the mass of the carrier, the active component and the assistant, and the dosage of the assistant is 0.1-1% of the sum of the mass of the carrier, the active component and the assistant. According to the present invention, the catalyst can be used in the chloroethylene carbonate gas phase catalysis dehydrochlorination reaction to generate the vinylene carbonate so as to achieve the continuous synthesis of the vinylene carbonate, the continuous synthesis method is easy to industrialize, the three wastes are reduced, the safety and the environmental protection are provided, the product yield is stabilized at 65-70%, and the product purity can achieve 99.996%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of vinylene carbonate synthesis, and particularly relates to a catalyst for vinylene carbonate synthesis and a method for continuous synthesis of vinylene carbonate. Background Art

[0002] Vinylene carbonate (VC), also known as 1,3-dioxol-2-one, ethylene carbonate, can be used to prepare photoresists, and can also be used in medical organic polymer materials, enzyme fixation after modification, and intermediates for organic synthesis. In addition, vinylene carbonate can undergo polymerization reaction on the surface of the negative electrode of the battery during the initial charge and discharge of the lithium battery, thereby generating polyalkyl lithium carbonate compounds. The formation of this substance will effectively inhibit the embedding of solvent molecules and the bloating of the lithium battery, which can improve the capacity and cycle life of the battery, and can also effectively prevent the co-insertion reaction between solvent molecules in the electrolyte. Since vinylene carbonate will undergo polymerization reaction, a layer of SEI (solid electrolyte interface) film can be formed on the negative electrode of the battery (graphene type), which will minimize the degree of decomposition of the graphite battery electrolysis, thereby effectively improving the cycle life of the lithium battery. Therefore, vinylene carbonate is currently the most ideal, most effective, and most widely used electrolyte additive and overcharge protection additive.

[0003] With the improvement of various performance requirements of lithium batteries and their further promotion and application, the usage of battery electrolyte additives has also changed significantly, among which the usage ratio of vinylene carbonate has increased significantly. With the popularization of new energy vehicles, vinylene carbonate, as the most used electrolyte additive, will see a rapid increase in market demand. Therefore, it is of great practical significance to study the synthesis route of efficient and green vinylene carbonate.

[0004] At present, the industrial synthesis of vinylene carbonate usually adopts the traditional kettle reaction, that is, ethylene carbonate (EC) is used as the raw material for chlorination reaction to obtain monochloroethylene carbonate (4-chloro-1,3-dioxolan-2-one, CEC), and then CEC and organic amine acid-binding agent (generally triethylamine) are added to organic solvent or in the absence of solvent to undergo elimination reaction to obtain crude vinylene carbonate. This method has cheap and easy-to-obtain raw materials, relatively small environmental pollution, mature process, and mild conditions, but the purity of crude vinylene carbonate is not high, and it needs to be purified by multiple distillations and crystallizations, resulting in a low overall yield of the process. In addition, the traditional kettle reaction has serious self-polymerization, and it is difficult to transfer the tar produced in the reaction process. The amount of triethylamine used is large, and there is no good triethylamine recovery method at home and abroad, resulting in serious pollution of the three wastes of the process. At the same time, the overall production cost of the process is high, about 55,000 yuan / ton, while the current market price of VC is about 65,000 yuan / ton, which seriously compresses the economic benefits of enterprises producing this product. Therefore, developing a green method for synthesizing vinylene carbonate and obtaining safe, environmentally friendly, high-yield, high-purity vinylene carbonate products are currently faced with technical bottlenecks and technical problems that need to be solved urgently.

[0005] Catalytic dehydrogenation with EC as raw material and catalytic dehydrochlorination with CEC as raw material are the two most atom-economical and promising methods for VC synthesis in the future. The invention with application number CN200510048191.X discloses the use of metals and metal oxides as catalysts to catalyze the dehydrogenation of EC to obtain VC; the invention with application number CN202111389822.X discloses adding a certain mass of supported copper-based catalyst, EC and hydrogen acceptor to a reaction device, and carrying out catalytic dehydrogenation-hydrogenation coupling reaction at 200-300°C in a nitrogen atmosphere to prepare vinylene carbonate products; the invention with application number CN200680016151.X discloses that zinc oxide and / or zinc chloride are fixed on silicon dioxide or activated carbon particles, and reacted at 300-600°C in a fixed bed, with a yield of up to 69%. Although both EC catalytic dehydrogenation and CEC catalytic dehydrochlorination have extremely broad development prospects, there are still large technical barriers and industrialization has not yet been achieved. Therefore, it is of great significance to develop a method for synthesizing vinylene carbonate by catalytic dehydrochlorination using CEC as a raw material, which is easy to industrialize. Summary of the invention

[0006] The present invention aims to provide a catalyst for synthesizing vinylene carbonate, so as to solve the problem that it is difficult to industrialize the synthesis of vinylene carbonate by catalytic dehydrochlorination using CEC as a raw material.

[0007] In order to achieve the above-mentioned purpose, the scheme of the present invention is: a catalyst for synthesizing vinylene carbonate, the catalyst comprising a carrier, an active component and an auxiliary agent, the carrier is one of spherical γ-alumina, spherical silica, HY-5 and HZSM-5, the active component is one or more of zinc chloride, lithium chloride, nickel chloride, ferric chloride, cupric chloride, cuprous chloride and magnesium chloride, the auxiliary agent is one of magnesium hydroxide, calcium hydroxide and potassium hydroxide; the amount of the active component is 5-20% of the sum of the mass of the carrier, the active component and the auxiliary agent, and the amount of the auxiliary agent is 0.1-1% of the sum of the mass of the carrier, the active component and the auxiliary agent.

[0008] Optionally, the particle size of the carrier is 1-5 mm.

[0009] Optionally, the carrier is γ-aluminum oxide, the active component is cupric chloride, and the auxiliary agent is magnesium hydroxide.

[0010] Optionally, the amount of the active component is 10% of the total mass of the carrier, the active component and the auxiliary agent, and the amount of the auxiliary agent is 0.1% of the total mass of the carrier, the active component and the auxiliary agent.

[0011] Optionally, the catalyst is prepared by an excess impregnation method, which comprises the following steps:

[0012] S1. Carrier pretreatment: Place the carrier in a muffle furnace and heat it to 450-550°C, then calcine at 450-550°C for 1.5-3h;

[0013] S2. Prepare solution: add active ingredients and auxiliary agents into deionized water, stir evenly, and obtain solution;

[0014] S3, ultrasonic oscillation: adding the carrier calcined in step S1 to the solution in step S2, and ultrasonically oscillating for 2-5 hours;

[0015] S4, frying in water bath to dry: fry the liquid in step S3 in a water bath at 80-90°C to dry;

[0016] S5, drying: placing the sample fried in step S4 in a vacuum drying oven at 105° C. for 12-24 hours to obtain a catalyst precursor;

[0017] S6, calcination: placing the catalyst precursor in step S5 into a muffle furnace and heating it to 400-550° C., and calcining it at a constant temperature of 400-550° C. for 3-5 hours to obtain the catalyst.

[0018] The present invention also provides a method for continuously synthesizing vinylene carbonate, which uses the above catalyst as a catalyst for gas-phase catalytic dehydrochlorination of vinyl chlorocarbonate to generate vinylene carbonate. The method comprises: preheating vinyl chlorocarbonate and nitrogen and passing them into a tubular reactor to catalytically remove hydrogen chloride to obtain vinylene carbonate; wherein the vinyl chlorocarbonate is in gas phase after preheating.

[0019] Optionally, the method comprises the following steps:

[0020] S1. Catalyst filling: loading the catalyst into the tubular reactor to form a catalyst bed in the tubular reactor;

[0021] S2. Gas replacement: introduce nitrogen into the tubular reactor, ensure that the air tightness is intact, and continue to purge until all the air in the tubular reactor is exhausted;

[0022] S3, catalytic reaction: ethylene chlorocarbonate and nitrogen are preheated and introduced into a tubular reactor, and gaseous ethylene chlorocarbonate and nitrogen enter the catalyst bed. The catalytic reaction temperature is 350-500°C, and gaseous ethylene chlorocarbonate is catalytically removed from hydrogen chloride to obtain a mixed gas;

[0023] S4, separation: the mixed gas is cooled to obtain a liquid phase and a non-condensable gas, the liquid phase is flashed to obtain a crude vinylene carbonate product, and the tail gas generated during the flash evaporation of the non-condensable gas and the liquid phase is subjected to water absorption, alkali solution absorption and drying processes to recover nitrogen;

[0024] S5, crude product distillation: the crude vinylene carbonate obtained in step S4 is rapidly distilled out by a high vacuum pump at an oil temperature of 50-75°C and a top temperature of 25-35°C, with a vacuum degree of 300-500Pa, to obtain a distilled product;

[0025] S6, distillation: collecting multiple batches of distillation products obtained in step S5 and mixing them, and distilling them using a thorn-shaped distillation column. The distillation conditions are: oil temperature 60-75°C, kettle temperature 55-65°C, top temperature 34-37°C, vacuum degree 300-500Pa, to obtain a distillation product;

[0026] S7, crystallization: the distillation product obtained in step S6 is statically crystallized at 19°C for 3-4 hours, and then heated to 22-23°C to sweat for 3-4 hours. During the sweating process, sampling and analysis are performed periodically, and the fractions are switched according to the content, and vinylene carbonate products with a content of >99.99% are collected.

[0027] Optionally, in step S4, the crude vinylene carbonate is sampled and weighed every 0.5 h, the conversion rate of vinyl chloride carbonate and the content of each impurity are continuously detected, and the catalyst activity is observed.

[0028] Optionally, in step S3, the feed flow rate of gas-phase chloroethylene carbonate is 2-15 g / min, and the flow rate of nitrogen is 1-4 g / min.

[0029] The beneficial effects achieved by the present invention are:

[0030] 1. The catalyst of the present invention can be used in the reaction of preparing vinylene carbonate by removing hydrogen chloride from vinyl chlorocarbonate in gas phase catalysis, effectively improving the conversion rate of vinyl chlorocarbonate and the selectivity of vinylene carbonate, and has excellent industrial application prospects. Moreover, in the present invention, the yield of vinylene carbonate is stabilized at 65-70%, the purity of vinylene carbonate can reach 99.996%, and the product yield is good and the purity is high.

[0031] 2. The reactants in the present invention pass through the tubular reactor in a continuous flow manner. Therefore, the present invention can achieve efficient heat and mass transfer, thereby improving the production efficiency of vinylene carbonate; furthermore, the reactants can be evenly distributed in the tubular reactor, reducing the variation of the reaction rate and improving the stability of the reaction. In addition, the present invention can achieve precise control of the reaction by precisely controlling the flow rate of the reactants, and monitor key parameters such as temperature and pressure, etc., and automatically control the reaction conditions through feedback control and actuators, reduce reaction temperature fluctuations, avoid local overheating, reduce the generation of by-products, and improve reaction safety. In addition, the continuous flow process can be directly expanded from laboratory scale to industrial scale, simplifying the necessary step-by-step amplification process in traditional intermittent processes, reducing economic costs and time costs, and the present invention is easier to industrialize.

[0032] 3. Compared with the traditional kettle reaction, the reaction of the present invention is carried out continuously and no solvent is used, thus reducing the solvent removal process and simplifying the process; the reaction does not produce solid salt, thus reducing the solid-liquid separation process; the reaction does not involve raw material recovery, thus reducing the investment in the recovery process, thereby reducing the overall investment and reducing the generation of "three wastes", which is more economical and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 1 is a process flow chart of a continuous synthesis method of vinylene carbonate according to an embodiment of the present invention;

[0034] Figure 2 The gas chromatogram of the raw material ethylene chlorocarbonate in the embodiment of the present invention;

[0035] Figure 3 The gas chromatogram of crude vinylene carbonate in the multi-batch continuous reaction stability experiment of the present invention;

[0036] Figure 4 is a gas chromatogram of vinylene carbonate after crude distillation in the present invention;

[0037] Figure 5 is a gas chromatogram of vinylene carbonate after distillation in the present invention;

[0038] Figure 6 is a gas chromatogram of vinylene carbonate after primary crystallization in the present invention;

[0039] Figure 7 It is the gas chromatogram of the finished product vinylene carbonate of the present invention. DETAILED DESCRIPTION

[0040] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0041] The present invention provides a catalyst for synthesizing vinylene carbonate, the catalyst comprising a carrier, an active component and an auxiliary agent, the carrier being one of spherical γ-alumina, spherical silica, HY-5 and HZSM-5, the active component being one or more of zinc chloride, lithium chloride, nickel chloride, ferric chloride, cupric chloride, cuprous chloride and magnesium chloride, and the auxiliary agent being one of magnesium hydroxide, calcium hydroxide and potassium hydroxide; the amount of the active component is 5-20% of the sum of the mass of the carrier, the active component and the auxiliary agent, and the amount of the auxiliary agent is 0.1-1% of the sum of the mass of the carrier, the active component and the auxiliary agent. When the loading amount of the active component is too high, it will cause uneven distribution on the carrier, and the binding ability with the carrier will be weakened. At the same time, too high loading amount will easily cause the active component to fall off during the catalytic process, thereby aggravating the deactivation of the catalyst and shortening the life of the catalyst. On the contrary, if the loading amount of the active component is too low, it cannot meet the demand for active sites in the reaction process, resulting in insufficient catalytic efficiency and poor reaction effect. The above-mentioned active component loading amount is a better range verified by experiments.

[0042] Among them, the particle size of the carrier is 1-5mm, the carrier is preferably γ-aluminum oxide, the active component is preferably cupric chloride, and the auxiliary agent is preferably magnesium hydroxide; the amount of the active component is preferably 10% of the sum of the mass of the carrier, the active component and the auxiliary agent, and the amount of the auxiliary agent is preferably 0.1% of the sum of the mass of the carrier, the active component and the auxiliary agent.

[0043] The catalyst is prepared by an excess impregnation method, which comprises the following steps:

[0044] S1. Carrier pretreatment: Place the carrier in a muffle furnace and heat it to 450-550°C, then calcine at 450-550°C for 1.5-3h.

[0045] S2. Prepare solution: add active components and auxiliary agents into deionized water, stir evenly, and obtain a solution.

[0046] S3, ultrasonic oscillation: adding the carrier calcined in step S1 to the solution in step S2, and ultrasonically oscillating for 2-5 hours.

[0047] S4, frying to dryness in a water bath: frying the liquid in step S3 to dryness in a water bath at 80-90°C.

[0048] S5, drying: the sample fried to dryness in step S4 is placed in a vacuum drying oven at 105° C. for 12-24 hours to obtain a catalyst precursor.

[0049] S6. Calcination: Place the catalyst precursor in step S5 into a muffle furnace and heat it to 400-550° C., and calcine at 400-550° C. for 3-5 hours to obtain a catalyst.

[0050] The present invention also provides a method for continuously synthesizing vinylene carbonate, which uses the above catalyst as a catalyst for the gas-phase catalytic reaction of vinyl chlorocarbonate to generate vinylene carbonate. Specifically, the method comprises the following steps:

[0051] S1. Catalyst filling: loading the catalyst into the tubular reactor to form a catalyst bed in the tubular reactor.

[0052] S2. Gas replacement: Introduce nitrogen into the tubular reactor, ensure that the air tightness is intact, and then continue to purge until all the air in the tubular reactor is exhausted.

[0053] S3. Catalytic reaction: Ethylene chlorocarbonate and nitrogen are preheated and introduced into a tubular reactor, and gaseous ethylene chlorocarbonate and nitrogen enter the catalyst bed. The catalytic reaction temperature is 350-500°C, and gaseous ethylene chlorocarbonate is catalytically removed from hydrogen chloride to obtain a mixed gas; wherein, the feed flow rate of gaseous ethylene chlorocarbonate is 2-15 g / min, and the flow rate of nitrogen is 1-4 g / min.

[0054] S4, separation: after the mixed gas is cooled, a liquid phase and a non-condensable gas are obtained. After the liquid phase is flashed, a crude vinylene carbonate is obtained. The non-condensable gas (HCl, CO2, N2, etc.) and the tail gas (HCl, CO2, etc.) generated during the flash evaporation of the liquid phase are absorbed by water, absorbed by alkaline solution and dried, and the nitrogen is recovered. During this period, the crude vinylene carbonate is sampled and weighed every 0.5h, and the conversion rate of vinyl chloride and the content of each impurity are continuously tested to observe the catalyst activity.

[0055] S5, crude product distillation: the crude vinylene carbonate obtained in step S4 is rapidly distilled out by using a high vacuum pump at an oil temperature of 50-75° C. and a top temperature of 25-35° C., with a vacuum degree of 300-500 Pa, to obtain a distilled product.

[0056] S6, distillation: collect multiple batches of distillation products obtained in step S5 and mix them, and perform distillation using a distillation column. The distillation conditions are: oil temperature 60-75°C, kettle temperature 55-65°C, top temperature 34-37°C, vacuum degree 300-500Pa, to obtain a distillation product.

[0057] S7, crystallization: the distillation product obtained in step S6 is statically crystallized at 19°C for 3-4 hours, and then heated to 22-23°C to sweat for 3-4 hours. During the sweating process, sampling and analysis are performed periodically, and the fractions are switched according to the content, and vinylene carbonate products with a content of >99.99% are collected.

[0058] The following specific examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range according to the description herein, and are not limited to the specific values ​​​​exemplified below.

[0059] Example 1

[0060] This embodiment provides a catalyst for synthesizing vinylene carbonate, which is prepared by an excess impregnation method, specifically comprising the following steps:

[0061] S1. Carrier pretreatment: Place a 1-5 mm spherical γ-alumina carrier in a muffle furnace and heat it to 550°C over 1.5 hours. Roast it at 550°C for 1.5 hours. After the roasting, cool it down to room temperature naturally and take it out for use.

[0062] S2. Prepare solution: accurately weigh 10 g of zinc chloride and dissolve it in 200 g of deionized water, stir evenly to obtain a solution.

[0063] S3. Ultrasonic oscillation: Accurately weigh 90 g of the carrier calcined in step S1, pour it into the solution in step S2, and ultrasonically oscillate for 2 h.

[0064] S4, frying to dryness in a water bath: frying the liquid in step S3 to dryness in a 90°C water bath.

[0065] S5, drying: the sample fried to dryness in step S4 is placed in a vacuum drying oven at 105° C. for 12 h to obtain a catalyst precursor.

[0066] S6, calcination: placing the catalyst precursor in step S5 into a muffle furnace, heating it to 450°C over 3h, calcining it at 450°C for 3h, and naturally cooling it to room temperature after calcination to obtain a catalyst.

[0067] This embodiment also provides a method for continuously synthesizing vinylene carbonate, the process flow of which is as follows: Figure 1 As shown, the specific steps include:

[0068] 1) Catalyst filling: 180 g of catalyst was loaded into a tubular reactor to form a catalyst bed in the tubular reactor. The catalyst was the catalyst for vinylene carbonate synthesis prepared in this example.

[0069] 2) Gas replacement: Open the nitrogen main valve and pressure reducing valve, adjust the nitrogen flow rate to 5L / min through the gas flow controller, check the air tightness of the device, and after ensuring that the air tightness is intact, continue to purge for 20 minutes until all the air in the tubular reactor is exhausted.

[0070] 3) Catalytic reaction: adjust the temperature in the tubular reactor to 420°C (catalytic reaction temperature), start the raw material feed pump, and introduce chloroethylene carbonate (CEC) and nitrogen into the tubular reactor after preheating, wherein the temperature of chloroethylene carbonate after preheating is 200°C, chloroethylene carbonate is in gas phase, and the temperature of nitrogen after preheating is 350°C; the feed flow rate of gaseous chloroethylene carbonate is 4g / min, and the flow rate of nitrogen is 2.92g / min. The gaseous chloroethylene carbonate and nitrogen enter the catalyst bed, and the gaseous chloroethylene carbonate catalytically removes hydrogen chloride to obtain a mixed gas. Among them, the mixed gas mainly consists of a small amount of unreacted chloroethylene carbonate, product vinylene carbonate, hydrogen chloride, nitrogen, a small amount of impurities chloroacetaldehyde and carbon dioxide, etc.

[0071] 4) Separation: After the mixed gas is cooled, a liquid phase and a non-condensable gas are obtained, wherein the liquid phase is flashed to obtain a crude vinylene carbonate, and the tail gas generated during the flash evaporation of the non-condensable gas and the liquid phase is subjected to water absorption, alkaline solution absorption and drying processes to recover nitrogen; during this period, the crude vinylene carbonate is sampled and weighed every 0.5 h, the conversion rate of vinyl chloride and the content of each impurity are continuously tested, and the catalyst activity is observed.

[0072] 5) Crude product distillation: The crude vinylene carbonate obtained in step 4) is rapidly distilled out using a high vacuum pump at an oil temperature of 50-75° C. and a top temperature of 25-35° C. The vacuum degree is 300-500 Pa to obtain a distilled product.

[0073] 6) Distillation: Collect multiple batches of distillation products obtained in step 5) and mix them, and perform distillation using a distillation column. The distillation conditions are: oil temperature 60-75°C, kettle temperature 55-65°C, top temperature 34-37°C, vacuum degree 300-500Pa to obtain a distillation product.

[0074] 7) Crystallization: The distillation product obtained in step 6) is statically crystallized at 19° C. for 3-4 hours, and then heated to 22-23° C. to sweat for 3-4 hours. During the sweating process, sampling and analysis are performed periodically, and the fractions are switched according to the content, and vinylene carbonate products with a content of >99.99% are collected.

[0075] In this embodiment, the conversion rate of chloroethylene carbonate (CEC) is 99.1%, and the selectivity of vinylene carbonate (VC) is 81.7%.

[0076] Example 2

[0077] The difference between this embodiment and embodiment 1 is that in step S1 of this embodiment, the carrier is replaced by spherical silicon dioxide from spherical γ-alumina, and the rest remains unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 57.4%, and the selectivity of vinylene carbonate is 80.8%.

[0078] Example 3

[0079] The difference between this embodiment and embodiment 1 is that in step S1 of this embodiment, the carrier is replaced by HY-5 from spherical γ-alumina, and the rest remains unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 97.4%, and the selectivity of vinylene carbonate is 80.1%.

[0080] Example 4

[0081] The difference between this embodiment and embodiment 1 is that in step S1 of this embodiment, the carrier is replaced by HZSM-5 from spherical γ-alumina, and the rest remains unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 98.2%, and the selectivity of vinylene carbonate is 79.8%.

[0082] Example 5

[0083] The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the active component is replaced by copper chloride from zinc chloride, and the rest remains unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 98.9%, the selectivity of vinylene carbonate is 90.8%, and the catalyst life is 25h.

[0084] Example 6

[0085] The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the active component is replaced by lithium chloride from zinc chloride, and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 50.8%, and the selectivity of vinylene carbonate is 76.8%.

[0086] Example 7

[0087] The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the active component is replaced by nickel chloride from zinc chloride, and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 56.8%, and the selectivity of vinylene carbonate is 70.7%.

[0088] Example 8

[0089] The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the active component is replaced by ferric chloride from zinc chloride, and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 65.8%, and the selectivity of vinylene carbonate is 51.5%.

[0090] Example 9

[0091] The difference between this embodiment and embodiment 1 is that in step S2 of this embodiment, the active component is replaced by magnesium chloride from zinc chloride, and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 49.6%, and the selectivity of vinylene carbonate is 74.5%.

[0092] Example 10

[0093] The difference between this embodiment and embodiment 5 is that step S2 of this embodiment is different from step S2 of embodiment 5. In step S2 of this embodiment, 10 g of copper chloride and 0.1 g of magnesium hydroxide are accurately weighed and dissolved in 200 g of deionized water, and stirred evenly to obtain a solution; in step S3 of this embodiment, 89.9 g of the carrier calcined in step S1 is accurately weighed, and the rest remain unchanged. In this embodiment, the catalyst life is 168 h.

[0094] Embodiment 11

[0095] The difference between this embodiment and embodiment 10 is that in step S2 of this embodiment, the auxiliary agent is replaced by calcium hydroxide instead of magnesium hydroxide, and the rest remains unchanged. In this embodiment, the catalyst life is 109 hours.

[0096] Example 12

[0097] The difference between this embodiment and embodiment 10 is that in step S2 of this embodiment, the auxiliary agent is replaced by potassium hydroxide instead of magnesium hydroxide, and the rest remains unchanged. In this embodiment, the catalyst life is 79 hours.

[0098] Embodiment 13

[0099] The difference between this embodiment and embodiment 10 is that in step S6 of this embodiment, the calcination temperature is 550° C., and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 97.4%, the selectivity of vinylene carbonate is 90.8%, and the catalyst life is 104 hours.

[0100] Embodiment 14

[0101] The difference between this embodiment and embodiment 10 is that in step S6 of this embodiment, the calcination temperature is 350° C., and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 50.0%, the selectivity of vinylene carbonate is 20.0%, and the catalyst life is 24 hours.

[0102] Embodiment 15

[0103] The difference between the present embodiment and embodiment 10 is only that: the parameters in the vinylene carbonate continuous synthesis method in the present embodiment are different, and in the step 3) of the present embodiment, the feed flow rate of gas phase chloroethylene carbonate is 2g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion is 98.9%, and the vinylene carbonate selectivity is 87.8%.

[0104] Example 16

[0105] The difference between the present embodiment and embodiment 10 is only that: the parameters in the vinylene carbonate continuous synthesis method in the present embodiment are different, and in the step 3) of the present embodiment, the feed flow rate of gas phase chloroethylene carbonate is 6g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion is 90.51%, and the vinylene carbonate selectivity is 90.1%.

[0106] Embodiment 17

[0107] The difference between the present embodiment and embodiment 10 is only that: the parameters in the vinylene carbonate continuous synthesis method in the present embodiment are different, and in the step 3) of the present embodiment, the feed flow rate of gas phase chloroethylene carbonate is 15g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion is 71.8%, and the vinylene carbonate selectivity is 90.5%.

[0108] Embodiment 18

[0109] The difference between the present embodiment and embodiment 10 is that the parameters in the continuous synthesis method of vinylene carbonate in the present embodiment are different. In step 3) of the present embodiment, the nitrogen flow rate is 1g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion is 100%, and the vinylene carbonate selectivity is 71.1%.

[0110] Embodiment 19

[0111] The difference between the present embodiment and embodiment 10 is only that: the parameters in the vinylene carbonate continuous synthesis method in the present embodiment are different, and in the step 3) of the present embodiment, the nitrogen flow rate is 3.5g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion is 75.8%, and the vinylene carbonate selectivity is 90.8%.

[0112] Embodiment 20

[0113] The difference between the present embodiment and embodiment 10 is only that: the parameters in the vinylene carbonate continuous synthesis method in the present embodiment are different, and in the step 3) of the present embodiment, the nitrogen flow rate is 4g / min, and all the other are unchanged. In the present embodiment, the chloroethylene carbonate conversion rate is 51.1%, and the vinylene carbonate selectivity is 90.24%.

[0114] Embodiment 21

[0115] The difference between this embodiment and embodiment 10 is that the parameters in the continuous synthesis method of vinylene carbonate in this embodiment are different. In step 3) of this embodiment, the catalytic reaction temperature is 350° C., and the rest remain unchanged. In this embodiment, the conversion rate of vinyl chlorocarbonate is 90.4%, and the selectivity of vinylene carbonate is 90.1%.

[0116] Embodiment 22

[0117] The difference between this embodiment and embodiment 10 is that the parameters in the continuous synthesis method of vinylene carbonate in this embodiment are different. In step 3) of this embodiment, the catalytic reaction temperature is 450° C., and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 100%, and the selectivity of vinylene carbonate is 84.1%.

[0118] Embodiment 23

[0119] The difference between this embodiment and embodiment 10 is that the parameters in the continuous synthesis method of vinylene carbonate in this embodiment are different. In step 3) of this embodiment, the catalytic reaction temperature is 500° C., and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 100%, and the selectivity of vinylene carbonate is 70.05%.

[0120] Comparative Example 1

[0121] The difference between this comparative example and Example 5 is that in step S1 of this comparative example, the carrier is replaced by fruit shell activated carbon from spherical γ-alumina, and the rest remains unchanged. In this example, the conversion rate of chloroethylene carbonate is 50.0%, and the selectivity of vinylene carbonate is 76.9%.

[0122] Comparative Example 2

[0123] The difference between this comparative example and Example 5 is that in step S1 of this comparative example, the carrier is replaced by fluorinated graphite from spherical γ-alumina, and the rest remains unchanged. In this example, the conversion rate of chloroethylene carbonate is 49.8%, and the selectivity of vinylene carbonate is 78.7%.

[0124] Comparative Example 3

[0125] The difference between this comparative example and Example 1 is that in step S2 of this example, the active component is replaced by potassium chloride from copper chloride, and the rest remains unchanged. In this example, the catalyst is inactive.

[0126] Comparative Example 4

[0127] The difference between this comparative example and Example 10 is that in step S2 of this example, the auxiliary agent is replaced by sodium hydroxide instead of magnesium hydroxide, and the rest remains unchanged. In this example, the catalyst life is 24 hours.

[0128] Comparative Example 5

[0129] The difference between this embodiment and embodiment 10 is that in step S6 of this embodiment, the calcination temperature is 250° C., and the rest remain unchanged. In this embodiment, the conversion rate of chloroethylene carbonate is 30.4%, the selectivity of vinylene carbonate is 5.4%, and the catalyst is rapidly deactivated.

[0130] The catalyst components, parameters of the continuous synthesis method of vinylene carbonate, conversion rate of vinyl chloride carbonate, selectivity of vinylene carbonate and catalyst life in Examples 1-23 and Comparative Examples 1-5 are summarized in Table 1.

[0131] Table 1 Parameters and data results of each embodiment and each comparative example

[0132]

[0133]

[0134]

[0135] As can be seen from Table 1, by comparing Examples 1-4 and Comparative Examples 1-2, it can be intuitively seen that γ-Al2O3, HY-5 and HZSM-5 are carriers with Lewis acid active centers, have higher conversion rates in the catalytic dehydrochlorination reaction of vinyl chloride carbonate, and have almost the same selectivity for vinylene carbonate. On the whole, γ-Al2O3 can be selected as the carrier.

[0136] Comparing Example 1, Example 5-9 and Comparative Example 3, it can be seen that when gas-phase chloroethylene carbonate is catalyzed to dehydrochlorinate, transition metal or alkaline earth metal chloride is used as the active component, all of which have catalytic activity and can catalyze the reaction. From the above results, it can be seen that the selectivity of +1 and +2 valence metal catalyzed dehydrochlorination is higher (except potassium chloride), and the selectivity of +3 valence metal to dehydrochlorination is lower. Among them, when CuCl2 is the active component, the catalyst selectivity is the highest.

[0137] By comparing Example 5, Examples 10-12 and Comparative Example 4, it can be seen that when the auxiliary agent is Mg(OH)2, the life of the catalyst can be significantly extended.

[0138] By comparing Example 10, Examples 13-14 and Comparative Example 5, it can be seen that the calcination temperature has a great influence on the conversion rate of vinyl chloride carbonate, the selectivity of vinyl carbonate and the life of the catalyst itself. When the calcination temperature is ≥450°C, the conversion rate of vinyl chloride carbonate and the selectivity of vinyl carbonate are both high, but when the calcination temperature is too high, the life of the catalyst is shortened; when the calcination temperature is too low, the binding ability between the active component and the carrier is weak, the active component of the catalyst is easy to lose, and the catalyst activity is low, so the appropriate calcination temperature is 450°C.

[0139] By comparing Example 10 with Examples 15-17, it can be seen that the optimal feed flow rate of CEC is 4 g / min, at which time the conversion rate of CEC is 98.9% and the selectivity of VC is 90.8%.

[0140] By comparing Example 10 and Examples 18-20, it can be seen that as the nitrogen flow rate increases, the conversion rate of chloroethylene carbonate gradually decreases. When the nitrogen flow rate is too low, the generated product vinyl carbonate stays in the bed for a long time and is easy to decompose, and the solid selectivity decreases; when the nitrogen flow rate is high, the conversion rate of chloroethylene carbonate is low but does not affect the selectivity of vinyl carbonate. In summary, the optimal flow rate of nitrogen is 2.92g / min.

[0141] By comparing Example 10 and Examples 21-23, it can be seen that as the reaction temperature increases, the conversion rate of vinyl chloride carbonate gradually increases, but the selectivity of vinylene carbonate gradually decreases. Overall, the optimal reaction temperature is 420°C.

[0142] Stability test

[0143] To verify the stability of the continuous synthesis method of the present invention, Table 2 shows the stability experimental data of multiple batches of continuous reactions, wherein each batch of feed is 500 g, and the content of feed CEC is 80%. The gas chromatogram of the raw material CEC is as follows: Figure 2 As shown, the gas chromatogram of crude vinylene carbonate is as follows Figure 3 shown.

[0144] Table 2 Results of multiple batches of continuous reaction stability experiments

[0145] batch Feed amount (g) Output (g) VC content (%) Discount rate (%) Batch 1 500 251.56 72.6 65.0 Batch 2 500 278.6 71.8 71.2 Batch 3 500 295.5 70.7 65.3 Batch 4 500 256.4 73.1 66.7 Batch 5 500 267.2 69.8 66.4 Batch 6 500 271.28 72.4 69.9 Batch 7 500 279.38 70.4 70.0 Batch 8 500 257.4 71.5 65.5 Batch 9 500 261.1 72.2 67.0 Batch 10 500 255.6 72.1 65.6

[0146] Each batch of products was crudely steamed, and the data after crude steaming are shown in Table 3. The gas chromatogram of vinylene carbonate after crude steaming is shown in Figure 4 shown.

[0147] Table 3 Results of multiple batches of continuous reaction crude steaming experiments

[0148] batch Feed amount (g) Output (g) VC content (%) Crude steam yield (%) Batch 1 251.56 178.68 92.4 90.4 Batch 2 278.6 192.30 93.1 89.5 Batch 3 295.5 203.5 92.5 90.1 Batch 4 256.4 182.8 93.5 91.2 Batch 5 267.2 182.49 92.8 90.8 Batch 6 271.28 191.75 92.7 90.5 Batch 7 279.38 193.28 92.5 90.9 Batch 8 257.4 179.28 92.9 90.5 Batch 9 261.1 184.38 92.23 90.5 Batch 10 255.6 179.7 92.4 90.1

[0149] Each batch of products was distilled separately. The data after distillation are shown in Table 4. The gas chromatogram of vinylene carbonate after distillation is shown in Table 4. Figure 5 shown.

[0150] Table 4 Results of multiple batches of continuous reactive distillation experiments

[0151] batch Feed amount (g) Output (g) VC content (%) Distillation yield (%) Batch 1 178.68 153.09 99.0 91.8 Batch 2 192.30 166.39 99.1 92.1 Batch 3 203.5 174.39 99.2 91.9 Batch 4 182.8 159.7 99.0 92.5 Batch 5 182.49 156.55 99.2 91.7 Batch 6 191.75 165.18 99.0 92.0 Batch 7 193.28 166.32 99.0 92.1 Batch 8 179.28 154.14 99.3 91.9 Batch 9 184.38 157.99 99.1 91.9 Batch 10 179.7 153.84 99.3 92.0

[0152] The above 10 batches of distilled vinylene carbonate products were combined into 2 batches (batches 1-5 were combined into the first batch, and batches 6-10 were combined into the second batch). The two batches of products were subjected to two static crystallizations. The results are shown in Tables 5 and 6. The gas chromatogram of vinylene carbonate after the first crystallization is as follows: Figure 6 As shown, the gas chromatogram of vinylene carbonate after the second crystallization is as follows Figure 7 shown.

[0153] Table 5. Results of a static crystallization data

[0154]

[0155] Table 6 Secondary static crystallization data results

[0156]

[0157] A total of 10 batches of stability experiments were conducted this time, with 500g of feed in each batch. After reaction, crude steaming, distillation and static crystallization, a product with a content of 99.996% and a moisture content of 8-10ppm was obtained, which is higher than the implementation standard. The pilot process achieved the expected indicators:

[0158] Reaction: The CEC feed content is 80%, the yield after the reaction is stable at 65-70%, and the content of the crude vinylene carbonate is about 70-72%.

[0159] Rough distillation: After distillation of crude VC with a content of 70-72%, VC with a content of 92% can be obtained, and the distillation yield is about 90%.

[0160] Distillation: After distillation of 92% VC, about 99% VC can be obtained, and the distillation yield is about 92%.

[0161] Static crystallization: the first crystallization is purified from 99% to 99.95%, with a one-way yield of about 55%; the second crystallization is purified from 99.95% to 99.996%, with a one-way yield of about 50%, and the cycle yield of the crystallization process is >95%.

[0162] The above are only embodiments of the present invention. The invention is not limited to the fields involved in this implementation case. The common sense such as the known specific structures and characteristics in the scheme is not described in detail here. The ordinary technicians in the relevant field know all the common technical knowledge in the technical field to which the invention belongs before the application date or priority date, can obtain all the existing technologies in the field, and have the ability to apply the conventional experimental means before that date. The ordinary technicians in the relevant field can improve and implement this scheme in combination with their own abilities under the enlightenment given by this application. Some typical known structures or known methods should not become obstacles for ordinary technicians in the relevant field to implement this application. It should be pointed out that for those skilled in the art, without departing from the structure of the present invention, several deformations and improvements can be made, which should also be regarded as the protection scope of the present invention, which will not affect the effect of the implementation of the present invention and the practicality of the present invention. The protection scope required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to explain the content of the claims.

Claims

1. A catalyst for the synthesis of vinylene carbonate, Features: The catalyst comprises a carrier, an active component and an auxiliary agent, wherein the carrier is one of spherical γ-alumina, spherical silicon dioxide, HY-5 and HZSM-5, the active component is one or more of zinc chloride, lithium chloride, nickel chloride, ferric chloride, cupric chloride, cuprous chloride and magnesium chloride, and the auxiliary agent is one of magnesium hydroxide, calcium hydroxide and potassium hydroxide; the amount of the active component is 5-20% of the total mass of the carrier, the active component and the auxiliary agent, and the amount of the auxiliary agent is 0.1-1% of the total mass of the carrier, the active component and the auxiliary agent.

2. The vinylene carbonate synthesis catalyst according to claim 1, Features: The particle size of the carrier is 1-5 mm.

3. The vinylene carbonate synthesis catalyst according to claim 1, Features: The carrier is gamma-aluminum oxide, the active component is cupric chloride, and the auxiliary agent is magnesium hydroxide.

4. The vinylene carbonate synthesis catalyst according to claim 1, Features: The dosage of the active component is 10% of the total mass of the carrier, the active component and the auxiliary agent, and the dosage of the auxiliary agent is 0.1% of the total mass of the carrier, the active component and the auxiliary agent.

5. The vinylene carbonate synthesis catalyst according to claim 1, Features: The catalyst is prepared by an excess impregnation method, which comprises the following steps: S1. Carrier pretreatment: Place the carrier in a muffle furnace and heat it to 450-550°C, then calcine at 450-550°C for 1.5-3h; S2. Prepare solution: add active ingredients and auxiliary agents into deionized water, stir evenly, and obtain solution; S3, ultrasonic oscillation: adding the carrier calcined in step S1 to the solution in step S2, and ultrasonically oscillating for 2-5 hours; S4, frying in water bath to dry: fry the liquid in step S3 in a water bath at 80-90°C to dry; S5, drying: placing the sample fried in step S4 in a vacuum drying oven at 105° C. for 12-24 hours to obtain a catalyst precursor; S6, calcination: placing the catalyst precursor in step S5 into a muffle furnace and heating it to 400-550° C., and calcining it at a constant temperature of 400-550° C. for 3-5 hours to obtain the catalyst.

6. A method for continuous synthesis of vinylene carbonate, Features: The catalyst for synthesizing vinylene carbonate as claimed in any one of claims 1 to 5 is used as a catalyst for the gas phase catalytic dehydrochlorination reaction of vinyl chlorocarbonate to produce vinylene carbonate.

7. The method for continuous synthesis of vinylene carbonate according to claim 6, Features: The method comprises: preheating chloroethylene carbonate and nitrogen and then passing them into a tubular reactor to catalytically remove hydrogen chloride to obtain vinylene carbonate; wherein the chloroethylene carbonate is in gas phase after being preheated.

8. The method for continuous synthesis of vinylene carbonate according to claim 7, Features: The method comprises the following steps: S1. Catalyst filling: loading the catalyst into the tubular reactor to form a catalyst bed in the tubular reactor; S2. Gas replacement: introduce nitrogen into the tubular reactor, ensure that the air tightness is intact, and continue to purge until all the air in the tubular reactor is exhausted; S3, catalytic reaction: ethylene chlorocarbonate and nitrogen are preheated and introduced into a tubular reactor, and gaseous ethylene chlorocarbonate and nitrogen enter the catalyst bed. The catalytic reaction temperature is 350-500°C, and gaseous ethylene chlorocarbonate is catalytically removed from hydrogen chloride to obtain a mixed gas; S4, separation: the mixed gas is cooled to obtain a liquid phase and a non-condensable gas, the liquid phase is flashed to obtain a crude vinylene carbonate product, and the tail gas generated during the flash evaporation of the non-condensable gas and the liquid phase is subjected to water absorption, alkali solution absorption and drying processes to recover nitrogen; S5, crude product distillation: the crude vinylene carbonate obtained in step S4 is rapidly distilled out by a high vacuum pump at an oil temperature of 50-75°C and a top temperature of 25-35°C, with a vacuum degree of 300-500Pa, to obtain a distilled product; S6, distillation: collecting multiple batches of distillation products obtained in step S5 and mixing them, and distilling them using a thorn-shaped distillation column. The distillation conditions are: oil temperature 60-75°C, kettle temperature 55-65°C, top temperature 34-37°C, vacuum degree 300-500Pa, to obtain a distillation product; S7, crystallization: the distillation product obtained in step S6 is statically crystallized at 19°C for 3-4 hours, and then heated to 22-23°C to sweat for 3-4 hours. During the sweating process, sampling and analysis are performed periodically, and the fractions are switched according to the content, and vinylene carbonate products with a content of >99.99% are collected.

9. The method for continuous synthesis of vinylene carbonate according to claim 8, Features: In step S4, the crude vinylene carbonate is sampled and weighed every 0.5 h, the conversion rate of vinyl chloride carbonate and the content of each impurity are continuously detected, and the catalyst activity is observed.

10. The method for continuous synthesis of vinylene carbonate according to claim 7 or 8, Features: In step S3, the feed flow rate of gas-phase chloroethylene carbonate is 2-15 g / min, and the flow rate of nitrogen is 1-4 g / min.

Citation Information

Patent Citations

  • Process for producing vinylene carbonate

    CN101175742A

  • Catalyst for gas phase catalytic cracking of 1,1,2-trichloroethane to prepare cis-1,2-dichloroethene and preparation method thereof

    CN104785233A

  • Solid catalyst for liquid-phase synthesis of vinylene carbonate as well as preparation method and application of solid catalyst

    CN114797957A

  • Synthesis method of vinylene carbonate

    CN116693494A

  • Method for preparing vinylene carbonate without solvent

    CN117402134A

Cited By

  • Catalyst for synthesizing vinylene carbonate as well as preparation method and application of catalyst