Preparation method of hair-ball-shaped hollow bismuth trioxide / carbon microspheres as well as product and application of hair-ball-shaped hollow bismuth trioxide / carbon microspheres
By using an ultra-low temperature crystallization method to prepare hollow carbon microspheres in a photocatalyst and combining it with a hydrothermal method to form hairy spherical hollow bismuth trioxide/carbon microspheres, the problem of small specific surface area of existing photocatalysts is solved and efficient organic dyes are achieved Wastewater degradation.
Patent Information
- Application Number
- CN202410767892.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-01
AI Technical Summary
Existing photocatalysts such as Fe2O3 and WO3 have small specific surface areas and few mesopores, resulting in low catalytic mass transfer efficiency, slow reactions and few cycles, making it difficult to efficiently treat organic dye wastewater.
Hollow carbon microspheres were prepared using ultra-low temperature crystallization method, and hairy spherical hollow bismuth trioxide/carbon microspheres were synthesized through hydrothermal method. Their huge specific surface area and "hole" effect were used to improve the photocatalytic activity of the catalyst.
The photocatalytic degradation activity of the two dyes is significantly improved. The degradation rate of methylene blue reaches 99% within 140 minutes, and the catalytic reaction time is shortened.
Smart Images

Figure CN118719043A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite microsphere preparation, and relates to a preparation method of hairy hollow bismuth trioxide / carbon microspheres, and products and applications thereof. Background Art
[0002] With the rapid development of human society and science and technology, organic wastewater is increasing day by day. Organic wastewater has the following characteristics: (1) Toxicity. Endangering human life and safety; (2) Consuming a large amount of oxygen. Organic wastewater contains a large amount of organic matter such as protein and cellulose. The process of microbial decomposition of organic matter requires the consumption of a large amount of dissolved oxygen in the water, causing the death of aquatic animals such as fish; (3) High stability. Organic pollutants have complex structures, many of which cannot be decomposed by microorganisms and will remain stable in water for a long time. Researching effective treatment methods has become a top priority, but several commonly used methods have obvious disadvantages. For example, the physical adsorption method has the disadvantages of high cost and easy secondary pollution; microorganisms can only treat one or several other organic dye wastewaters with similar properties, the cultivation cost is relatively high, the labor cost is high, and they need to be cultivated from scratch after death; the disadvantages of electrochemical electrolysis are high power consumption and high cost; photocatalytic oxidation refers to a new oxidation technology that uses highly active hydroxyl radicals (OH) generated by photocatalysts in the reaction system to degrade pollutants into small molecules, which is considered to be the most promising technology. Photocatalytic technology is a green, low-carbon, environmentally friendly and energy-saving technology. It can use sunlight as a power source and has the advantages of good photodegradation effect, mild reaction conditions and low economic cost. Fe2O3 and WO3 are widely used degradation catalysts, most of which are in amorphous state, with embedded catalytic sites and no catalytic effect inside. They have small specific surface area and no mesopores in the materials, and the catalytic degradation efficiency needs to be further improved.
[0003] In addition, Bi2O3 is a typical P-type semiconductor with narrow band gap, non-toxicity and low cost, and has been proven to be a suitable photocatalyst, which can be applied to organic dye wastewater treatment, photocatalytic water splitting hydrogen production and gas sensors. However, it has problems such as irregular morphology, small specific surface area, no pores, and catalytic site embedding, and has low efficiency in organic wastewater and photocatalytic water splitting hydrogen production.
[0004] Therefore, it is necessary to study bismuth trioxide (Bi2O3 / C)-based catalysts with larger specific surface area and higher catalytic activity. Summary of the invention
[0005] In order to overcome the deficiencies of the above-mentioned prior art, the present invention provides a hairy hollow bismuth trioxide / carbon microsphere (Bi2O3 / C microsphere) to solve the problems of low catalytic mass transfer efficiency, slow reaction and few cycles due to small specific surface area of the catalyst and few mesopores in the photocatalytic process. Compared with nanomaterials such as pure Fe2O3 and WO3, the photocatalytic degradation activity of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) for both dyes has been greatly improved. The reason for the enhanced photocatalytic performance of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) is that the hairy balls provide a huge specific surface area for Bi2O3 to attach, and a large amount of attached Bi2O3 has a better energy band structure than Fe2O3 and WO3, a strong light absorption ability and a "hole" effect, which produces hydroxyl radicals, and the combination forms a catalytic degradation scheme. Through experiments, we can see that as the irradiation time gradually increases, the concentration of methylene blue (MB) molecules in the solution decreases significantly. When the irradiation time reaches 140 minutes, the degradation rate of MB is nearly 99%, and the mixed aqueous solution also changes from blue to colorless and transparent. The degradation is complete and can be used for water remediation using sunlight.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] 1. A method for preparing hairy hollow bismuth trioxide / carbon microspheres, the preparation method comprising the following steps:
[0008] (1) hollow carbon microspheres are prepared by ultra-low temperature crystallization method: under the condition of vacuum and nitrogen, initiator, polymerization monomer, cross-linking agent, deoxyethanol solution, acrylic acid and pre-ultrasonicated deionized water are mixed, heated for polymerization and then placed in liquid nitrogen for freezing, and the emulsion is completely crystallized, vacuumed and then returned to room temperature for centrifugation and air drying, and then cooled after carbonization to obtain hollow carbon microspheres;
[0009] (2) Preparing hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) by a hydrothermal method: placing the hollow carbon microspheres in a mixture of anhydrous ethanol and deionized water, adjusting the pH to 10, adding bismuth citrate to carry out a hydrothermal reaction in a reactor, cooling, washing and drying to obtain hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres).
[0010] Preferably, the initiator in step (1) is potassium persulfate or azobisisobutyramidine hydrochloride.
[0011] Preferably, in step (1), the polymerizable monomer is styrene, ethylene glycol dimethacrylate (EGDMA) or acrylic acid;
[0012] The polymerizable monomer is a mixture formed by mixing styrene, ethylene glycol dimethacrylate (EGDMA) and acrylic acid in a molar ratio of 2.0-9.0:0.1-0.5:20.0-35.0.
[0013] Preferably, in step (1), the cross-linking agent is ethylene glycol dimethacrylate (EGDMA) or p-vinylbenzene.
[0014] Preferably, in step (1), the volume ratio of deoxyethanol to deionized water in the deoxyethanol solution is 4-25:100-300.
[0015] Preferably, in step (2), triethylamine or ammonia water is used to adjust the pH during the pH adjustment process, wherein the dropping speed is 1 to 3 d / s;
[0016] The hydrothermal reaction is specifically: hydrothermal reaction at 180-200° C. for 24-36 hours.
[0017] Preferably, in step (2), the mass ratio of the hollow carbon microspheres to bismuth citrate is 0.1-0.15:1.0-1.5.
[0018] 2. The hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared according to the above preparation method.
[0019] Preferably, the diameter of the hairy hollow bismuth trioxide / carbon microspheres is 232±30 nm, the hollow diameter is 180-200 nm, and the pore size distribution is between 2 and 60 nm.
[0020] 3. Application of the above-mentioned hairy hollow bismuth trioxide / carbon microspheres in photocatalytic degradation of methylene blue.
[0021] The beneficial effects of the present invention are:
[0022] 1. The present invention discloses a method for preparing hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres), which mainly comprises first preparing hollow carbon microspheres by ultra-low temperature crystallization, and then preparing hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) by hydrothermal method. The preparation method of the present invention is simple to operate, and the prepared hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) use bismuth citrate as a bismuth source and hollow porous hairy carbon balls with a large specific surface area as carriers. Ultra-low temperature crystallization and hydrothermal method are used to synthesize "hairy" hollow Bi2O3 / C microspheres with unique morphology. Due to the "hole" effect, hydroxyl radicals are generated, which can be used for photocatalytic degradation.
[0023] 2. The hairy ball-shaped hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared by the present invention use hollow carbon balls as templates, and synthesize a "hairy ball"-shaped hollow structure Bi2O3 / C microsphere with a large specific surface area through low-temperature crystallization and hydrothermal methods. This special structure effectively increases the surface area of Bi2O3, allowing the carbon balls to attach more Bi2O3, and the hollow structure is conducive to the rapid embedding and crystallization of bismuth ions, effectively shortening the transmission path of lithium ions. When the "hairy ball"-shaped hollow Bi2O3 / C microspheres are used as photocatalytic materials, they have a higher initial surface area than pure Bi2O3, and have a more efficient effect in catalytic degradation of pollution.
[0024] 3. The present invention also discloses the application of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared by the present invention in the photocatalytic degradation of methylene blue (MB). The hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) have the highest photodegradation activity, showing better photocatalytic performance than carbon spheres (3%, 140 min) and Bi2O3 (10%, 140 min). Under simulated visible light, the concentration of 50 mg / L MB was reduced by 99% within 140 min.
[0025] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0027] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0028] Figure 1 The present invention is a flow chart of the preparation of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres);
[0029] Figure 2 The SEM image of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1;
[0030] Figure 3 TEM image of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1;
[0031] Figure 4XRD comparison diagram of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1, Bi2O3 and tetragonal Bi2O3 (PDF#74-1374) standard cards;
[0032] Figure 5 The test graph of the specific surface area of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) and Bi2O3 prepared in Example 1;
[0033] Figure 6 The pore size distribution diagram of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1;
[0034] Figure 7 The Raman spectrum of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1;
[0035] Figure 8 A comparison of the degradation of methylene blue by the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres), carbon spheres and Bi2O3 prepared in Example 1;
[0036] Fig. 9 This is the UV-visible absorption spectrum of the degradation of methylene blue by hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) within a certain reaction time. DETAILED DESCRIPTION
[0037] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied by other different specific embodiments, and the details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that, in the absence of conflict, the features in the following embodiments and embodiments can be combined with each other. In the following embodiments, unless otherwise specified, the experimental methods used are all conventional methods, and the materials, reagents, etc. used can be purchased by chemical reagent companies.
[0038] Example 1
[0039] A hairy hollow bismuth trioxide / carbon microsphere (Bi2O3 / C microsphere), the specific preparation method is as follows:
[0040] (1) Hollow carbon microspheres were prepared by ultra-low temperature crystallization method: 0.1 g potassium persulfate (0.38 mmol, 0.4 mol%) was added to a 250 mL three-necked flask, and the evacuation was vented with nitrogen. After replacement three times, 10 mL styrene (8.8 mmol), 4 mL ethylene glycol dimethacrylate (EGDMA) (60 mg, 0.3 mmol), 30 mL deoxyethanol solution (volume concentration of 20%), 2.0 mL acrylic acid (29.2 mmol) and 150 mL pre-ultrasonicated Deionized water, the temperature was raised to 85°C and stirred for 36 hours, then the reaction was stopped; after centrifugation for 8 minutes, it was washed three times with deionized water and ethanol in sequence to obtain an emulsion; it was placed in a reaction tube with a vacuum port, frozen in liquid nitrogen for 20 minutes, and after the emulsion was completely crystallized, it was vacuumed for 4 hours, restored to room temperature, normal pressure, and centrifuged to dry naturally to obtain a white powder; the air-dried white powder was placed in a muffle furnace, under the protection of a nitrogen atmosphere, the heating rate was controlled to be 3°C / min, the temperature was raised to 500°C, and then kept warm for 3 hours, and hollow carbon microspheres were obtained by cooling.
[0041] (2) Preparation of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) by a hydrothermal method: 50 mL of anhydrous ethanol and 25 mL of deionized water were injected into a flask with a magnet, ultrasonicated for 3 min, and then 120 mg of the hollow carbon microspheres prepared above were added after stirring. 5 mL of triethylamine was added dropwise to adjust the pH of the solution to 10. After stirring for 30 min, 1.2 g of bismuth citrate was added to obtain a black suspension. After stirring for 2 h, the suspension was transferred to a 100 mL reactor and subjected to a hydrothermal reaction at 200 °C for 24 h. After cooling, the product of the hydrothermal reaction was filtered until the solution was neutral. The product was washed with deionized water (50 mL×3) and ethanol (50 mL×3) once, and dried in a vacuum at 50 °C to obtain hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres).
[0042] Embodiments 2 to 6
[0043] The implementation method and synthesis conditions are the same as those in Example 1, except that the polymerization monomer in Example 1 is changed from "styrene" to a polymerization monomer formed by styrene, EGDMA, and acrylic acid in molar ratios of 4.4:0.5:24.6, 2.2:0.25:24.6, 9.0:0.1:20.0, 2.0:0.1:24.6, and 2.0:0.5:35.0, respectively.
[0044] Embodiments 7 to 9
[0045] The implementation method and synthesis conditions are the same as those in Example 1, except that the volume ratios of deoxyethanol and deionized water in the deoxyethanol solution in Example 1 are changed to 4:300, 25:100, and 20:300, respectively.
[0046] Embodiments 10 to 11
[0047] The implementation method and synthesis conditions are the same as those in Example 1, except that the mass ratios of hollow carbon microspheres and bismuth citrate in Example 1 are changed to 0.1:1.5 and 0.15:1.0, respectively.
[0048] Performance Testing
[0049] Figure 1 The present invention is a flow chart for the preparation of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres).
[0050] Figure 2 and Figure 3 The SEM and TEM images of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1 are shown respectively. Figure 2 and Figure 3 It can be seen that the size distribution of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1 is 232±30nm, the inside is hollow, and the outer layer has many crystalline burrs, indicating that the hydrothermal method allows Bi2O3 to successfully attach to the surface of the carbon sphere and crystallize.
[0051] Figure 4 The XRD comparison diagram of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1, Bi2O3 and tetragonal Bi2O3 (PDF#74-1374) standard cards. Figure 4 It can be known that the diffraction peak of the hairy hollow bismuth trioxide / carbon microsphere (Bi2O3 / C microsphere) prepared in Example 1 is very close to the diffraction peak of Bi2O3, and is completely consistent with the peak of the standard card tetragonal Bi2O3 (PDF#74-1374), without the appearance of impurity peaks, which indicates that the sample prepared by the method of Example 1 is of high purity and does not introduce other impurities. By comparing the diffraction peaks of Bi2O3 / C and Bi2O3, it is found that there is no obvious C peak in the diffraction peak of the hairy hollow bismuth trioxide / carbon microsphere (Bi2O3 / C microsphere), because a large amount of amorphous carbon is produced during the carbonization process, and the amorphous carbon has a low crystallinity and cannot be scanned out. In addition, the diffraction peak of the hairy hollow bismuth trioxide / carbon microsphere (Bi2O3 / C microsphere) prepared in Example 1 is sharper, indicating that Bi2O3 is well crystallized. It can also be seen from the XRD spectrum that the (101) crystal plane exposure of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) is higher than that of Bi2O3, which will be beneficial to the adsorption of pollutants.
[0052] Figure 5The figure shows the test graph of the specific surface area of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) and Bi2O3 prepared in Example 1. Figure 5 It can be seen that the specific surface area of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) is 351.22 m 2 / mg -1 , which is much larger than the specific surface area of Bi2O3 (98.22 m 2 mg -1 It can be seen from this that after bismuth trioxide (Bi2O3) is attached to carbon in Example 1, its contact area with the catalytic substrate is greatly increased, which is beneficial to catalytic degradation.
[0053] Figure 6 The pore size distribution diagram of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1. Figure 6 It can be seen that the pore size distribution of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1 is between 2 and 10 nm, which is conducive to the free growth of Bi2O3 crystals, and is also conducive to the entry and exit of pollutants, and is convenient for catalytic degradation.
[0054] Figure 7 The Raman spectrum of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1 is shown in FIG. Figure 7 It can be seen that the Raman spectrum of the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared in Example 1 is at 1321 cm -1 and 1582cm -1 Two characteristic peaks D and G appear at the 3 SP of vibration and complete graphitized structure 2 Vibration peak.
[0055] Figure 8 This is a comparison of the degradation of methylene blue by the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres), carbon spheres and Bi2O3 prepared in Example 1. Figure 8 It can be seen that the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) have the highest photodegradation activity, showing better photocatalytic performance than carbon balls (3%, 140 min) and Bi2O3 (10%, 140 min), and under simulated visible light, the concentration of 50 mg / L MB was reduced by 99% within 140 min.
[0056] Fig. 9 The UV-visible absorption spectrum of the degradation of methylene blue by hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) within a certain reaction time. Fig. 9It can be seen that the absorption peak intensity of the MB solution at 664 nm is constantly weakening. Under simulated visible light, the absorption peak intensity of the MB solution is significantly lowered, which is attributed to the photocatalytic degradation effect.
[0057] Similarly, the above-mentioned performance test was carried out on the hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared under other conditions in Examples 2 to 11. From the results, it can be seen that the products prepared under other conditions in Examples 2 to 11 do meet the physical properties of hairy hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres), and can also be used as photocatalysts to catalyze the degradation of pollutants such as methylene blue.
[0058] In summary, the present invention discloses a method for preparing hairy ball-shaped hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres), which mainly comprises first preparing hollow carbon microspheres by ultra-low temperature crystallization, and then preparing hairy ball-shaped hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) by hydrothermal method. The preparation method of the present invention is simple to operate, and the prepared hairy ball-shaped hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) use bismuth citrate as a bismuth source and hollow porous hairy carbon balls with a large specific surface area as carriers, and ultra-low temperature crystallization and hydrothermal method are used to synthesize "hairy ball"-shaped hollow Bi2O3 / C microspheres with unique morphology. Due to the "hole" effect, hydroxyl radicals are generated, which can be used for photocatalytic degradation. The hairy ball-shaped hollow bismuth trioxide / carbon microspheres (Bi2O3 / C microspheres) prepared by the present invention use hollow carbon balls as templates, and synthesize a "hairy ball"-shaped hollow structure Bi2O3 / C microsphere with a large specific surface area through a low-temperature crystallization method and a hydrothermal method. This special structure effectively increases the surface area of Bi2O3, allowing the carbon balls to attach more Bi2O3, and the hollow structure is conducive to the rapid embedding and crystallization of bismuth ions, effectively shortening the transmission path of lithium ions. When the "hairy ball"-shaped hollow Bi2O3 / C microspheres are used as photocatalytic materials, they have a higher initial surface area than pure Bi2O3, and have a more efficient effect in catalytic degradation of pollution.
[0059] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for preparing hairy hollow bismuth trioxide / carbon microspheres, characterized in that: The preparation method comprises the following steps: (1) hollow carbon microspheres are prepared by ultra-low temperature crystallization method: under the condition of vacuum and nitrogen, initiator, polymerization monomer, cross-linking agent, deoxyethanol solution, acrylic acid and pre-ultrasonicated deionized water are mixed, heated for polymerization and then placed in liquid nitrogen for freezing, and the emulsion is completely crystallized, vacuumed and then returned to room temperature for centrifugation and air drying, and then cooled after carbonization to obtain hollow carbon microspheres; (2) Preparing hairy hollow bismuth trioxide / carbon microspheres by a hydrothermal method: placing the hollow carbon microspheres in a mixture of anhydrous ethanol and deionized water, adjusting the pH to 10, adding bismuth citrate to carry out a hydrothermal reaction in a reactor, cooling, washing and drying to obtain hairy hollow bismuth trioxide / carbon microspheres.
2. The preparation method according to claim 1, characterized in that: The initiator in step (1) is potassium persulfate or azobisisobutyramidine hydrochloride.
3. The preparation method according to claim 1, characterized in that: In step (1), the polymerizable monomer is styrene, ethylene glycol dimethacrylate or acrylic acid; The polymerizable monomer is a mixture of styrene, ethylene glycol dimethacrylate and acrylic acid in a molar ratio of 2.0-9.0:0.1-0.5:20.0-35.
0.
4. The preparation method according to claim 1, characterized in that: In step (1), the cross-linking agent is ethylene glycol dimethacrylate or p-vinylbenzene.
5. The preparation method according to claim 1, characterized in that: In step (1), the volume ratio of deoxyethanol to deionized water in the deoxyethanol solution is 4-25:100-300.
6. The preparation method according to claim 1, characterized in that: In step (2), triethylamine or ammonia water is used to adjust the pH during the pH adjustment process, wherein the dropping speed is 1 to 3 d / s; The hydrothermal reaction is specifically: hydrothermal reaction at 180-200° C. for 24-36 hours.
7. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the hollow carbon microspheres to bismuth citrate is 0.1-0.15:1.0-1.
5.
8. Hairy hollow bismuth trioxide / carbon microspheres prepared according to the preparation method according to any one of claims 1 to 7.
9. The hairy hollow bismuth trioxide / carbon microspheres according to claim 8, characterized in that: The diameter of the hairy hollow bismuth trioxide / carbon microspheres is 232±30 nm, the hollow diameter is 180-200 nm, and the pore size distribution is between 2-60 nm.
10. Use of the hairy hollow bismuth trioxide / carbon microspheres according to any one of claims 8 to 9 in photocatalytic degradation of methylene blue.
Citation Information
Patent Citations
Method for preparing ball-flower-shaped gamma-bismuth trioxide powder
CN102491417A
Solvothermal preparation method of bismuth trioxide microspheres and application thereof
CN103420414A
Polymer porous microsphere, carbon sphere and ultra-black material prepared from the same, and applications
CN109280209A
Hollow porous microspheres
US20100264097A1