Cobalt-doped nano zinc oxide as well as green synthesis method and application thereof
By using bioactive compounds in seabuckthorn leaves to synthesize cobalt-doped nano-zinc oxide, the high cost and environmental pollution problems of chemical reduction methods are solved, and the effects of green synthesis and efficient photocatalytic degradation of dyes are achieved.
Patent Information
- Application Number
- CN202411178170.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing chemical reduction method to synthesize nano-zinc oxide involves high production costs and environmental pollution risks, and fails to effectively utilize plant resources.
Using seabuckthorn leaves from Inner Mongolia as raw materials, cobalt-doped nano-zinc oxide was synthesized through plant reduction method. Bioactive compounds in seabuckthorn leaves were used for green synthesis and applied in photocatalytic degradation of dyes.
It achieves efficient utilization of resources, reduces the risk of environmental pollution caused by chemical substances, and accelerates the chemical adsorption reaction on the material surface through cobalt doping, improving the effect of photocatalytic degradation of dyes.
Smart Images

Figure CN118719073A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chemical synthesis, relates to the technical field of synthesizing nano zinc oxide by plant reduction method, and specifically relates to cobalt-doped nano zinc oxide and a green synthesis method and application thereof. Background Art
[0002] Nano zinc oxide is a new type of nanomaterial with high surface area, volume ratio and high reactivity. It has attracted wide attention due to its high performance, high efficiency and eco-friendliness. There are many ways to prepare nano zinc oxide, including physical, chemical and biological synthesis. At present, the commonly used method is chemical reduction, which uses chemical substances as reducing agents and stabilizers. The production cost is high. In the actual preparation process, due to its complicated operation process, it may also cause environmental pollution.
[0003] The current research trend is to use plant reduction method to synthesize nano zinc oxide, using green plants instead of chemicals, reducing the risk of environmental pollution while increasing the availability of plants. Summary of the invention
[0004] The present invention mainly utilizes the leaves of seabuckthorn plants widely planted in Inner Mongolia, and adopts a reduction method to synthesize nano zinc oxide particles in a green way. Seabuckthorn has the characteristics of cold resistance, drought resistance, and wind and sand resistance. It is an ecological tree planted in large quantities in Northwest my country. Its fruit is rich in nutrients, and the content of vitamin C, vitamin E and carotene are higher than other fruits. However, there are fewer ways to utilize its leaves. Seabuckthorn leaves are a high-quality raw material for synthesizing nano zinc oxide, rich in flavonoids and various bioactive compounds, and these chemicals can reduce metal ions and stabilize them at the nanometer scale.
[0005] In order to solve the technical problems raised in the background technology, the present invention proposes a green synthesis method of cobalt-doped nano zinc oxide and provides the application of nano zinc oxide particles in photocatalytic degradation of dyes.
[0006] The first technical solution of the present invention is a green synthesis method of cobalt-doped nano zinc oxide, comprising the following steps: 1) Grind the dried seabuckthorn leaves into powder using a grinder and store them in a sealed container to prevent air oxidation; 2) Weighing the dried seabuckthorn leaf powder, adding water and placing on a magnetic stirrer, heating and stirring, placing in an incubator overnight, cooling and filtering to obtain a seabuckthorn leaf plant extract; 3) taking a mixed solution of zinc acetate and cobalt nitrate, adding the seabuckthorn leaf plant extract obtained in step 2), adjusting the pH of the solution with NaOH, and placing the solution in a constant temperature box after ultrasonic treatment to complete the reaction; 4) After the solution is centrifuged, the upper liquid phase is removed, and the remaining solid part is washed with ethanol and distilled water, and the solid part is collected and dried in an oven; 5) The dried solid is calcined in a muffle furnace and ground to obtain modified nano zinc oxide particles.
[0007] Wherein, the seabuckthorn leaves in step 1) are Chinese seabuckthorn, and the extract is rich in phytochemicals such as alkaloids, phenols, and flavonoids, which play an important role in synthesizing nanoparticles; The seabuckthorn leaves in step 1) are preferably Chinese seabuckthorn leaves in July; The alkaloid content of the seabuckthorn leaves in step 1) is 1.321-1.376 mg / g, the polyphenol content is 19.246-19.511 mg / g, and the flavonoid content is 27.509-28.432 mg / g.
[0008] Wherein, in step 2), the solution pH is adjusted to 8-11, preferably 9-11.
[0009] Wherein, in step 2), the solid-to-liquid ratio of seabuckthorn leaf powder to water is 50-150 g / L.
[0010] Wherein, in step 2), the heating temperature of the magnetic stirrer is 60-65°C, the heating and stirring are performed for 4 hours, and the temperature of the constant temperature box is 37°C.
[0011] Wherein, in step 3), the concentration of zinc acetate in the mixed solution is 0.1-1M, the concentration of cobalt nitrate is 0.1M, the volume ratio of zinc acetate to cobalt nitrate in the solution is 5:95-15:85, and the volume ratio of seabuckthorn leaf plant extract to the mixed solution of zinc acetate and zinc nitrate is 1:1.
[0012] Wherein, in step 5), the calcination temperature in the muffle furnace is 400-550° C. and the calcination time is three hours.
[0013] The second technical solution of the present invention is a modified nano zinc oxide prepared by the above method, wherein the atomic percentage of O is 50-56%, the atomic percentage of Co is 1.6-2.0%, and the atomic percentage of Zn is 42-48%; The weight percentage of O element is 19-24%, the weight percentage of Co element is 2-3%, and the weight percentage of Zn element is 73-78%.
[0014] The third technical solution of the present invention is to use the cobalt-doped nano zinc oxide prepared by the above method for photocatalytic degradation of dyes.
[0015] The beneficial effects of the present invention are: (1) The plant reducing agent used in the present invention is seabuckthorn leaf extract. Seabuckthorn is an ecological tree widely planted in Inner Mongolia. Using it as a raw material to synthesize nano zinc oxide can not only realize the resource utilization of the leaves, but also reduce the pollution of chemical substances to the environment in the chemical synthesis method.
[0016] (2) It has a certain degradation effect on dyes in aqueous solution and can be further developed for photocatalytic degradation of dyes.
[0017] (3) Cobalt nitrate is added to complete the doping of cobalt element in the preparation of nano zinc oxide. Cobalt has rich electronic states and high solubility. Co ions can easily replace Zn ions in the ZnO lattice because the ionic radius of cobalt is comparable. Cobalt doping can accelerate the chemical adsorption reaction on the surface of the material and act as a catalyst.
[0018] (4) When the pH of the mixed solution of seabuckthorn extract and zinc acetate is in the range of 10-12, a large number of hydroxide ions will preferentially combine with zinc ions to form a stable zinc hydroxide complex, such as [Zn(OH)4] 2- At the same time, within this range, reducing substances in the extract, such as polyphenol compounds, can further reduce zinc hydroxide to zinc oxide nanoparticles. When the pH is in the range of 10-12, the removal rate of methylene blue is relatively high. This is because the isoelectric point of ZnO is 9.5. Methylene blue is a cationic dye. When the solution pH is in the range of 10-12, it is greater than the isoelectric point of ZnO. The catalyst surface is negatively charged, which is conducive to the adsorption of methylene blue molecules. An overly high pH environment may make organic compounds such as polysaccharides and flavonoids in seabuckthorn extract unstable, thereby affecting the reduction stage. An overly low pH environment affects the formation of zinc hydroxide complexes due to fewer hydroxide ions, reduces the yield of nano zinc oxide, and increases the preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Example 1 SEM electron microscope characterization of nano zinc oxide; Figure 2 Example 2 SEM electron microscope characterization of nano zinc oxide; Figure 3 Example 3 SEM electron microscope characterization of nano zinc oxide; Figure 4 Example 1: Energy spectrum scanning diagram of nano zinc oxide; Figure 5 Example 2: Energy spectrum scanning diagram of nano zinc oxide; Figure 6 Energy spectrum scanning diagram of nano zinc oxide in Example 3. DETAILED DESCRIPTION
[0020] The following examples are provided for a better understanding of the present invention and are not intended to limit the present invention. Any improvements and changes made based on the specific embodiments of the present invention are within the scope of protection of the claims of the present invention.
[0021] Example 1 A method for preparing modified nano zinc oxide S1. Accurately weigh 25 g of dried seabuckthorn leaf powder, put it in a conical flask filled with 500 mL of distilled water, heat and stir it on a magnetic stirrer at a speed of 400 rpm for 4 hours, the heating temperature is 60°C, and after stirring, place it in an incubator overnight. After cooling the reactant, filter it to obtain a pure plant extract; S2. Measure 100 mL of plant extract into a conical flask, add 5 mL of cobalt nitrate and 95 mL of zinc acetate mixed solution dropwise, the concentration of zinc acetate in the mixed solution is 0.1 M, the concentration of cobalt nitrate is 0.1 M, adjust the solution pH to 11, and place it in a constant temperature box after ultrasonic treatment to complete the reaction; the experimental ultrasonic frequency is 40 KHz. The ultrasonic time is 30 minutes, and the reaction time in the constant temperature box is two hours; S3, the reaction solution was centrifuged at 10000r / min for ten minutes, the upper liquid phase was removed, the remaining solid part was washed with ethanol and distilled water, and the obtained solid part was dried in an oven; S4. The dried solid part is manually ground and calcined in a muffle furnace at 500° C. for 3 hours to obtain cobalt-doped nano zinc oxide.
[0022] The SEM electron microscope characterization image of the nano zinc oxide prepared in this embodiment is as follows: Figure 1 As shown, the energy spectrum scan is shown in Figure 4 , Table 1 is the energy spectrum element analysis data table.
[0023] Table 1
[0024] The present invention analyzes the elemental composition of the sample according to energy spectrum scanning. Figure 4 It can be seen that the particles contain three elements: ZnO, O and Co, which confirms the existence of cobalt-doped nano zinc oxide.
[0025] Example 2 A method for preparing modified nano zinc oxide The steps of this embodiment are basically the same as those of embodiment 1, wherein the solid-liquid ratio of seabuckthorn leaf powder to water in step S1 is 50 g / L, the concentration of zinc acetate in the mixed solution in step S2 is 0.5 M, the concentration of cobalt nitrate is 0.1 M, the volume ratio of zinc acetate to cobalt nitrate in the mixed solution is 10:90, and the pH of the solution in S2 is adjusted to 8.
[0026] The SEM electron microscope characterization image of the nano zinc oxide prepared in this embodiment is as follows: Figure 2As shown, the energy spectrum scan is shown in Figure 5 , Table 2 is the energy spectrum element analysis data table.
[0027] Table 2
[0028] Example 3 A method for preparing modified nano zinc oxide The steps of this embodiment are basically the same as those of embodiment 1, wherein the solid-liquid ratio of seabuckthorn leaf powder to water in step S1 is 150 g / L, the concentration of zinc acetate in the mixed solution in step S2 is 1 M, the concentration of cobalt nitrate is 0.1 M, the volume ratio of zinc acetate and cobalt nitrate in the mixed solution is 15:85, and the pH of the solution in S2 is adjusted to 9.
[0029] The SEM electron microscope characterization image of the nano zinc oxide prepared in this embodiment is as follows: Figure 3 As shown, the energy spectrum scan is shown in Figure 6 , Table 3 is the energy spectrum element analysis data table.
[0030] Table 3
[0031] The embodiments of the present invention and the comparative examples were tested, and the three modified nano zinc oxides obtained were subjected to photocatalytic experiments. The methylene blue (MB) concentration was set to 5 mg / L, 50 mL of MB solution was taken in a reaction container, and 25 mg of the cobalt-doped nano zinc oxide obtained in the embodiment was added respectively. The reaction container was placed in a dark environment for 30 min before illumination to allow the MB and the catalyst to reach adsorption-desorption equilibrium. The reaction was carried out under ultraviolet light for 180 min, and the reaction solution was centrifuged at 10000 r / min for ten minutes. The supernatant was taken every 30 min for a total of 3 hours, and a total of six extractions were performed. The absorbance was measured at a wavelength of 664 nm, and three groups of experiments were performed in sequence.
[0032] Table 4 Performance of each embodiment for photocatalytic degradation of dyes
[0033] It can be seen from the above table that under the condition of a reaction time of 180 min, the removal rates of MB at PH = 8, 9, and 11 are 33.88%, 33.41%, and 45.41%, respectively. The results show that in Example 1, when PH = 11, the removal effect is better and can reach about 45%.
[0034] Obviously, the above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the invention.
[0035] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the interpretation or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A green synthesis method of cobalt-doped nano zinc oxide, characterized in that: The following steps are involved: 1) Grind the dried seabuckthorn leaves into powder and store in a sealed container; 2) Weighing the dried seabuckthorn leaf powder, adding water and then magnetically stirring, heating and stirring, placing in an incubator overnight, cooling and then filtering to obtain a seabuckthorn leaf plant extract; 3) taking a mixed solution of zinc acetate and cobalt nitrate, adding the seabuckthorn leaf plant extract obtained in step 2), adjusting the pH of the solution to 8-11 with NaOH, and placing the solution in a constant temperature box after ultrasonic treatment to complete the reaction; 4) centrifuging the solution after the reaction in step 3) to remove the upper liquid phase, washing the remaining solid part with ethanol and distilled water, and collecting the solid part and drying it in an oven; 5) calcining and grinding the dried solid in a muffle furnace to obtain modified nano zinc oxide particles; In the step 1), the alkaloid content in the seabuckthorn leaves is 1.321-1.376 mg / g, the polyphenol content is 19.246-19.511 mg / g, and the flavonoid content is 27.509-28.432 mg / g; In the step 3), the concentration of zinc acetate in the mixed solution is 0.1-1 M, the concentration of cobalt nitrate is 0.1 M, and the volume ratio of zinc acetate to cobalt nitrate in the mixed solution is 5:95-15:
85.
2. The method according to claim 1, characterized in that In the step 2), the solid-to-liquid ratio of seabuckthorn leaf powder to water is 50-150 g / L.
3. The method according to claim 1, characterized in that The magnetic stirring heating temperature in step 2) is 60-65°C.
4. The method according to claim 1, characterized in that: In step 3), the volume ratio of the seabuckthorn leaf plant extract to the mixed solution of zinc acetate and cobalt nitrate is 1:
1.
5. The method according to claim 1, characterized in that The pH of step 3) is 9-11.
6. The method according to claim 1, characterized in that The calcination temperature in step 5) is 400-550°C.
7. Nano zinc oxide prepared by the method according to any one of claims 1 to 6, wherein the atomic percentage of O is 50-56%, the atomic percentage of Co is 1.6-2.0%, and the atomic percentage of Zn is 42-48%; The weight percentage of O element is 19-24%, the weight percentage of Co element is 2-3%, and the weight percentage of Zn element is 73-78%.
8. Use of nano zinc oxide prepared by the method according to any one of claims 1 to 6 in photocatalytic degradation of dyes.
Citation Information
Patent Citations
Method for preparing cobalt-doped zinc oxide (CoxZn1-xO) multifunctional magnetic nano powder by alcohol heating process
CN101870495A
Preparation method for Co / ZnO composite material
CN106362750A
Nano-zinc oxide greenly synthesized from camphor tree leaves, and preparation method and application thereof
CN113307301A
Copper-doped zinc oxide nano antibacterial material as well as preparation method and application thereof
CN116282128A
Polymer material
JP2010077064A
Cited By
Molybdenum-doped nano zinc oxide with high visible light photocatalytic performance as well as preparation method and application of molybdenum-doped nano zinc oxide
CN119793438A
Molybdenum-doped nano-zinc oxide with high visible-light photocatalytic performance and preparation method and application thereof
CN119793438B