Preparation method and application of anion modified Ni-MoO2 / Cu heterostructure catalyst
The anion-modified Ni-MoO2/Cu heterostructure catalyst solves the problems of slow kinetics of hydrogen production reaction in alkaline water electrolysis and poor stability of platinum-based catalysts, achieving efficient and stable catalysis under alkaline conditions, and has the ability to replace precious metals. Catalyst potential.
Patent Information
- Application Number
- CN202410784705.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Under alkaline conditions, the kinetics of the hydrogen production reaction by electrolysis of water is slow and the hydrogen production rate is low. Commercial platinum-based catalysts are expensive and have poor stability at high current densities. As a result, the development of efficient and stable hydrogen evolution reaction electrocatalysts has become a research hotspot.
Anion-modified Ni-MoO2/Cu heterostructure catalyst is used, prepared by hydrothermal, electrodeposition and high-temperature annealing methods. As a hydrogen evolution catalyst under alkaline conditions, nickel metal is used as the conductive substrate, and molybdenum and copper are combined to form an active catalytic layer. .
It exhibits excellent catalytic activity and stability under alkaline conditions, can achieve efficient electrolysis of water for hydrogen production at lower current densities, has the potential to replace precious metal catalysts, and shows high efficiency and stability in industrial applications.
Smart Images

Figure CN118719079A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a preparation method and application of an anion-modified Ni-MoO2 / Cu heterostructure catalyst, belonging to the technical field of nanomaterials. Background Art
[0002] Hydrogen production by water electrolysis is one of the environmentally friendly hydrogen production technologies, which can convert solar energy or electrical energy into chemical energy for storage. Compared with water electrolysis under acidic conditions, hydrogen production under alkaline conditions is cost-effective for large-scale applications. However, the kinetics of the hydrogen evolution reaction in alkaline electrolytes are slow and the hydrogen production rate is low. Therefore, the development of efficient and stable electrocatalysts for the hydrogen evolution reaction is a hot topic in current research. Commercial platinum-based catalysts have problems such as high prices and poor stability under high current densities in working conditions. In recent years, research on low-cost, environmentally friendly non-precious metals to replace platinum-based materials has become a hot topic. Today, Mo-based has been proven to be one of the most promising alternative materials to precious metal Pt-based catalysts. Summary of the invention
[0003] The present invention provides a method for preparing an anion-modified heterostructure catalyst electrode, using nickel metal as a conductive substrate and adopting hydrothermal, electrodeposition and high-temperature annealing methods to prepare an active catalyst layer. The catalyst exhibits good catalytic activity and stability in hydrogen evolution reaction under alkaline conditions, and has good industrial application prospects and commercial value.
[0004] This application intends to construct an anion-modified Ni-MoO2 / Cu heterostructure hydrogen evolution catalyst. The catalyst exhibits excellent catalytic activity and stability when catalyzing alkaline hydrogen evolution reaction under traditional three-electrode conditions.
[0005] According to one aspect of the present application, a method for preparing an anion-modified Ni-MoO2 / Cu heterostructure catalyst is provided, the preparation method comprising the following steps:
[0006] (1) pretreating the nickel-based material by soaking the nickel-based material in a nitric acid solution for a period of time, and then rinsing the nickel-based material with deionized water for multiple times to obtain the pretreated nickel-based material;
[0007] (2) in a closed reactor, reacting and drying a mixture containing a molybdenum salt, an anion salt solution, and a pretreated nickel-based material to obtain an anion-modified Ni-MoO2 precursor;
[0008] (3) using the anion-modified Ni-MoO2 precursor as a cathode, and performing an electrodeposition treatment in a mixed solution containing copper sulfate and boric acid to obtain an anion-modified Ni-MoO2 / Cu precursor;
[0009] (4) Under an inactive atmosphere, the anion-modified Ni-MoO2 / Cu precursor is annealed to obtain the anion-modified Ni-MoO2 / Cu heterostructure catalyst.
[0010] Optionally, in step (1), the nickel-based material is selected from at least one of nickel foil, nickel foam, and nickel felt.
[0011] Optionally, the concentration of the nitric acid solution is 10wt.% to 50wt.%.
[0012] Optionally, the concentration of the nitric acid solution is independently selected from any value of 10wt%, 20wt%, 30wt%, 40wt%, 50wt% or a range between any two of the above.
[0013] Optionally, in step (1), the soaking time is 10 min to 30 min.
[0014] Optionally, the soaking time is independently selected from any value among 10 min, 12 min, 15 min, 20 min, 25 min, 30 min or a range between any two of the above.
[0015] Optionally, in step (2), the molybdenum salt is selected from at least one of ammonium molybdate, sodium molybdate and potassium molybdate.
[0016] Optionally, the concentration of the molybdenum salt solution is 0.01-0.1 mol / L.
[0017] Optionally, the concentration of the molybdenum salt solution is independently selected from any value among 0.01mol / L, 0.02mol / L, 0.03mol / L, 0.04mol / L, 0.05mol / L, 0.06mol / L, 0.07mol / L, 0.08mol / L, 0.09mol / L, 0.1mol / L or a range between any two of the above.
[0018] Optionally, the anion salt in the anion salt solution is selected from at least one of H3BO3, NH4Cl, NH4F, and NH4PO4.
[0019] Optionally, the concentration of the anionic salt solution is independently selected from any value among 0.2mol / L, 0.4mol / L, 0.6mol / L, 0.8mol / L, 1mol / L, 1.2mol / L, 1.4mol / L, 1.6mol / L, 1.8mol / L, 2mol / L or a range between any two of the above.
[0020] Optionally, the molar ratio of the molybdenum salt to the anion salt solution is 0.01-1:0.2-2, and the molar amount of the anion salt solution is based on the molar amount of the anion salt.
[0021] Optionally, in step (2), the reaction temperature is 150-200° C., and the reaction time is 10-30 h.
[0022] Optionally, in step (2), the reaction temperature is independently selected from any value of 150°C, 160°C, 170°C, 180°C, 190°C, 200°C or a range between any two of the above values.
[0023] Optionally, in step (2), the reaction time is independently selected from any value among 10 h, 15 h, 20 h, 25 h, 30 h, or a range between any two of the above.
[0024] Optionally, the drying temperature is 40 to 80° C., and the drying time is 6 to 24 hours.
[0025] Optionally, in step (3), the concentration of copper sulfate is 0.005-0.1 mol / L.
[0026] Optionally, in step (3), the concentration of copper sulfate is independently selected from any value among 0.005 mol / L, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, or a range between any two of the above.
[0027] Optionally, the concentration of the boric acid is 0.01-0.1 mol / L.
[0028] Optionally, in the electrodeposition treatment, the ratio of copper sulfate to boric acid in the deposition solution is 0.005-0.1:0.01-0.1.
[0029] Optionally, in step (3), the deposition current during the electrodeposition treatment is -2 to -10 mA cm -2 .
[0030] Optionally, the deposition time during the electrodeposition treatment is 200 to 400 seconds.
[0031] Optionally, the deposition time during the electrodeposition treatment is independently selected from any value among 200s, 220s, 250s, 280s, 300s, 350s, 380s, 400s or a range between any two of the above values.
[0032] Optionally, in step (4), the temperature of the annealing treatment is independently selected from any value of 300°C, 350°C, 400°C, 450°C, 500°C or a range between any two of the above values.
[0033] Optionally, in step (4), the annealing time is independently selected from any value among 1h, 2h, 3h, 4h or a range between any two of the above.
[0034] Optionally, the heating rate during the annealing treatment is 2-10° C. / min.
[0035] Optionally, in step (4), the inert atmosphere is selected from at least one of argon and nitrogen.
[0036] According to another aspect of the present application, there is provided an anion-modified Ni-MoO2 / Cu heterostructure catalyst prepared by the preparation method described above.
[0037] According to another aspect of the present application, there is provided an application of the above-mentioned anion-modified Ni-MoO2 / Cu heterostructure catalyst in catalyzing electrochemical hydrogen evolution reaction.
[0038] According to the fourth aspect of the present application, a highly efficient and stable catalyst for hydrogen production by water electrolysis is provided, and a water electrolysis hydrogen evolution test is carried out using a three-electrode assembly in an alkaline electrolyte solution, wherein the three-electrode assembly includes a working electrode, a counter electrode and a reference electrode, and the electrolyte is a 1M potassium hydroxide solution.
[0039] As an optional implementation method, the present application is implemented through the following technical solutions:
[0040] A method for preparing an anion-modified oxide and a metal heterostructure catalyst comprises the following steps:
[0041] 1) Commercially available nickel foam (NF, 2.5×3.5 cm 2 ) was used as a substrate, and ultrasonic cleaning was performed with acetone, ethanol, 1 mol / L HNO3 solution, and deionized water for 15 min in sequence to obtain cleaned NF;
[0042] 2) Weigh 2.47g of ammonium heptamolybdate tetrahydrate, add 30mL of deionized water, and stir for 20min to obtain a clear solution. Add the stirred solution and the pretreated nickel foam into a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal kettle, and react at 180°C in an oven for 16 hours. After the reaction is completed and the temperature drops naturally, take out the nickel foam from the reactor, rinse it with a large amount of water and ethanol, and then put the sample into a forced air drying oven to dry for 6 hours;
[0043] 3) Using electrochemical deposition, the sample in step 2) was used as the conductive carrier and catalyst carrier, and the electrochemical deposition precursor solution (the composition of the electrochemical deposition precursor solution was 10 mmol / L anhydrous copper sulfate + 50 mmol / L boric acid) was stirred at -5 mA cm -2 Electrodeposition was carried out for 300 s to obtain the Ni-MoO2 / Cu material precursor in situ.
[0044] 4) Place the Ni-MoO2 / Cu precursor synthesized in the previous step in a tubular furnace, fill the tubular furnace with high-purity argon as a reaction protective gas, and continue to pass the gas flow at a rate of 150 ml / min for 30 minutes to exhaust the oxygen in the tubular furnace. After the exhaust is completed, adjust the gas flow rate to 80 ml / min, and increase the temperature to 400°C at a rate of 5°C / min and maintain it for 2 hours. Wait for the reaction to end and cool naturally before taking out the sample to obtain the final product.
[0045] Optionally, in step 2), nickel acetate tetrahydrate and ammonium heptamolybdate tetrahydrate aqueous solution are prepared, stirred evenly, urea is added and stirring is continued until the solution presents a clear and transparent light green color; the stirred solution and the pretreated nickel foam are added to a stainless steel hydrothermal autoclave lined with polytetrafluoroethylene, and reacted in an oven at 150 to 200 degrees Celsius for 15 to 30 hours.
[0046] Optionally, in step 2), after the reaction is completed and the temperature is naturally lowered, the foam in the reactor is taken out, washed with a large amount of water and ethanol, and then the sample is placed in a vacuum drying oven and dried for 6 to 8 hours.
[0047] Optionally, in step 4), the obtained sample is placed in the center of a tube furnace, and the temperature is raised to 400±20° C. at a heating rate of 1 to 5° C. / min in a nitrogen or argon atmosphere and maintained for 1 to 5 hours.
[0048] The present application provides a preparation method and application of an anion-modified Ni-MoO2 / Cu heterostructure catalyst. The present invention has a high catalytic efficiency for hydrogen evolution reaction, and the hydrogen evolution reaction is 10 mA cm -2 At a current density of , the overpotential is 42mV. The catalyst can be used to produce hydrogen by electrolysis of water. It exhibits high catalytic activity and high stability in an alkaline environment, can improve the efficiency of hydrogen production by electrolysis of water, and has the potential to replace precious metal catalysts.
[0049] The beneficial effects of this application include:
[0050] 1) The preparation method of the anion-modified Ni-MoO2 / Cu heterostructure catalyst provided in the present application can adjust the hydrogen evolution activity of the catalyst by adding different anion salt solutions.
[0051] 2) The preparation method provided in the present application obtains a highly active and highly stable electrode system by changing the components, concentration, reaction temperature, reaction time and other parameters of the reaction solution, thereby meeting different requirements for catalytic performance.
[0052] 3) The integral electrode provided in the present application is based on nickel foam, and has the advantages of excellent conductivity and large specific surface area, which is beneficial to the transfer of electrons and protons in the reaction and the increase of catalyst loading.
[0053] 4) The in-situ preparation method provided in the present application is conducive to the close bonding between the catalyst and the conductive support, thereby improving its charge transport properties and mechanical stability, which is crucial in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 These are SEM images of Ni-MoO2 / Cu prepared in Example 1 of the present application at different magnifications.
[0055] Figure 2 These are TEM images of the sample in Example 1 of the present application at different magnifications.
[0056] Figure 3 This is the TEM element distribution diagram of the sample in Example 1 of the present application.
[0057] Figure 4 This is a graph of hydrogen evolution activity of the sample of Example 1 of this application and a commercial Pt / C catalyst in an alkaline electrolyte. The horizontal axis is the standard hydrogen electrode voltage (V vs RHE), and the vertical axis is the current density (mA / cm 2 ).
[0058] Figure 5 This is the constant current Vt curve of the sample in Example 1 of the present application in 1 mol / L KOH electrolyte solution. DETAILED DESCRIPTION
[0059] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0060] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0061] The present application uses a GeminiSEM 300 scanning electron microscope to measure the microscopic morphology of active substances in the catalyst.
[0062] The lattice spacing of the active substances in the catalyst was measured using a JEM 2100F transmission electron microscope.
[0063] The hydrogen evolution performance was characterized using a Coster electrochemical workstation, and the hydrogen evolution activity of the prepared catalyst was tested by testing the electrochemical polarization curve and constant current curve.
[0064] Example 1
[0065] Step 1: Use commercially available nickel foam (NF, 2×2 cm 2 ) was used as a substrate, and ultrasonic cleaning was performed with acetone, ethanol, 1 mol / L HNO3 solution, and deionized water for 15 min in sequence to obtain the cleaned NF (pretreated nickel foam);
[0066] Step 2: Weigh 2mmol, 2.47g of ammonium heptamolybdate tetrahydrate and 40mmol of ammonium fluoride, add 30mL of deionized water, and stir for 20min to obtain a clear solution. Add the stirred solution and the pretreated nickel foam to a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal kettle, and react at 180°C in an oven for 16 hours. After the reaction is completed and the temperature is naturally lowered, take out the nickel foam in the reactor, rinse it with a large amount of water and ethanol, and then put the sample into a forced air drying oven at 50°C for 6 hours;
[0067] Step 3: Using electrochemical deposition, the sample in step 2 was used as the conductive carrier and catalyst carrier, and the electrochemical deposition was carried out at -5 mA cm in a newly prepared 100 ml electrochemical deposition precursor solution (the components of the electrochemical deposition precursor solution were 1 mmol, 0.16 g anhydrous copper sulfate + 5 mmol, 0.31 g boric acid). -2 Electrodeposition was carried out for 300 s to obtain the Ni-MoO2(F) / Cu material precursor in situ.
[0068] Step 4: Place the precursor synthesized in step 3 in a tube furnace, fill the tube furnace with high-purity argon as a reaction protection gas, and continue to pass the gas flow at a rate of 150 ml / min for 30 minutes to exhaust the oxygen in the tube furnace. After the exhaust is completed, adjust the gas flow rate to 80 ml / min, and increase the temperature to 400°C at a rate of 5°C / min and maintain it for 2 hours. Wait for the reaction to end and cool naturally before taking out the sample to obtain the final product.
[0069] like Figure 1 As shown, the SEM image of the sample prepared in Example 1 shows that it has a nanosheet array morphology.
[0070] like Figure 2 As shown, the TEM image of the sample prepared in Example 1 shows that it has a heterogeneous interface of Cu and MoO2.
[0071] like Figure 3 As shown, the TEM element distribution diagram of the sample prepared in Example 1 shows that Ni, Mo, Cu, O, and F elements are uniformly distributed.
[0072] like Figure 4 As shown, the sample prepared in Example 1 exhibited very excellent alkaline hydrogen evolution performance, and the anion F modification greatly improved the catalytic performance of the catalyst.
[0073] Embodiment 2:
[0074] Step 1: Use commercially available nickel foam (NF, 2.5×3 cm 2 ) as a substrate, and ultrasonically cleaned with acetone, ethanol, 1 mol / L HNO3 solution, and deionized water for 15 min in sequence to obtain a pretreated nickel foam;
[0075] Step 2: Weigh 2mmol, 2.47g of ammonium heptamolybdate tetrahydrate and 40mmol of ammonium chloride, add 30mL of deionized water, and stir for 20min to obtain a clear solution. Add the stirred solution and the pretreated nickel foam to a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal kettle, and react at 180°C in an oven for 16 hours. After the reaction is completed and the temperature is naturally lowered, take out the nickel foam in the reactor, rinse it with a large amount of water and ethanol, and then put the sample into a blast drying oven to dry for 6 hours;
[0076] Step 3: Using electrochemical deposition, the sample in step 2 was used as the conductive carrier and catalyst carrier, and the electrochemical deposition was carried out at -5 mA cm in a newly prepared 100 ml electrochemical deposition precursor solution (the components of the electrochemical deposition precursor solution were 1 mmol, 0.16 g anhydrous copper sulfate + 5 mmol, 0.31 g boric acid). -2 Electrodeposition was carried out for 300 s to obtain the Ni-MoO2(Cl) / Cu material precursor in situ.
[0077] Step 4: Place the MoO2(Cl) / Cu precursor synthesized in step 3 in a tube furnace, fill the tube furnace with high-purity argon as a reaction protective gas, and continue to pass the gas flow at a rate of 150 ml / min for 30 minutes to exhaust the oxygen in the tube furnace. After the exhaust is completed, adjust the gas flow rate to 80 ml / min, and increase the temperature to 400°C at a rate of 5°C / min and maintain it for 2 hours. Wait for the reaction to end and cool down naturally before taking out the sample to obtain the final product.
[0078] Embodiment 3:
[0079] Step 1: Use commercially available nickel foam (NF, 2.5×3.5 cm 2 ) as a substrate, and ultrasonically cleaned with acetone, ethanol, 1 mol / L HNO3 solution, and deionized water for 15 min in sequence to obtain a pretreated nickel foam;
[0080] Step 2: Weigh 2mmol, 2.47g of ammonium heptamolybdate tetrahydrate and 40mmol of boric acid, add 30mL of deionized water, and stir for 20min to obtain a clear solution. Add the stirred solution and the pretreated nickel foam to a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal kettle, and react at 180°C in an oven for 16 hours. After the reaction is completed and the temperature is naturally lowered, take out the nickel foam in the reactor, rinse it with a large amount of water and ethanol, and then put the sample into a forced air drying oven at 60°C for 6 hours;
[0081] Step 3: Using electrochemical deposition, the sample in step 2 is used as the conductive carrier and catalyst carrier, and in a newly prepared 100 ml electrodeposition precursor solution (the components of the electrodeposition precursor solution are 1 mmol, 0.16 g anhydrous copper sulfate + 5 mmol, 0.31 g boric acid) at -5 mA cm -2 Electrodeposition was carried out for 300 s to obtain the Ni-MoO2(B) / Cu material precursor in situ.
[0082] Step 4: Place the precursor synthesized in step 3 in a tube furnace, fill the tube furnace with high-purity argon as a reaction protection gas, and continue to pass the gas flow at a rate of 150 ml / min for 30 minutes to exhaust the oxygen in the tube furnace. After the exhaust is completed, adjust the gas flow rate to 80 ml / min, and increase the temperature to 400°C at a rate of 5°C / min and maintain it for 2 hours. Wait for the reaction to end and cool naturally before taking out the sample to obtain the final product.
[0083] Comparative Example 1:
[0084] Step 1: Use commercially available nickel foam (NF, 2×2 cm 2 ) was used as a substrate, and ultrasonic cleaning was performed with acetone, ethanol, 1 mol / L HNO3 solution, and deionized water for 15 min in sequence to obtain the cleaned NF (pretreated nickel foam);
[0085] Step 2: Weigh 2mmol, 2.47g of ammonium heptamolybdate tetrahydrate, add 30mL of deionized water, and stir for 20min to obtain a clear solution. Add the stirred solution and the pretreated nickel foam to a 50ml polytetrafluoroethylene-lined stainless steel hydrothermal kettle, and react at 180°C in an oven for 16 hours. After the reaction is completed and the temperature drops naturally, take out the nickel foam in the reactor, rinse it with a large amount of water and ethanol, and then put the sample into a forced air drying oven at 60°C for 6 hours;
[0086] Step 3: Using electrochemical deposition, the sample in step 2 was used as the conductive carrier and catalyst carrier. In a newly prepared 100 ml electrodeposition precursor solution (the components of the electrodeposition precursor solution were 1 mmol, 0.16 g anhydrous copper sulfate + 5 mmol, 0.31 g boric acid), the reaction mixture was stirred at -5 mA cm -2Electrodeposition was carried out for 300 s to obtain the Ni-MoO2 / Cu material precursor in situ.
[0087] Step 4: Place the Ni-MoO2 / Cu precursor synthesized in step 3 in a tubular furnace, fill the tubular furnace with high-purity argon as a reaction protective gas, and continue to pass the gas flow at a rate of 150 ml / min for 30 minutes to exhaust the oxygen in the tubular furnace. After the exhaust is completed, adjust the gas flow rate to 80 ml / min, and increase the temperature to 400°C at a rate of 5°C / min and maintain it for 2 hours. Wait for the reaction to end and cool down naturally before taking out the sample to obtain the final product.
[0088] Test Example 1
[0089] A composite electrode system containing Ni-MoO2(F) / Cu was prepared according to the method of Example 1, and its hydrogen evolution performance was tested under laboratory conditions (1 mol / L KOH, room temperature). When catalyzing the electrochemical hydrogen evolution reaction, it showed excellent activity and stability. Among them, the catalyst with the best activity had a current density of 10 mA cm in 1 mol / L KOH solution and room temperature. -2 Only 42mV overpotential is required, and at 200mA / cm 2 and 500mA cm -2 It ran stably for 240 hours without obvious activity decay. Figure 5 As shown, the sample prepared in Example 1 exhibits very excellent alkaline hydrogen evolution stability.
[0090] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing an anion-modified Ni-MoO2 / Cu heterostructure catalyst, characterized in that: The preparation method comprises the following steps: (1) pretreating the nickel-based material to obtain a pretreated nickel-based material; (2) in a closed reactor, placing the pretreated nickel-based material into a mixed solution containing a molybdenum salt and an anion salt, reacting and drying to obtain an anion-modified Ni-MoO2 precursor; (3) using the anion-modified Ni-MoO2 precursor as a cathode, and performing an electrodeposition treatment in a mixed solution containing copper sulfate and boric acid to obtain an anion-modified Ni-MoO2 / Cu precursor; (4) Under an inactive atmosphere, the anion-modified Ni-MoO2 / Cu precursor is annealed to obtain the anion-modified Ni-MoO2 / Cu heterostructure catalyst.
2. The preparation method according to claim 1, characterized in that: In the step (2), the molybdenum salt is selected from at least one of ammonium molybdate, sodium molybdate and potassium molybdate; Preferably, the concentration of the molybdenum salt solution is 0.01 to 0.1 mol / L; Preferably, the anion salt in the anion salt solution is selected from at least one of H3BO3, NH4Cl, NH4F, and NH4PO4; Preferably, the concentration of the anionic salt solution is 0.2 to 2 mol / L; Preferably, the molar ratio of the molybdenum salt to the anion salt solution is 0.01-1:0.2-2, and the molar amount of the anion salt solution is based on the molar amount of the anion salt.
3. The preparation method according to claim 1, characterized in that: In the step (2), the reaction temperature is 150-200° C. and the reaction time is 10-30 h; Preferably, the drying temperature is 40 to 80° C., and the drying time is 10 to 24 hours.
4. The preparation method according to claim 1, characterized in that: In the step (3), the concentration of copper sulfate is 0.005-0.1 mol / L; Preferably, the concentration of the boric acid is 0.01 to 0.1 mol / L; Preferably, in the electrodeposition treatment, the ratio of copper sulfate to boric acid in the deposition solution is 0.005-0.1:0.01-0.
1.
5. The preparation method according to claim 1, characterized in that: In the step (3), the deposition current during the electrodeposition treatment is -2 to -10 mA cm -2 ; Preferably, the deposition time during the electrodeposition treatment is 200 to 400 seconds.
6. The preparation method according to claim 1, characterized in that: In the step (1), the pretreatment is performed by soaking in a solution containing nitric acid; Preferably, the concentration of the nitric acid is 10 to 50 wt %; Preferably, the soaking time is 10 to 30 minutes; Preferably, the nickel-based material is selected from at least one of nickel foil, nickel foam and nickel felt.
7. The preparation method according to claim 1, characterized in that: In the step (4), the annealing temperature is 300 to 500° C. and the annealing time is 1 to 4 hours; Preferably, the heating rate during the annealing treatment is 2-10° C. / min.
8. The preparation method according to claim 1, characterized in that: In the step (4), the inert atmosphere is selected from at least one of argon and nitrogen.
9. An anion-modified Ni-MoO2 / Cu heterostructure catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the anion-modified Ni-MoO2 / Cu heterostructure catalyst according to claim 9 in catalytic electrochemical hydrogen evolution reaction.
Citation Information
Patent Citations
Self-supporting transition metal-phosphorus alloy catalyst, and preparation method and application thereof
CN105107535A
Copper / cuprous oxide / molybdenum dioxide electrocatalytic material and preparation method and application thereof
CN110180552A
B-P co-doped double-transition metal catalyst as well as preparation method and application thereof
CN111790415A
Bifunctional catalyst for electrochemical hydrogen evolution reaction and urea electrocatalytic oxidation reaction as well as preparation method and application of bifunctional catalyst
CN115896802A
Colloidal-copper based water oxidation electrocatalyst
US20210237037A1