Preparation method of manganese dioxide / cobalt-manganese spinel composite catalyst
The manganese dioxide/cobalt manganese spinel composite catalyst prepared by ion exchange and calcination method solves the problem of high metal leaching of single-component catalysts in acidic water and soil, and achieves efficient degradation of organic pollutants in water and soil. , has the advantages of low cost and reusability.
Patent Information
- Application Number
- CN202410969306.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
AI Technical Summary
Existing single-component catalysts have high leaching concentrations of metals Co and Mn in acidic water and soil, leading to secondary pollution of heavy metal ions, and their catalytic activity is not high, making it difficult to effectively degrade organic pollutants in water and soil.
The manganese dioxide/cobalt manganese spinel composite catalyst was prepared using ion exchange and calcination methods to form an α-MnO2/(Co,Mn)(Co,Mn)2O4 catalyst with a coral-like heterojunction structure. The mutual substitution of points and the interfacial electric field enhance the catalytic activity and increase the specific surface area through morphology control.
It achieves high activity, low metal ion leaching, wide pH range and reusable catalytic effect, which is far better than the simple α-MnO2 catalyst. It can efficiently degrade organic pollutants in water and soil and avoid the secondary release of heavy metal ions. pollute.
Smart Images

Figure CN118719087A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst, and specifically belongs to the technical field of environmental functional materials. Background Art
[0002] Improving ecology and environment is a major issue related to the sustainable development of the economy and society and the improvement of people's quality of life. A wide variety of pollutants enter water bodies and soil, posing a huge threat to human health. Pharmaceuticals and Personal Care Products (PPCPs) are a class of emerging organic pollutants that enter water bodies and soil environments mainly through human or animal excretion, production process waste, medical process waste, etc. PPCPs are characterized by persistence, bioaccumulation and difficulty in degradation. my country is a major producer and consumer of PPCPs. PPCPs are continuously input into the environment, and their residual concentration in the environment is on the rise. Therefore, it is urgent to develop efficient PPCPs pollutant reduction technology. The main technologies for reducing PPCPs pollutants include physical methods, chemical methods and biological methods. Among them, advanced oxidation technology (AOPs) in the chemical method can directly mineralize / decompose PPCPs pollutants or improve the biodegradability of pollutants through oxidation, and has good application prospects. In advanced oxidation technology, compared with the common advanced oxidation process based on hydrogen peroxide activation, the active species produced in the PS-AOPs process based on persulfate (PS) activation have higher redox potential, wider pH solution application range and longer life. In addition, persulfate as an oxidant is more stable than other oxidants, has less environmental pollution and lower cost. Usually, persulfate needs to be activated by other means to produce active species. Commonly used activation methods include: thermal activation, transition metal catalytic activation, photoactivation, ultrasonic activation and microwave activation. Among the many catalysts for activating persulfate, transition metal oxide heterogeneous catalysts have the advantages of high catalytic activity and low secondary pollution.
[0003] Among many transition metal oxides, manganese (Mn) has the advantages of large natural reserves, environmental friendliness, and diverse valence states. Manganese oxides can be transformed into each other during the catalytic process and accompanied by the transfer of single electrons. As a heterogeneous catalyst, it has great application prospects in the field of activating persulfate for water treatment. Saputra et al. (Saputra, E., et al., Manganese oxides at different oxidation states for heterogeneous activation of peroxymonosulfate for phenol degradation in aqueous solutions. Applied Catalysis B: Environmental, 2013, 142-143: 729-735.) found that crystalline nano manganese oxides of different valence states (MnO2, Mn3O4, Mn2O3 and MnO, etc.) can effectively activate persulfate, thereby effectively oxidizing and removing phenol from water; among them, the catalytic activity of MnO2 is better than that of other manganese oxides. In addition, MnO2 has four crystal forms, namely α-MnO2, β-MnO2, γ-MnO2 and δ-MnO2. Shen et al. (Shen ST, et al., Understanding the nonradical activation of peroxymonosulfate by different crystallographic MnO2: The pivotal role of Mn III content on the surface. Journal of Hazardous Materials, 2022, 439: 129613.) It was found that the activity of the above four different crystalline forms of MnO2 in activating persulfate to degrade acetaminophen was α-MnO2>γ-MnO2>β-MnO2>δ-MnO2. It can be seen that in terms of activating persulfate, α-MnO2 exhibits better catalytic activity than other manganese oxides.
[0004] In order to further improve the catalytic activity of α-MnO2 in activating persulfate, α-MnO2 is formed into a heterojunction structure with other metal oxide catalysts, and the interfacial electric field formed at the heterojunction interface is used to accelerate the activation of Mn 3+ / Mn 2+ , Mn 4+ / Mn 3+The catalytic activity of the catalyst can be improved by cycling, and the metal dissolution on the catalyst surface can be effectively inhibited. In addition, the composite can effectively increase the catalytic active sites, and at the same time, the specific surface area can be increased by morphology control to enhance the adsorption and mass transfer effects. The synergistic effect of different metals can also enhance the yield and generation rate of free radicals. Therefore, the composite catalyst formed by the composite of α-MnO2 and other metal (including Fe, Ce, Cu, Mg, Co and Cr, etc., Li Juexiu et al. Research progress on manganese-based catalysts for activation of persulfate to degrade organic wastewater. Environmental Chemistry, 2023, 42 (11): 3861-3877.) oxides usually has better catalytic performance.
[0005] Among the numerous other metal oxides composited with α-MnO2, the active center of Co in the structures of Co3O4, CoMn2O4, etc. has the highest catalytic activity among all metal centers in activated persulfate (Liang H, et al., Excellent performance of mesoporous Co3O4 / MnO2 nanoparticles in heterogeneous activationof peroxymonosulfate for phenol degradation in aqueous solutions. AppliedCatalysis B: Environmental, 2012, 127: 330-335.). In addition, the Co active center can also enhance the overall catalytic activity of the composite catalyst through the synergistic effect with the Mn active center on the surface of α-MnO2. However, although the simple combination of cobalt-containing metal oxides and α-MnO2 can effectively improve its catalytic activity, it still cannot effectively reduce the leaching concentration of metal Co and Mn in the composite catalyst in acidic water and soil, which is easy to cause secondary pollution of heavy metal ions. Therefore, the present invention prepares a manganese dioxide / cobalt manganese spinel composite catalyst (α-MnO2 / (Co,Mn)(Co,Mn)2O4) by ion exchange and calcination for the first time. Based on its unique coral-like morphology, heterogeneous interface structure and mutual substitution of Co and Mn sites in (Co,Mn)(Co,Mn)2O4, the composite catalyst exhibits catalytic activity far superior to that of the simple α-MnO2 catalyst. At the same time, the composite catalyst also has the advantages of low metal ion leaching (<0.5 mg / L), wide pH application range (3-9), and reusability (repeated more than 4 times). Summary of the invention
[0006] The invention provides a method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst. The prepared composite catalyst has high activity, high stability and strong anti-interference ability, can be reused, can completely degrade organic pollutants in water and soil at low cost, and overcomes the problem of low catalytic activity of existing single-component catalysts.
[0007] The invention discloses a method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst, which adopts ion exchange and calcination methods to form a manganese dioxide / cobalt manganese spinel composite catalyst α-MnO2 / (Co, Mn)(Co, Mn)2O4 with a coral-like heterojunction structure through self-assembly of α-MnO2 and (Co, Mn)(Co, Mn)2O4 nanoparticles. The method specifically comprises the following steps: Step 1: The potassium permanganate solution and the divalent manganese salt solution are hydrothermally reacted and then naturally cooled to room temperature. The product is filtered, washed and dried to obtain a precursor powder; Step 2: Add a certain amount of precursor powder to a divalent cobalt salt solution, stir the reaction continuously, filter, wash and dry, and then calcine at 400-700°C to obtain a manganese dioxide / cobalt manganese spinel composite catalyst composed of α-MnO2 and (Co, Mn)(Co, Mn)2O4; wherein the solid-to-liquid ratio of the precursor powder to the divalent cobalt salt solution is 1:50-250 in terms of g / mL.
[0008] The divalent manganese salt is at least one of manganese acetate, manganese sulfate, manganese nitrate, manganese chloride and manganese acetylacetonate.
[0009] The molar ratio of the potassium permanganate to the divalent manganese salt is 6:1.
[0010] The conditions of the hydrothermal reaction are: 120° C., reaction time 6 to 12 hours.
[0011] The divalent cobalt salt is at least one of cobalt nitrate, cobalt acetate, cobalt chloride, cobalt acetylacetonate and ethylenediamine cobalt.
[0012] The mass ratio of manganese to cobalt in the precursor powder and the divalent cobalt salt solution is 105-5:1.
[0013] The stirring reaction is as follows: the stirring speed is 200 to 700 rpm and the reaction time is 6 to 36 hours.
[0014] The calcination time is 60 to 180 minutes.
[0015] The beneficial effects of the invention are as follows: the preparation method of the invention adopts ion exchange and calcination methods, and self-assembles α-MnO2 and (Co, Mn)(Co, Mn)2O4 nanoparticles to form a manganese dioxide / cobalt manganese spinel composite catalyst with a coral-like heterojunction structure. The preparation method is simple, the catalytic activity is high, and the catalyst can efficiently catalyze and activate persulfate to degrade organic pollutants in soil and water. Moreover, the leaching of metal ions is low (<0.5 mg / L), and secondary pollution of heavy metal ions can be avoided. The catalyst has a wide pH application range (3-9) and can be reused (repeated more than 4 times). The catalyst is easy to use, low in cost, and easy to be applied in actual wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 : Powder X-ray diffraction spectrum of the manganese dioxide / cobalt manganese spinel composite catalyst prepared in Example 1 of the present invention; Figure 2 : Scanning electron microscope image of the manganese dioxide / cobalt manganese spinel composite catalyst prepared in Example 1 of the present invention; Figure 3 : A graph showing the degradation of carbamazepine by potassium peroxymonosulfate activated by the manganese dioxide / cobalt manganese spinel composite catalyst prepared in Example 1 of the present invention; Figure 4 : A graph showing the degradation of carbamazepine by potassium peroxymonosulfate activated by four cycles of the manganese dioxide / cobalt manganese spinel composite catalyst prepared in Example 1 of the present invention; Figure 5 : A graph showing the degradation of carbamazepine by activation of potassium peroxymonosulfate at different solution pHs using the manganese dioxide / cobalt manganese spinel composite catalyst prepared in Example 1 of the present invention; Figure 6 : Removal curve of total organic carbon in the process of degrading carbamazepine by potassium peroxymonosulfate activated by manganese dioxide / cobalt manganese spinel prepared in Example 1 of the present invention; Figure 7 : The metal ion leaching concentration of the solution after the manganese dioxide / cobalt manganese spinel prepared in Example 1 of the present invention is activated with potassium peroxymonosulfate to degrade carbamazepine. DETAILED DESCRIPTION
[0017] Example 1 1. Preparation of manganese dioxide / cobalt manganese spinel composite catalyst The specific steps are as follows: (1) Dissolve 6 mmol potassium permanganate and 1 mmol manganese sulfate in 70 mL deionized water, and transfer the resulting mixed solution to a 100 mL stainless steel autoclave with a Teflon liner. Seal the autoclave and place it in an oven at 120°C for 12 hours, then cool naturally to room temperature. Collect the product by vacuum filtration, wash the product with deionized water until it is neutral, and then dry it at 60°C to obtain the precursor; (2) Disperse 1 g of the precursor powder in 250 mL of 6 mM cobalt nitrate hexahydrate solution with a solid-liquid ratio of 1:250, stir continuously at room temperature at a stirring speed of 400 rpm for 6 h, collect the product by vacuum filtration, wash the product with deionized water until neutral, and then dry it at 60 °C for later use; (3) The dried product obtained in (2) is placed in a muffle furnace and calcined in an air atmosphere at 600° C. for 120 minutes. After natural cooling, the collected product is the manganese dioxide / cobalt manganese spinel composite catalyst.
[0018] Depend on Figure 1 The results show that the diffraction peaks at 2θ of 12.8, 18.1, 28.8, 37.5, 41.9, 49.8 and 60.3° correspond to the (110), (200), (310), (211), (301), (411) and (521) crystal planes in α-MnO2 (PDF#44-0141), respectively; the diffraction peaks at 2θ of 29.3, 31.2, 32.8 and 36.3° correspond to the (202), (220), (113) and (311) crystal planes in (Co,Mn)(Co,Mn)2O4 (PDF#18-0408), respectively. It can be seen that the phases of the prepared manganese dioxide / cobalt manganese spinel composite catalyst are α-MnO2 and (Co,Mn)(Co,Mn)2O4.
[0019] pass Figure 2 It can be seen that the synthesized manganese dioxide / cobalt manganese spinel composite catalyst exhibits the morphology of a coral-like structure formed by self-assembly of nanoparticles.
[0020] 2. Application of manganese dioxide / cobalt manganese spinel composite catalyst Catalytic degradation: Manganese dioxide / cobalt manganese spinel composite catalyst is used to activate and degrade organic pollutants in soil and water.
[0021] The degradation process was carried out in a 250 mL beaker, with carbamazepine as the target pollutant and potassium permonosulfate as the oxidant. High performance liquid chromatography was used to test the performance of manganese dioxide / cobalt manganese spinel composite catalyst in activating potassium permonosulfate to degrade carbamazepine.
[0022] The degradation reaction conditions are as follows: at 30°C, 0.02 g of manganese dioxide / cobalt manganese spinel composite catalyst is added to 100 mL of carbamazepine solution with an initial concentration of 20 mg / L for degradation. After stirring evenly, 0.03 g of potassium permonosulfate is added. After the reaction is initiated, the test results show that the degradation rate of carbamazepine reaches 100% within 30 minutes ( Figure 3 ), under the same conditions, the single-component α-MnO2 activated potassium persulfate can only degrade about 30% of carbamazepine. It can be seen that the prepared manganese dioxide / cobalt manganese spinel composite catalyst exhibits a catalytic activity far superior to that of the single-component α-MnO2.
[0023] In addition, by Figure 4 It can be seen that the prepared manganese dioxide / cobalt manganese spinel composite catalyst can still achieve a degradation rate of 100% for carbamazepine after the fourth activation with potassium permonosulfate, indicating that the composite catalyst has good reusability.
[0024] Depend on Figure 5 It can be seen that the prepared manganese dioxide / cobalt manganese spinel composite catalyst can effectively activate potassium permonosulfate to achieve 100% degradation and removal of carbamazepine in the solution pH range of 3-9, indicating that the composite catalyst has a wide pH range of application.
[0025] Depend on Figure 6 It can be seen that the prepared manganese dioxide / cobalt manganese spinel composite catalyst activated potassium permonosulfate to degrade carbamazepine, and the mineralization rate reached 55.5% in 30 minutes.
[0026] Depend on Figure 7 It can be seen that the prepared manganese dioxide / cobalt manganese spinel composite catalyst activated potassium permonosulfate to degrade carbamazepine. After 30 minutes, the leaching concentrations of Co and Mn were 0.3 and 0.005 mg / L, respectively, both lower than the 1 mg / L requirement of the national standard GB25467-2010.
[0027] Example 2 1. Preparation of manganese dioxide / cobalt manganese spinel composite catalyst (1) Dissolve 6 mmol potassium permanganate and 1 mmol manganese sulfate in 70 mL deionized water, and transfer the resulting mixed solution to a 100 mL stainless steel autoclave with a Teflon liner. Seal the autoclave and place it in an oven at 120°C for 10 hours, then cool naturally to room temperature. Collect the product by vacuum filtration, wash the product with deionized water until it is neutral, and then dry it at 60°C to obtain the precursor; (2) Disperse 0.8 g of the precursor powder in 100 mL of 4 mM cobalt acetate solution with a solid-liquid ratio of 1:125. Stir continuously at room temperature at a stirring speed of 500 rpm for 24 h. Collect the product by vacuum filtration, wash the product with deionized water until it is neutral, and then dry it at 60 °C for later use. (3) The dried product obtained in (2) is placed in a muffle furnace and calcined in an air atmosphere at 400° C. for 180 minutes. After natural cooling, the collected product is the manganese dioxide / cobalt manganese spinel composite catalyst.
[0028] 2. Application of manganese dioxide / cobalt manganese spinel composite catalyst Catalytic degradation: Manganese dioxide / cobalt manganese spinel composite catalyst is used to activate and degrade organic pollutants in soil and water.
[0029] The degradation process was carried out in a 250 mL beaker. Carbamazepine was used as the target pollutant and potassium permonosulfate was used as the oxidant. High performance liquid chromatography was used to test the performance of manganese dioxide / cobalt manganese spinel composite catalyst in activating potassium permonosulfate to degrade carbamazepine.
[0030] The degradation reaction conditions are as follows: at 30°C, 0.02 g of manganese dioxide / cobalt manganese spinel composite catalyst is added to 100 mL of carbamazepine solution with an initial concentration of 20 mg / L for degradation. After stirring evenly, 0.03 g of potassium permonosulfate is added. After the reaction is initiated, the test results show that the degradation rate of carbamazepine reaches 85% within 30 minutes.
[0031] Example 3 1. Preparation of manganese dioxide / cobalt manganese spinel composite catalyst (1) Dissolve 6 mmol potassium permanganate and 1 mmol manganese sulfate in 70 mL deionized water, and transfer the resulting mixed solution to a 100 mL stainless steel autoclave with a Teflon liner. Seal the autoclave and place it in an oven at 120°C for 10 hours, then cool naturally to room temperature. Collect the product by vacuum filtration, wash the product with deionized water until it is neutral, and then dry it at 60°C to obtain the precursor; (2) Disperse 2 g of the precursor powder in 300 mL of 6 mM cobalt chloride solution with a solid-liquid ratio of 1:150. Stir continuously at room temperature at a stirring speed of 700 rpm for 24 h. Collect the product by vacuum filtration, wash the product with deionized water until it is neutral, and then dry it at 60 °C for later use. (3) The dried product obtained in (2) is placed in a muffle furnace and calcined in an air atmosphere at 700° C. for 180 minutes. After natural cooling, the collected product is the manganese dioxide / cobalt manganese spinel composite catalyst.
[0032] 2. Application of manganese dioxide / cobalt manganese spinel composite catalyst Catalytic degradation: Manganese dioxide / cobalt manganese spinel composite catalyst is used to activate and degrade organic pollutants in soil and water.
[0033] The degradation process was carried out in a 250 mL beaker. Carbamazepine was used as the target pollutant and potassium permonosulfate was used as the oxidant. High performance liquid chromatography was used to test the performance of manganese dioxide / cobalt manganese spinel composite catalyst in activating potassium permonosulfate to degrade carbamazepine.
[0034] The degradation reaction conditions are as follows: at 30°C, 0.02 g of manganese dioxide / cobalt manganese spinel composite catalyst is added to 100 mL of carbamazepine solution with an initial concentration of 20 mg / L for degradation. After stirring evenly, 0.03 g of potassium permonosulfate is added. After the reaction is initiated, the test results show that the degradation rate of carbamazepine reaches 95% within 30 minutes.
[0035] Note: Project funding: Jiangxi Province Major Discipline and Technology Leader Funding Program (Project No.: 20232BCJ22015, Project Name: Study on the mechanism of selective degradation of PPCPs in water by persulfate activated by oxygen-rich vacancy manganese oxide nanofiber membrane).
Claims
1. A method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst, characterized in that: The preparation method adopts ion exchange and calcination method to form a manganese dioxide / cobalt manganese spinel composite catalyst α-MnO2 / (Co, Mn)(Co, Mn)2O4 with a coral-like heterojunction structure through self-assembly of α-MnO2 and (Co, Mn)(Co, Mn)2O4 nanoparticles; specifically comprises the following steps: Step 1: The potassium permanganate solution and the divalent manganese salt solution are hydrothermally reacted and then naturally cooled to room temperature. The product is filtered, washed and dried to obtain a precursor powder; Step 2: Add a certain amount of precursor powder to a divalent cobalt salt solution, stir the reaction continuously, filter, wash and dry, and then calcine at 400-700°C to obtain a manganese dioxide / cobalt manganese spinel composite catalyst composed of α-MnO2 and (Co, Mn)(Co, Mn)2O4; wherein the solid-to-liquid ratio of the precursor powder to the divalent cobalt salt solution is 1:50-250 in terms of g / mL.
2. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The divalent manganese salt is at least one of manganese acetate, manganese sulfate, manganese nitrate, manganese chloride and manganese acetylacetonate.
3. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The molar ratio of the potassium permanganate to the divalent manganese salt is 6:
1.
4. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The conditions of the hydrothermal reaction are: 120° C., reaction time 6 to 12 hours.
5. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The divalent cobalt salt is at least one of cobalt nitrate, cobalt acetate, cobalt chloride, cobalt acetylacetonate and ethylenediamine cobalt.
6. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The mass ratio of manganese to cobalt in the precursor powder and the divalent cobalt salt solution is 105-5:
1.
7. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The stirring reaction is as follows: the stirring speed is 200 to 700 rpm and the reaction time is 6 to 36 hours.
8. The method for preparing a manganese dioxide / cobalt manganese spinel composite catalyst according to claim 1, characterized in that: The calcination time is 60 to 180 minutes.
Citation Information
Patent Citations
Preparation method of manganese dioxide modified nickel-cobalt spinel catalyst
CN112794375A
Manganese-cobalt catalyst as well as preparation method and application thereof
CN116116425A
Preparation method of carbon nanotube / manganese dioxide composite electrode
WO2020098276A1
Cited By
Wastewater treatment process
CN120483373A
A wastewater treatment process
CN120483373B