Preparation method of CdS-TiO2-NH2-MIL-101 catalyst for photocatalytic CH4 dry reforming

By uniformly wrapping quantum dots of CdS and TiO2 on the surface of the NH2-MIL-101 material, a MOFs-based composite catalyst with a dual-core shell structure CdS-TiO2@NH2-MIL-101 is formed, which solves the problem of easy carbon deposition on the catalyst and fast photogenerated electron recombination rate. problem, improve the conversion efficiency and cycle stability of CO2 and CH4, and achieve efficient photocatalytic CH4 dry reforming.

CN118719142APending Publication Date: 2024-10-01HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311175253.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the current dry reforming process of CH4 driven by solar energy, the catalyst is prone to carbon deposition, coking and deactivation, the recombination rate of photogenerated electrons and holes is fast, and the cycle stability is poor, resulting in low conversion efficiency of CO2 and CH4.

Method used

Design a dual-core-shell structure MOFs-based composite catalyst CdS-TiO2@NH2-MIL-101. The CdS and TiO2 of quantum dots are evenly wrapped on the surface of the NH2-MIL-101 material through the ultrasonic impregnation method to form a synergistic core-shell structure. Improve the number of catalytic active sites and photoelectrochemical performance.

Benefits of technology

It significantly improves the absorbance of the catalyst and the separation rate of photogenerated electrons and holes, enhances the conversion efficiency of CO2 and CH4, achieves high-yield CO and H2 generation, and improves the cycle stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719142A_ABST
    Figure CN118719142A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a CdS-TiO2-coated NH2-MIL-101 catalyst for photocatalytic CH4 dry reforming, and the core-shell structure type NH2-MIL-101-based composite catalyst is characterized in that TiO2 and CdS of quantum dots are dispersed in an organic solvent, and are uniformly wrapped on the surface or in pore channels of NH2-MIL-101 through an ultrasonic impregnation method, so that a special core-shell structure is formed. According to the structure, the synergistic effect among MOF, TiO2 and CdS is well realized, and the absorbance, the photoelectrochemical property and the catalytic active site number of the composite material are improved. In addition, the preparation method of the dual-core-shell CdS-TiO2-NH2-MIL-101 catalyst has the advantages of simplicity in operation, easiness in large-scale preparation, energy conservation, safety and the like. The invention belongs to the field of photocatalysis and energy storage and conversion, and particularly relates to a method for converting two greenhouse gases of CO2 and CH4 into a chemical product with high additional value by utilizing solar energy through a semiconductor material. In addition, the prepared CdS-TiO2 (at) NH2-MIL-101 catalyst with the dual-core-shell structure shows good catalytic performance in the process of photocatalytic CH4 dry reforming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photocatalysis and energy storage and conversion, and specifically relates to the use of solar energy to convert two greenhouse gases, CO2 and CH4, into high-value chemical products through semiconductor materials. Background Art

[0002] The capture, utilization and storage technology of CO2 can realize the efficient utilization of fossil energy and is one of the key technologies for greenhouse gas emission reduction and global low-carbon development. However, the cost of carbon capture in my country is relatively high at this stage. Therefore, it is a very urgent task to develop advanced and energy-saving CO2 utilization technology.

[0003] Methane dry reforming (DRM) can realize the direct conversion and utilization of CH4 and CO2, which is of great significance for carbon emission reduction and resource utilization of CO2-rich natural gas. However, the traditional thermal catalytic conversion of CO2 and CH4 has disadvantages such as easy carbon deposition, coking and deactivation of catalysts, and harsh reaction conditions. The CH4 dry reforming method driven by solar energy is an emerging, green, energy-saving and sustainable CO2 utilization technology, which has attracted widespread attention from researchers.

[0004] In recent years, the new carbon-nitrogen-based composite materials developed and designed by Professor Luo Xiao's team have successfully achieved the rapid conversion of CO2 and CH4 into CO and H2 at room temperature, with the CO yield reaching 36-173.8 μmol g -1 (Luo, et al. Green Energy & Environment, 2021, 6 (6): 938-951; Luo, et al. Catalysis Science & Technology, 2022, 12 (9): 2804-2818; Huang et al. Journal of Energy Chemistry, 2023, 83: 423-432.). Dispersing TiO2 on the surface of 2D C3N4 can increase the number of catalytic active sites and promote the separation efficiency of electrons and holes. Coincidentally, Professor Yin Shuangfeng's team used a dual active site method to couple Pd-loaded boron-doped C3N4 nanosheets with Cu-loaded C3N4 to develop a new Cu-CNN / Pd-BDCNN catalyst. The results showed that the Cu-CNN / Pd-BDCNN catalyst can rapidly convert CO2 and CH4 in a room temperature continuous reactor, with CO and H2 yields of 844.1 and 852.6 μmol g, respectively. -1 (Zhou et al. Advanced Functional Materials, 2023: 2214068). Despite this, it still has disadvantages such as fast recombination rate of photogenerated electrons and holes and poor cycle stability.

[0005] Metal-organic frameworks (MOFs) are considered to be promising photocatalysts due to their good visible light response, high porosity and large specific surface area. However, the recombination rate of photogenerated electrons and holes in MOFs is relatively fast and the number of catalytic active sites is relatively small. To this end, we designed a double core-shell NH2-MIL-101-based composite material to enhance the absorbance of MOFs, inhibit the recombination of carriers to a certain extent, and increase the number of catalytic active sites on the MOFs surface. Summary of the invention

[0006] Technical problem: Develop and design a dual-core-shell structured MOFs-based composite catalyst to increase the absorbance of the NH2-MIL-101 material, the number of catalytic active sites, the separation rate of photogenerated electrons and holes, and to a certain extent suppress the recombination rate of electrons and holes, thereby achieving rapid conversion of CO2 and CH4.

[0007] Technical solution: The technical solution of the present invention is to provide a method for preparing a CdS-TiO2@NH2-MIL-101 catalyst for photocatalytic CH4 dry reforming. The MOFs-based composite photocatalyst with a double core-shell structure is to uniformly wrap quantum dots of CdS and TiO2 on the surface of NH2-MIL-101 (Fe) material by ultrasonic impregnation, and the specific preparation method is as follows.

[0008] (1) 1.24 mmol of 2-aminoterephthalic acid was placed in beaker A containing 7.5 mL of N,N-dimethylformamide (DMF) solution, and the mixed solution was stirred at room temperature for 10 minutes.

[0009] (2) 7.5 mL of DMF solution and 2.497 mmol of FeCl3·6H2O were added to beaker B, and the mixed solution was stirred at room temperature for 10 minutes.

[0010] (3) Then, the liquid in beaker A was dripped into beaker B, and the mixture was transferred to a 50 mL hydrothermal reactor, which was heated in air at 110° C. for 24 hours.

[0011] (4) The obtained reddish-brown suspension was filtered using a centrifuge, washed three times with a DMF solution, and the washed filter cake was dried in air and dried in a vacuum environment at 80° C. for 12 h.

[0012] (5) Typically, HNO3, ethanol, and tetrabutyl titanate solution are placed in a beaker, and the mixed solution is stirred evenly at room temperature for 2 min and then stirred in a water bath at 291.15 K for 20 h.

[0013] (6) The obtained TiO2 quantum dot liquid was evaporated at room temperature and aged in air at 353.15 K to obtain TiO2 quantum dot powder. (7) 1.6 mmol Cd(OAc)2·2H2O and 130 mL dimethyl sulfoxide were added to a beaker, and the mixed solution was uniformly stirred at room temperature for 30 minutes.

[0014] (8) The above substances were then quickly transferred to a hydrothermal reactor and heated in air at 180 °C for 12 h. The hydrothermal reactor was naturally cooled to room temperature, and the resulting suspension was filtered through a centrifuge and washed three times with ethanol and water respectively.

[0015] (9) The obtained solid was dried in air at 100° C. for 12 hours and ground into solid powder to obtain CdS quantum dot powder.

[0016] (10) TiO2 and NH2-MIL-101(Fe) were placed in a beaker containing 10 mL of ethanol solution, ultrasonicated in a water bath for 6-7 h, and then vacuum dried at 80 °C for 12 h and ground into a solid powder to obtain TiO2@NH2-MIL-101(Fe).

[0017] (11) CdS and TiO2@NH2-MIL-101(Fe) were placed in a beaker containing 10 mL of ethanol solution, ultrasonicated in a water bath for 6-7 h, and then heated at 80 °C.

[0018] After vacuum drying for 12 h, the mixture was ground into solid powder to obtain CdS-TiO2@NH2-MIL-101(Fe).

[0019] Preferably, in step (4), the temperature at which the cleaned filter cake is dried in air is controlled at 303.151K.

[0020] Preferably, in step (5), the amounts of HNO3, ethanol and tetra-n-butyl titanate used are 1.4 mL, 120 mL and 2.0 mL respectively.

[0021] Preferably, in step (6), the aging time of TiO2 quantum dots in air at 353.15K is strictly controlled to 1 hour.

[0022] Preferably, in step (10), the solution temperature of the ultrasonic cleaning apparatus is controlled at 323.15K.

[0023] Preferably, in step (11), the solution temperature of the ultrasonic cleaning apparatus is controlled at 323.15K.

[0024] The present invention is to prepare a dual core-shell structure CdS-TiO2@NH2-MIL-101(Fe) composite photocatalyst by ultrasonic impregnation method. It is characterized in that CdS, TiO2 and NH2-MIL-101(Fe) are dispersed in an ethanol solution. Through the interaction of ultrasound and heat, the semiconductor material is uniformly dispersed in the pores or on the surface of NH2-MIL-101, thereby forming a special core-shell structure. This structure well realizes the synergistic effect between MOF, TiO2 and CdS, and improves the absorbance, photoelectrochemical performance and number of catalytic active sites of the composite material. In addition, the method of the dual core-shell CdS-TiO2@NH2-MIL-101 catalyst in the present invention has the advantages of simple operation, easy large-scale preparation, energy saving and safety. In addition, the prepared dual core-shell structure CdS-TiO2@NH2-MIL-101 catalyst shows good catalytic performance in photocatalytic CH4 dry reforming. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : X-ray diffraction pattern (XRD) of the catalyst in Example 1.

[0026] Figure 2 : Scanning electron microscopy (SEM) image of the catalyst in Example 1.

[0027] Figure 3 : Transmission electron microscopy (TEM) image of the catalyst in Example 1.

[0028] Figure 4 : Instantaneous photocurrent response curve (IT) of the catalyst in Example 1.

[0029] Figure 5 : Solid ultraviolet diffuse reflectance spectrum (UV-Vis) of the catalyst in Example 1.

[0030] Figure 6 : Performance diagram of CdS-TiO2@NH2-MIL-101 photocatalytic CH4 dry reforming.

[0031] Figure 7 : Schematic diagram of photocatalytic CH4 dry reforming over dual-core-shell catalysts. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with the embodiments.

[0033] Example 1: TiO2@NH2-MIL-101-60 (NFT-60) catalyst

[0034] Take the preparation process of 60-TiO2@NH2-MIL-101 as an example. First, 60 mg TiO2 and 100 mg NH2-MIL-101 were placed in a beaker containing 10 mL of ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 60-TiO2@MOF (NFT-60).

[0035] Example 2: TiO2@NH2-MIL-101-30 (NFT-30) catalyst

[0036] Take the preparation process of 30-TiO2@NH2-MIL-101 as an example. First, 30 mg TiO2 and 100 mg NH2-MIL-101 were placed in a beaker containing 10 mL of ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 30-TiO2@MOF (NFT-30).

[0037] Example 3: TiO2@NH2-MIL-101-90 (NFT-90) catalyst

[0038] Take the preparation process of 90-TiO2@NH2-MIL-101 as an example. First, 90 mg TiO2 and 100 mg NH2-MIL-101 were placed in a beaker containing 10 mL of ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 90-TiO2@MOF (NFT-90).

[0039] Example 4: 10-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst

[0040] Take the preparation process of 10-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst as an example. First, 10 mg CdS and 100 mg 60-TiO2@MOF were placed in a beaker containing 10 mL ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 10-CdS-TiO2@NH2-MIL-101 (NFTC-10).

[0041] Example 5: 5-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst

[0042] Take the preparation process of 5-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst as an example. First, 5 mg CdS and 100 mg 60-TiO2@MOF were placed in a beaker containing 10 mL ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 5-CdS-TiO2@NH2-MIL-101 (NFTC-5).

[0043] Example 6: 15-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst

[0044] Take the preparation process of 15-CdS-TiO2@NH2-MIL-101 (NFTC-10) catalyst as an example. First, 15 mg CdS and 100 mg 60-TiO2@MOF were placed in a beaker containing 10 mL ethanol solution, ultrasonicated in a water bath for 6-7 h, then vacuum dried at 80 ° C for 12 h, and ground into solid powder to obtain 15-CdS-TiO2@NH2-MIL-101 (NFTC-15).

[0045] Comparative Example 1: NH2-MIL-101 Catalyst

[0046] Typically, 1.24 mmol of 2-aminoterephthalic acid was placed in beaker A containing 7.5 mL of N,N-dimethylformamide (DMF) solution and stirred evenly at room temperature for 10 minutes. Similarly, 7.5 mL of DMF solution, also containing 2.497 mmol of FeCl3·6H2O, was added to beaker B. The mixed solution was stirred at room temperature for 10 minutes. Then, the liquid in beaker A was dripped into beaker B, and the mixture was transferred to a 50 mL hydrothermal reactor. The hydrothermal reactor was heated at 110 ° C in air for 24 hours. The obtained reddish-brown suspension was filtered with a centrifuge and washed three times with DMF solution. The washed filter cake was dried in air at 30 ° C and dried in a vacuum environment at 80 ° C for 12 hours. Finally, it was fully ground into a dynamic solid to obtain NH2-MIL-101 (MOF).

[0047] Comparative Example 2: TiO2 Catalyst

[0048] Typically, 1.4 mL HNO3, 120 mL ethanol and 2.0 mL tetrabutyl titanate solution are placed in a beaker, the mixed solution is stirred evenly at room temperature for 2 min, and then stirred in a water bath at 291.15 K for 20 h. The obtained TiO2 quantum dot liquid is evaporated at room temperature and aged in air at 353.15 K for 1 h to obtain TiO2 quantum dot powder.

[0049] from Figure 1It was observed that NH2-MIL-101 exhibited characteristic peaks at 8.90°, 10.30°, 16.40°, 20.20°, and 24.50°, which is consistent with the data reported in the literature. In addition, TiO2 also had characteristic peaks at 25.34° and 48.040°. It is worth noting that the TiO2@NH2-MIL-101 catalyst has characteristic peaks of both NH2-MIL-101 and TiO2. Compared with NFT-60, CdS-TiO2@NH2-MIL-101 showed new characteristic peaks at 26.2° and 43.90°. This is the result of the interaction between CdS and TiO2@NH2-MIL-101, indicating that CdS is uniformly dispersed on the surface of TiO2@NH2-MIL-101.

[0050] Figure 2 It shows that the morphology of MOF changes greatly after adding TiO2 to the framework of MOF. In addition, the morphology of NFT-60 is similar to an asymmetric ellipse or sphere with a layer of tiny solid particles on it. However, as the mass fraction of TiO2 in NFT increases, the irregularity of the NFT morphology increases, which is related to the complete wrapping of TiO2 on the surface of MOF. After further grafting CdS on NFT-60, it was found that the morphology of CdS-TiO2@NH2-MIL-101 is similar to a solid donut structure, with different solid small particles filled in the outermost layer and the middle.

[0051] Figure 3 It shows that the MOF alone has an octahedral structure, and TiO2 is uniformly wrapped on the MOF surface to form irregular ellipsoidal spheres. CdS was further loaded onto the composite material NFT-60, and it was observed that NFTC-10 formed three layers of concentric circular patterns with different color depths. The SEM characterization results are consistent with this, indicating that CdS was successfully grafted onto the composite material.

[0052] from Figure 4 It was observed that a single MOF material has a weak photocurrent response. Fortunately, grafting TiO2 on MOF can significantly improve the photocurrent response intensity of the composite material. Among them, NFT-60 has the highest photocurrent response intensity among all binary composites. In addition, the ternary hybrid material prepared by combining CNT-60 with a small amount of CdS showed a significant change in the photoresponse intensity, which is almost four times that of NFT-60. The above data show that the introduction of CdS and TiO2 can significantly improve the separation rate of photogenerated electron and hole pairs in the CdS-TiO2@NH2-MIL-101 composite material.

[0053] from Figure 5It can be found that MOF has a strong absorbance in the wavelength range of 380-500nm. When a small amount of TiO2 is loaded on MOF, it can be found that the absorption intensity of NFT-30 in the ultraviolet region decreases, but the absorption capacity in the visible light region increases. Further increasing the mass fraction of TiO2 in MOF, the absorbance of the composite material at 380-800nm ​​is significantly enhanced. Among the binary hybrid materials, NFT-60 exhibits the best light absorption capacity, followed by NFT-90. Interestingly, by adding a small amount of CdS to the structure of NFT-60, it was observed that the absorbance of CdS-TiO2@NH2-MIL-101 decreased at 380-430nm, but the absorbance at 430-800nm ​​increased significantly.

[0054] Application Examples

[0055] Photocatalytic CH4 reforming over CdS-TiO2@NH2-MIL-101

[0056] Usually, 50 mg of catalyst powder is evenly dispersed on the surface of glass fiber filter paper, and the irradiation area is 144.44 cm 2 . The reactor is maintained under negative pressure by a vacuum pump. Then, a mixed gas of CO2 and CH4 provided by a stainless steel compression cylinder is introduced into the reactor and evenly dispersed in the equipment with the help of a pump equipped with the 6A system. Among them, the feed ratio (1:1) of CO2 to CH4 in the mixed gas is controlled by a gas distributor. Then, when the system pressure reaches 40 kPa, the feed gas valve is closed. Then, the photocatalytic performance is measured for 4 hours under the irradiation of a high-pressure xenon lamp (300 W) simulating sunlight. Finally, the reaction products are analyzed by gas chromatography every 30 minutes, and the data are recorded online.

[0057] Table 1 Comparison of photocatalytic CH4 reforming performance of catalysts in Examples and Comparative Examples

[0058] catalyst <![CDATA[Production (CO: μmol g -1 )]]> <![CDATA[Production (H2: μmol g -1 )]]> <![CDATA[OD TiO2]]> 31.16 0 <![CDATA[NH2-MIL-101]]> 126.72 0 <![CDATA[30-TiO2@NH2-MIL-101]]> 291.76 3.88 <![CDATA[60-TiO2@NH2-MIL-101]]> 468.24 8.77 <![CDATA[90-TiO2@NH2-MIL-101]]> 376.45 6.82 <![CDATA[5-CdS-TiO2@NH2-MIL-101]]> 312.88 84.92 <![CDATA[10-CdS-TiO2@NH2-MIL-101]]> 364.46 100.43 <![CDATA[15-CdS-TiO2@NH2-MIL-101]]> 218.98 64.78

[0059] The CO yield of NH2-MIL-101 was 126.7 μmol g -1 , which is 407% higher than the catalytic performance of TiO2. On this basis, the photocatalytic performance of HN2-MIL-10 materials loaded with different masses of TiO2 was studied, such as Figure 6 b. Here, the CO yield of NFT-30 was 291.76 μmol g -1 Importantly, the addition of TiO2 can greatly improve the catalytic performance of MOF. With the increase of TiO2 mass fraction, the photocatalytic performance of TiO2@NH2-MIL-101 hybrid material is greatly enhanced. When the mass fraction of TiO2 is 60%, NFT-60 achieves the best catalytic performance, and the CO yield is 468.24 μmol g-1 The catalytic performance of NFT-90 was second, with a CO yield of 376.45 μmol g -1 .

[0060] Impressively, the H2 production of NFT-30, NFT-60, and NFT-90 was 3.88, 8.77, and 6.82 μmol g -1 . The H2 yield of TiO2@NH2-MIL-101 is lower than expected. This may be related to the type of active sites displayed by the water gas reverse shift reaction and catalyst exposure. Nevertheless, it can still be proved that NFT-60 has the best catalytic efficiency among the five catalysts, which is 1500% and 370% higher than TiO2 and MOF, respectively. Loading a small amount of CdS on the surface of the binary hybrid material NFT-60 solves this defect and improves the efficiency of the composite catalyst in catalytic conversion of CH4. Figure 6 d shows that a small amount of CdS can significantly increase the H2 production in the composite catalyst. Here, the H2 yield of 10%-CdS / TiO2@NH2-MIL-101 is 100.43 μmol g -1 The introduction of CdS into TiO2@NH2-MIL-101 can significantly improve the yield of H2.

Claims

1. The present invention discloses a method for preparing a CdS-TiO2@NH2-MIL-101 catalyst for photocatalytic CH4 dry reforming. The core-shell structure NH2-MIL-101-based composite catalyst is prepared by dispersing quantum dot TiO2 and CdS in an organic solvent and uniformly encapsulating the catalyst by ultrasonic impregnation. On the surface or in the pores of NH2-MIL-101, the preparation method comprises the following steps: (1) 1.24 mmol of 2-aminoterephthalic acid was placed in beaker A containing 7.5 mL of N,N-dimethylformamide (DMF) solution, and the mixed solution was stirred at room temperature for 10 minutes; (2) 7.5 ml of DMF solution and 2.497 mmol of FeCl3·6H2O were added to a beaker, and the mixed solution was stirred at room temperature for 10 minutes; (3) Then, the liquid in beaker A was dripped into beaker B, and the mixture was transferred to a 50 mL hydrothermal reactor, which was heated in air at 110 °C for 24 h; (4) The obtained reddish-brown suspension was filtered by a centrifuge, washed three times with a DMF solution, and the washed filter cake was dried in air and dried in a vacuum environment at 80° C. for 12 h; (5) Typically, HNO3, ethanol, and tetrabutyl titanate solution are placed in a beaker, the mixed solution is stirred evenly at room temperature for 2 min, and then stirred in a water bath at 291.15 K for 20 h; (6) evaporating the obtained TiO2 quantum dot liquid at room temperature and aging it in air at 353.15K to obtain TiO2 quantum dot powder; (7) Add 1.6 mmol Cd(OAC)2·2H2O and 130 mL dimethyl sulfoxide into a beaker, and stir the mixed solution evenly at room temperature for 30 minutes; (8) The above substances were then quickly transferred to a hydrothermal reactor and heated in air at 180°C for 12 h. The hydrothermal reactor was naturally cooled to room temperature. The resulting suspension was filtered through a centrifuge and washed three times with ethanol and water respectively. (9) drying the obtained solid in air at 100° C. for 12 hours and grinding it into a solid powder to obtain CdS quantum dot powder; (10) TiO2 and NH2-MIL-101(Fe) were placed in a beaker containing 10 mL of ethanol solution, subjected to water bath sonication for 6-7 h, and then vacuum dried at 80 °C for 12 h, and ground into a solid powder to obtain TiO2@NH2-MIL-101(Fe); (11) CdS and TiO2@NH2-MIL-101(Fe) were placed in a beaker containing 10 mL of ethanol solution, sonicated in a water bath for 6-7 h, and then vacuum dried at 80 °C for 12 h and ground into a solid powder to obtain CdS-TiO2@NH2-MIL-101(Fe).

2. The preparation method according to claim 1, characterized in that: In step (4), the temperature of the cleaned filter cake during drying in air is controlled at 303.15±1K.

3. The preparation method according to claim 1, characterized in that: In step (5), the amounts of HNO3, ethanol and tetra-n-butyl titanate used are 1.4 mL, 120 mL and 2.0 mL, respectively.

4. The preparation method according to claim 1, characterized in that: In step (6), the aging time of TiO2 quantum dots in air at 353.15K is strictly controlled to be 1 hour.

5. The preparation method according to claim 1, characterized in that: In step (10), the solution temperature of the ultrasonic cleaning apparatus is controlled at 323.15K.

6. The preparation method according to claim 1, characterized in that: In step (11), the solution temperature of the ultrasonic cleaning apparatus is controlled at 323.15K.