Heterogeneous rhodium catalyst for preparing isononanal through diisobutylene hydroformylation as well as method and application of heterogeneous rhodium catalyst

By using a monodentate phospholipid phosphine ligand copolymer to support a rhodium catalyst in the hydroformylation reaction of diisobutylene, the problem of insufficient efficiency and selectivity of the existing catalysts is solved, a high-efficiency, low-cost catalytic effect is achieved, and the process flow is simplified. , suitable for industrial applications.

CN118719149APending Publication Date: 2024-10-01QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410649994.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing rhodium or cobalt catalysts have insufficient efficiency and selectivity in the hydroformylation reaction of diisobutylene, and the loss of the catalyst and product separation increase production costs, making it difficult to achieve industrial application.

Method used

A monodentate phospholipid phosphine ligand copolymer-loaded rhodium catalyst was developed. It was prepared by the impregnation method of Rh precursor and monodentate phospholipid phosphine ligand copolymer. The Rh loading was 0.01%-10%, using argon gas protection and specific The catalyst is prepared under solvent conditions, achieving efficient recovery and reuse of the catalyst.

Benefits of technology

The catalyst exhibits high efficiency and good selectivity in the hydroformylation reaction of diisobutylene, reduces production costs, simplifies the process flow, and improves the recovery rate and stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719149A_ABST
    Figure CN118719149A_ABST
Patent Text Reader

Abstract

The invention discloses a monodentate phosphatide phosphine ligand copolymer supported rhodium catalyst and a preparation method thereof, and a method for preparing isononyl alcohol by catalyzing isomerization hydroformylation of diisobutylene by using the catalyst. According to the catalyst disclosed by the invention, the used raw materials are cheap, the conditions are relatively mild, reagents used in experiments are safe and low in toxicity, and large-scale production can be realized; compared with a bidentate phosphorus ligand polymer, the synthesis process is simpler, the high efficiency of a phospholipid ligand is ensured, meanwhile, the existence of the phosphine ligand stabilizes the polymer structure and further prevents Rh loss, the prefabricated catalyst is high in recovery rate after catalysis is completed, subsequent separation and purification are facilitated, and the selectivity of linear aldehyde is better due to the influence of a substrate structure. Compared with the prior art, on the premise that catalytic activity, selectivity and the like are basically equivalent, the raw material price is lower, the preparation process is simpler, and therefore the production cost can be greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysis and fine chemical industry, and specifically relates to a heterogeneous rhodium catalyst and a preparation method thereof, and use of the catalyst in catalyzing the isomerization and hydroformylation of diisobutylene to prepare isononanol. Background Art

[0002] Isononyl alcohol (INA) is a chemical raw material used to react with phthalic anhydride to produce PVC plasticizer diisononyl phthalate (DINP). DINP is an excellent general-purpose non-toxic plasticizer. Compared with dioctyl phthalate DOP, DINP has better aging resistance, migration resistance, extraction resistance, higher high temperature resistance, light resistance and electrical insulation. In addition, DINP is an excellent general-purpose, non-toxic plasticizer, mainly used in polyvinyl chloride, cellulose acetate, ethyl cellulose and synthetic rubber, and is widely used in toy films, wires and cables. With the market's gradual recognition of the safety of DINP, the demand for DINP as an environmentally friendly substitute for DOP will grow rapidly. The production of isononyl alcohol includes two main steps. The first step is the hydroformylation reaction of diisobutylene to produce isononanal, and the second step is the hydrogenation reduction reaction of isononanal to produce isononyl alcohol.

[0003] In recent years, great progress has been made in the preparation of isononyl alcohol by (isomerization) hydroformylation of diisobutylene (2,4,4-trimethyl-1-pentene monomer or mixture) catalyzed by rhodium or cobalt catalysts, but neither rhodium nor cobalt catalysts can achieve efficient and high-selectivity conversion of diisobutylene. Bidentate phosphine ligand-assisted rhodium catalysts (J.Mol.Catal A:Chem.2002,188,79) can achieve high-selectivity conversion of diisobutylene, indicating that phosphine-containing rhodium catalysts play an important role in the isomerization and hydroformylation of diisobutylene, but the loss of metals and ligands in homogeneous catalysis and the separation of products greatly increase the production cost. In 2022, Shi Feng et al. (J.Phys.Chem.C 2022,126,273) reported the hydroformylation of 2,4,4-trimethyl-1-pentene catalyzed by N-doped carbon-supported CoFe alloy. This catalytic method can achieve high olefin conversion rate and linear aldehyde selectivity, but cannot achieve isomerization of internal olefins and the content of olefin reduction products is very high. The inventors of this application developed an organic molecular cage heterogeneous catalyst containing P skeleton structural units in a previous Chinese invention patent application (application number "202111169177.0". Although the catalyst has good catalytic effect, the catalyst is a bidentate ligand catalyst, the preparation process is relatively complicated, and the raw materials are expensive, which limits its prospects for industrial application. Summary of the invention

[0004] In view of the above-mentioned problems in the prior art, the present application combines the high efficiency and selectivity of organic phosphine ligands, the easy separation and purification of heterogeneous catalysis, and the recycling and reuse of metals, and successfully develops a phosphine ester porous organic polymer-supported rhodium catalyst, which can not only efficiently catalyze the hydroformylation of diisobutylene to prepare linear aldehydes with higher added value, but also can realize the recovery and reuse of the catalyst after the reaction is completed, avoiding the loss of metals and ligands, and having good cyclic catalytic performance. Compared with the previously developed catalyst (Chinese patent application number "202111169177.0", under the premise that the catalytic activity and selectivity are basically the same, the raw material price is lower and the preparation process is simpler, so the production cost can be greatly reduced.

[0005] According to one aspect of the present invention, one of the purposes of the present invention is to provide a novel monodentate phospholipid phosphine ligand copolymer-loaded rhodium catalyst, which is prepared by an impregnation method of a Rh precursor and a monodentate phospholipid phosphine ligand copolymer, wherein the Rh loading is 0.01%-10% of the total mass of the catalyst, preferably 0.11%-5% according to the Rh element; the Rh precursor can be selected from RhBr3, Rh2(SO4)3, Rh(NO3)3, Rh2(OAc)4, Rh4(CO) 12 , Rh(acac)(CO)2, Rh(acac)3, Rh(PPh3)3Br, [Rh(COD)2]BF4, and the structure of the monodentate phospholipid phosphine ligand copolymer can be represented by formula (I):

[0006]

[0007] The monodentate phospholipid phosphine ligand copolymer represented by formula (I) is polymerized by vinyl-functionalized phosphine-containing monomers and triphenylphosphine monomers, wherein m:n=1:0.1 to 1:20, preferably 1:0.2 to 1:15, for example, it can be 1:0.5, 1:1, 1:2.5, 1:5, 1:10 or any range between the above values, and m:n represents the molar ratio of the phospholipid monomer to the triphenylphosphine monomer constituting the monodentate phospholipid phosphine ligand copolymer.

[0008] The structure of formula (I) does not represent the linking order of the monomers. The linking order of the monomers is not fixed and it is a random polymer.

[0009] Among them, R 1 , R 2 , R 3 and R 4The same as or different from each other, and each is independently selected from hydrogen, halogen, cyano, C1-C10 alkyl, C1-C10 alkoxy, C3-C10 cycloalkyl, C6-C14 aryl, an eight- to ten-membered heteroaryl containing 1 to 3 heteroatoms selected from O or N, C6-C14 aryloxy, C1-C3 alkyl C6-C14 aryloxy, C1-C3 alkoxy C6-C14 aryloxy.

[0010] Preferably, R 1 , R 2 , R 3 and R 4 The same as or different from each other, and each is independently selected from hydrogen, halogen, cyano, C1-C4 alkyl, C1-C4 alkoxy, C3-C6 cycloalkyl, C6-C10 aryl, an eight- to ten-membered heteroaryl containing 1 to 2 heteroatoms selected from O or N, C6-C10 aryloxy, C1-C3 alkyl C6-C10 aryloxy, C1-C3 alkoxy C6-C10 aryloxy.

[0011] More preferably, R 1 , R 2 , R 3 and R 4 The same as or different from each other, each independently selected from hydrogen, methyl, ethyl, isopropyl, tert-butyl, cyclopentyl, cyclohexyl, 1-adamantyl, 2-furyl, phenyl, 1-naphthyl and other aromatic groups or hydrogen, fluorine, methyl, ethyl, cyano or methoxy, ethoxy, tert-butoxy, phenoxy, p-methoxyphenoxy, dimethylamino, cyano and the like.

[0012] According to another aspect of the present invention, another object of the present invention is to provide a method for preparing the above-mentioned monodentate phosphine ligand copolymer-loaded rhodium catalyst, which is carried out as follows: under argon protection, a certain amount of Rh precursor and monodentate phosphine ligand copolymer are taken, stirred at a certain temperature in a solvent for 4-8 hours, and the solvent is removed under reduced pressure to obtain the catalyst.

[0013] Preferably, the Ru precursor can be selected from RhBr3, Rh2(SO4)3, Rh(NO3)3, Rh2(OAc)4, Rh4(CO) 12 , Rh(acac)(CO)2, Rh(acac)3, Rh(PPh3)3Br, [Rh(COD)2]BF4, preferably Rh4(CO) 12 .

[0014] Preferably, the mass fraction of Rh loading is 0.01%-10%, preferably 0.11%-5%.

[0015] Preferably, the solvent is selected from n-hexane, dichloromethane, ethyl acetate, tetrahydrofuran, 1,4-dioxane, benzene, acetonitrile, methanol, ethanol, toluene, preferably 1,4-dioxane and toluene.

[0016] Preferably, the temperature is 0°C-150°C, preferably 10°C-50°C.

[0017] The preparation method of the monodentate phospholipid phosphine ligand copolymer is as follows: Under argon protection, a certain amount of vinyl functionalized phosphine-containing polymerization monomer is taken and a certain amount of triphenylphosphine comonomer Dissolve in 1,4-dioxane, add a certain amount of free radical initiator, and stir the reaction at a certain temperature for 24-48 hours.

[0018] Among them, the substituent R 1 , R 2 , R 3 and R 4 The definition of is the same as in formula (I).

[0019] Preferably, the molar ratio of the phosphine-containing polymer monomer to the triphenylphosphine comonomer is 1:0.1 to 1:20, preferably 1:0.2 to 1:15.

[0020] Preferably, the amount of the initiator used is 0.1% to 5%, preferably 1%, based on the molar amount of vinyl groups in the raw material.

[0021] Preferably, the free radical initiator is selected from one or more of benzoyl peroxide, tert-butyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, cyclohexanone peroxide, diisopropyl peroxydicarbonate, azobisisobutyronitrile, potassium persulfate, ammonium persulfate, and hydrogen peroxide, preferably tert-butyl peroxide or cyclohexanone peroxide.

[0022] Preferably, the reaction temperature is 50°C-150°C, preferably 80°C-100°C.

[0023] The preparation method of the vinyl functionalized phosphine-containing polymerized monomer is as follows:

[0024]

[0025] Among them, R 1 , R 2 , R 3 and R 4 The definition of is the same as in formula (I).

[0026] Step 1: Take compound A, Pd(PPh3)4 and R 1The substituted boric acid was added to the reactor, dissolved in DME / H2O, and reacted under reflux stirring for 24 hours. The solvent was removed under reduced pressure, and the obtained brown oily liquid was distilled to obtain a colorless oily compound B.

[0027] Step 2: Add compound B, PCl3 and TEA into a reaction bottle, add THF to dissolve, stir and react at room temperature for 8 hours, remove the solvent under reduced pressure, and separate by column chromatography to obtain a functionalized phosphine-containing polymer monomer (compound C).

[0028] Step 3: Add compound D and n-butyl lithium to a reaction bottle, add THF to dissolve, stir and react at -40°C for 3 hours, add PCl3, stir and react at 50°C for 2 hours. Add hydrochloric acid aqueous solution to adjust the pH to acidic, continue stirring for 30 minutes, filter, wash with water, and separate the filter cake by column chromatography to obtain yellow solid compound E.

[0029] Step 4: Add tert-butyl peroxide and compounds C and E to a dry Shrek tube, seal the tube under argon protection, and react at 80°C for 48 hours. Cool to room temperature, add methanol for precipitation, filter, wash with methanol, and dry in vacuo. The polymer represented by formula (I) is obtained as a white solid.

[0030] Another object of the present invention is to provide the use of the monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst in catalyzing the isomerization hydroformylation of dimerized isobutylene to prepare isononanal.

[0031] Another object of the present invention is to provide a method for preparing isononanal by catalyzing the isomerization hydroformylation of dimeric isobutylene using the monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to the present invention, the method being carried out as follows:

[0032] A certain amount of monodentate phospholipid phosphine ligand copolymer loaded rhodium catalyst and olefin compound prepared according to the present invention are added to an autoclave, replaced with synthesis gas (CO / H2=1:1) for 3 times, and then 2-8 MPa of synthesis gas is introduced, the reaction is stirred at a certain temperature for a certain time, and then the temperature is lowered and the gas is released.

[0033] Preferably, the olefin compound is selected from diisobutylene.

[0034] Preferably, the molar ratio of the olefin compound to Rh is 1000:1 to 30000:1, preferably 10000:1.

[0035] Preferably, the pressure of the synthesis gas is 2-8 MPa, preferably 4-6 MPa.

[0036] Preferably, the reaction temperature is 60-120°C, preferably 80-100°C.

[0037] Preferably, the reaction time is 1 to 24 hours, preferably 5 to 12 hours.

[0038] Beneficial Effects

[0039] Compared with the prior art, the present invention has the following advantages:

[0040] 1. In the synthesis of monodentate phosphite monomers and copolymers, the raw materials used are cheap, the conditions are relatively mild, the reagents used in the experiment are safe and have low toxicity, and large-scale production can be achieved; the polymer uses tri(4-vinylphenyl)phosphine as a comonomer, has more polymerization sites, and the formed polymer has a higher molecular weight and is easier to recycle and reuse.

[0041] 2. Compared with bidentate phosphorus ligand polymers, its synthesis process is simpler, ensuring the high efficiency of phospholipid ligands. At the same time, the presence of phosphine ligands stabilizes the polymer structure and further prevents Rh loss. The prefabricated catalyst has a high recovery rate after catalysis, which is conducive to subsequent separation and purification. Influenced by the substrate structure, the selectivity of linear aldehydes is better.

[0042] 3. In the isomerization hydroformylation reaction of diisobutylene, the phospholipid phosphine ligand copolymer-supported rhodium catalyst of the present invention exhibits a very good swelling effect in the solvent, making the catalytic sites more exposed, thereby exhibiting a better catalytic effect.

[0043] 4. The low temperature, low synthesis gas pressure, short reaction time and low catalyst loading (0.1 mol%) used in the isomerization hydroformylation of diisobutylene indicate that the catalyst has excellent catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0045] Figure 1 This is the adsorption analysis curve of the phospholipid phosphine ligand copolymer prepared in Preparation Example 11.

[0046] Figure 2 This is the pore size distribution diagram of the phospholipid phosphine ligand copolymer-loaded Rh catalyst prepared in Preparation Example 11.

[0047] Figure 3 This is a scanning electron microscope image of the phospholipid phosphine ligand copolymer-loaded Rh catalyst prepared in Preparation Example 11.

[0048] Figure 4 This is a transmission electron micrograph of the phospholipid phosphine ligand copolymer-loaded Rh catalyst prepared in Preparation Example 11.

[0049] Figure 5 This is the solid state NMR carbon spectrum of the phospholipid phosphine ligand copolymer loaded with Rh catalyst prepared in Preparation Example 11.

[0050] Figure 6 This is the thermogravimetric analysis spectrum of the phospholipid phosphine ligand copolymer loaded with Rh catalyst prepared in Preparation Example 11. DETAILED DESCRIPTION

[0051] Hereinafter, the preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the appended claims should not be interpreted as limited to the general and dictionary meanings, but should be interpreted based on the principle of allowing the inventor to appropriately define the terms for the best interpretation, based on the meaning and concept corresponding to the technical level of the present invention. Therefore, the description herein is only a preferred example for illustrative purposes, and is not intended to limit the scope of the present invention, so it should be understood that other equivalent implementations and modifications can be made without departing from the spirit and scope of the present invention.

[0052] The following examples are only listed as examples of embodiments of the present invention and do not constitute any limitation to the present invention. It can be understood by those skilled in the art that modifications within the scope of the essence and concept of the present invention fall within the scope of protection of the present invention. Unless otherwise specified, the reagents and instruments used in the following examples are all commercially available products.

[0053] In this document, the terms "include", "including", "have", "contain" or any other similar terms are open conjunctions, which are intended to cover non-exclusive inclusions. For example, a composition or product containing multiple elements is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or product. In addition, unless otherwise explicitly stated, the term "or" refers to an inclusive "or" rather than an exclusive "or". For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and A and B are both true (or exist). In addition, in this document, the interpretation of the terms "include", "including", "have", and "contain" should be considered to have been specifically disclosed and simultaneously cover closed or semi-closed conjunctions such as "consisting of" and "consisting essentially of".

[0054] In this article, all features or conditions defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible secondary ranges and individual values ​​within the range, especially integer values. For example, the range description of "1 to 8" should be deemed to have specifically disclosed all secondary ranges such as 1 to 7, 2 to 8, 2 to 6, 3 to 6, 4 to 8, 3 to 8, etc., especially secondary ranges defined by all integer values, and should be deemed to have specifically disclosed individual values ​​such as 1, 2, 3, 4, 5, 6, 7, 8, etc. within the range. Unless otherwise specified, the above interpretation method applies to all contents of the entire present invention, regardless of whether the range is broad or not.

[0055] If the quantity or other numerical value or parameter is expressed as a range, a preferred range or a series of upper and lower limits, it should be understood that all ranges consisting of any upper limit or preferred value of the range and the lower limit or preferred value of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.

[0056] In this document, under the premise of achieving the purpose of the invention, numerical values ​​should be understood to have the accuracy of the number of significant digits of the numerical value. For example, the number 40.0 should be understood to cover the range from 39.50 to 40.49.

[0057] Instruments used for material characterization:

[0058] (1) Gel chromatography: Model: HELEOS System, manufactured by Wyatt Corporation, USA

[0059] (2) Physical adsorption instrument: model: autosorb iQ, manufactured by Quantachrome Instruments, Inc.

[0060] (3) Cold field emission scanning electron microscope: Model S-4800, manufactured by Hitachi, Japan

[0061] (4) Transmission electron microscope: Model H-7650, manufactured by Hitachi, Japan

[0062] (5) Synchronous thermogravimetry-differential scanning calorimeter: Model STA449F5jupiter, manufactured by NETZSCH, USA

[0063] (6) Wide-cavity solid-state nuclear magnetic resonance spectrometer: model Bruker 400M, manufactured by Bruker Corporation, Switzerland

[0064] Example

[0065] Example 1: Preparation of Compound B

[0066] Under argon protection, DME / H2O (100 mL), 4-bromophenol (5 g, 1.0 eq), and vinylboronic acid pinacol ester (5.97 g, 1.2 eq) were added to a 250 mL three-necked flask, stirred for 5 minutes, and Pd(PPh3)4 (33 mg, 0.001 eq) was added at room temperature, and the mixture was stirred under reflux for 24 h. After filtration, the filter cake was washed with THF, the filtrate was evaporated to dryness, and separated by column chromatography to obtain 3.1 g of colorless oily liquid (Compound B). 1 H NMR (400MHz, CDCl3) δ9.66 (s, 1H), 7.44 (d, J = 8.3Hz, 2H), 6.72 (dd, J = 17.7, 3.1Hz, 1H ), 6.57 (d, J = 8.3Hz, 2H), 5.82 (dd, J = 17.7, 1.4Hz, 1H), 5.28 (dd, J = 11.1, 1.3Hz, 1H); 13 C NMR (101MHz, CDCl3) δ157.3,136.7,136.2,130.5,115.3,114.2.

[0067] Example 2: Preparation of Compound C

[0068] Take a 100mL three-necked flask, under argon protection, add compound PCl3 (145μL, 1.67mmol, 1eq) to a THF (30mL) solution containing compound B (600mg, 5.0mmol, 3eq) prepared in Example 1 and TEA (697μL, 3eq), and react at room temperature for 30min. Add 50mL of water to quench, extract twice with 30mL of EA, rotary evaporate, and separate by column chromatography to obtain 587mg of white solid (compound C). 1 H NMR (400MHz, CDCl3) δ7.38(d,J=8.3Hz,2H),7.11(d,J=8.2Hz,2H),6.69(dd,J=17.5,3.2Hz,1H),5.82(dd,J=17.7,1.4Hz,1H),5.28(dd,J=11.1,1.3Hz,1H); 13 C NMR (101MHz, CDCl3) δ150.1,134.9,132.9,126.5,119.7,112.3; 31 P NMR (162MHz,CDCl3)δ127.6.

[0069] Example 3: Preparation of Compound E

[0070] Take a 250mL three-necked flask, add compound D (5g, 1eq), ultra-dry THF (100mL), and n-butyl lithium (30mL, 1.2eq), and stir and react at -40°C for 1h under argon protection. Add PCl3 (868μL, 0.25eq) to the above reaction solution, stir and react at 50°C for 2h. Add hydrochloric acid aqueous solution to adjust the pH to acidic, stir for 30 minutes, filter, wash with water, and separate the filter cake by column chromatography to obtain 4.2g of solid (compound E).

[0071] Example 4: Preparation of phospholipid phosphine ligand copolymer SPL-P-0.5

[0072] Under argon protection, 500 mg of compound C, 219 mg of tri(4-vinylphenyl)phosphine and 10 mg of tert-butyl peroxide were added to a reaction bottle, 5 ml of THF was added to dissolve, and the mixture was transferred to a hydrothermal reactor and reacted at 80°C for 48 hours. The mixture was cooled to room temperature, methanol was added to disperse the mixture, and the mixture was filtered and dried to obtain 702 mg of phospholipid phosphine ligand copolymer.

[0073] Example 5: Preparation of phospholipid phosphine ligand copolymer SPL-P-1

[0074] Under argon protection, 500 mg of compound C, 438 mg of tri(4-vinylphenyl)phosphine and 13 mg of tert-butyl peroxide were added to a reaction bottle, 8 ml of THF was added to dissolve, and the mixture was transferred to a hydrothermal reactor and reacted at 80°C for 48 hours. The mixture was cooled to room temperature, methanol was added to disperse the mixture, and the mixture was filtered and dried to obtain 910 mg of phospholipid phosphine ligand copolymer.

[0075] Example 6: Preparation of phospholipid phosphine ligand copolymer SPL-P-2.5

[0076] Under argon protection, 300 mg of compound C, 657 mg of tri(4-vinylphenyl)phosphine and 14 mg of tert-butyl peroxide were added to a reaction bottle, 9 ml of THF was added to dissolve, and the mixture was transferred to a hydrothermal reactor and reacted at 80°C for 48 hours. The mixture was cooled to room temperature, methanol was added to disperse the mixture, and the mixture was filtered and dried to obtain 922 mg of phospholipid phosphine ligand copolymer.

[0077] Example 7: Preparation of phospholipid phosphine ligand copolymer SPL-P-5

[0078] Under argon protection, 200 mg of compound C, 876 mg of tri(4-vinylphenyl)phosphine and 16 mg of tert-butyl peroxide were added to a reaction bottle, 12 ml of THF was added to dissolve, and the mixture was transferred to a hydrothermal reactor and reacted at 80°C for 48 hours. The mixture was cooled to room temperature, methanol was added to disperse the mixture, and the mixture was filtered and dried to obtain 1.01 g of phospholipid phosphine ligand copolymer.

[0079] Example 8: Preparation of phospholipid phosphine ligand copolymer SPL-P-10

[0080] Under argon protection, 100 mg of compound C, 876 mg of tri(4-vinylphenyl)phosphine and 15 mg of tert-butyl peroxide were added to a reaction bottle, 10 ml of THF was added to dissolve, and the mixture was transferred to a hydrothermal reactor and reacted at 80°C for 48 hours. The mixture was cooled to room temperature, methanol was added to disperse the mixture, and the mixture was filtered and dried to obtain 938 mg of phospholipid phosphine ligand copolymer.

[0081] Example 9: Preparation of phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-P-0.5

[0082] Under argon protection, 500 mg of phospholipid phosphine ligand copolymer SPL-P-0.5 was dispersed in 30 ml of tetrahydrofuran, and 9 mg of Rh4(CO) was added. 12 , stirred at room temperature for 24 h, and the solvent was removed under reduced pressure to obtain 490 mg of phospholipid phosphine ligand copolymer-supported rhodium-based catalyst.

[0083] Example 10: Preparation of phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-P-1

[0084] Under argon protection, 500 mg of phospholipid phosphine ligand copolymer SPL-P-1 was dispersed in 30 ml of tetrahydrofuran, and 9 mg of Rh4(CO) was added. 12 , stirred at room temperature for 24 h, and the solvent was removed under reduced pressure to obtain 495 mg of phospholipid phosphine ligand copolymer-supported rhodium-based catalyst.

[0085] Example 11: Preparation of phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-P-2.5

[0086] Under argon protection, 500 mg of phospholipid phosphine ligand copolymer SPL-P-2.5 was dispersed in 30 ml of tetrahydrofuran, and 10 mg of Rh4(CO) was added. 12 , stirred at room temperature for 24 h, and the solvent was removed under reduced pressure to obtain 500 mg of phospholipid phosphine ligand copolymer-supported rhodium-based catalyst.

[0087] The molecular weight of the phospholipid phosphine ligand copolymer prepared in this embodiment is 40000-80000 g / mol, and the degree of polymerization m+n is about 85 to 210. The specific surface area is 527.6 m 2 / g, pore volume 0.078cm 3 / g. By Figure 3 Scanning electron microscopy shows that the polymer is porous, which is conducive to the catalytic reaction. Figure 5 It can be seen from the solid-state NMR spectrum that the phospholipid ligand monomer and tri(4-vinylphenyl)phosphine underwent a polymerization reaction, and the phosphorus atoms were not oxidized and existed in a trivalent state, which ensured the effectiveness of the coordination between the phosphorus atoms and the rhodium atoms, thus indirectly reflecting the reason why this ligand has high activity. Figure 6This is the thermogravimetric analysis curve of the phospholipid phosphine ligand copolymer loaded with Rh catalyst. From this curve, it can be seen that the polymer is stable within 240℃, and there is a 10% weight loss between 240℃-400℃, which is caused by the instability of the OP bond and the high temperature bond breaking. Therefore, the temperature of the catalytic reaction using this polymer should not be too high and should be controlled within 240℃. There is about 20% mass loss between 400℃-600℃, which is caused by the thermal decomposition of other chemical bonds.

[0088] Example 12: Preparation of phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-P-5

[0089] Under argon protection, 500 mg of phospholipid phosphine ligand copolymer SPL-P-5 was dispersed in 30 ml of tetrahydrofuran, and 11 mg of Rh4(CO) was added. 12 , stirred at room temperature for 24 h, and the solvent was removed under reduced pressure to obtain 488 mg of phospholipid phosphine ligand copolymer-supported rhodium-based catalyst.

[0090] Example 13: Preparation of phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-P-10

[0091] Under argon protection, 500 mg of phospholipid phosphine ligand copolymer SPL-P-10 was dispersed in 30 ml of tetrahydrofuran, and 11 mg of Rh4(CO) was added. 12 , stirred at room temperature for 24 h, and the solvent was removed under reduced pressure to obtain 502 mg of phospholipid phosphine ligand copolymer-supported rhodium-based catalyst.

[0092] Application Examples 1-4: Effect of Temperature

[0093] In a glove box, 18 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-P-0.5 prepared in Preparation Example 9, 8 mmol of diisobutylene and 4 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 2 MPa of synthesis gas was introduced, and the reaction was stirred at 90-120°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0094] The specific substrate conversion rate and aldehyde selectivity are shown in Table 1:

[0095] Table 1

[0096]

[0097] From the data in Table 1, it can be seen that under the catalysis of the phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-0.5, diisobutylene isomerization hydroformylation can be achieved at 90-120°C, and the conversion rate is highest at 110°C. Below 110°C, the conversion rate of diisobutylene decreases, but its selectivity for linear aldehydes is very high; above 110°C, both the conversion rate of diisobutylene and the selectivity for linear aldehydes decrease, and more olefin hydrogenation and aldehyde hydrogenation products are generated.

[0098] Application Examples 5-8: Effect of Catalyst

[0099] In a glove box, 18-22 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-0.5-10 prepared in Preparation Examples 9-13, 8 mmol of diisobutylene and 4 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) 3 times, and then 2 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0100] The specific substrate conversion rate and aldehyde selectivity are shown in Table 2:

[0101] Table 2

[0102]

[0103] Comparing the data of Application Examples 3 and 5-8, it can be seen that the conversion rates of diisobutylene for different catalysts are all high, and the selectivity of different catalysts for linear aldehydes is very good. Among them, the catalyst Rh@SPL-P-2.5 provides the best solution for the isomerization hydroformylation of diisobutylene.

[0104] Application Examples 9-12: Effect of Pressure

[0105] In a glove box, 20 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-2.5 prepared in Preparation Example 11, 8 mmol of diisobutylene and 4 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 3-6 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0106] The specific substrate conversion rate and aldehyde selectivity are shown in Table 3:

[0107] Table 3

[0108]

[0109] Comparing the application examples 6 and 9-12, it can be seen that the conversion rate of diisobutylene gradually increases with the increase of pressure, but the selectivity of the product aldehyde shows a trend of first increasing and then decreasing, and the results are not much different under the synthesis gas pressure of 2-5 MPa. However, the conversion rate and the selectivity of linear aldehyde are most ideal at 4 MPa. Therefore, 4 MPa is selected as the optimal reaction pressure.

[0110] Application Examples 13-16: Effect of Solvent

[0111] In a glove box, 20 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-2.5 prepared in Preparation Example 11, 8 mmol of diisobutylene and 4 mL of solvent were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0112] The specific substrate conversion rate and aldehyde selectivity are shown in Table 4:

[0113] Table 4

[0114]

[0115]

[0116] Comparison of application examples 10 and 13-16 shows that the change of solvent has no significant effect on the conversion rate of diisobutylene, but the selectivity of linear aldehydes shows different trends, that is, the selectivity of linear aldehydes in non-polar solvents is better, and the selectivity of linear aldehydes in polar solvents is poor. Therefore, toluene is selected as the solvent.

[0117] Application Examples 17-19: Effect of Concentration

[0118] In a glove box, 20 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-2.5 prepared in Preparation Example 11, 8 mmol of diisobutylene and 2-16 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0119] The specific substrate conversion rate and aldehyde selectivity are shown in Table 5:

[0120] Table 5

[0121]

[0122] Comparison of application examples 10 and 17-19 shows that the concentration change has a greater impact on the conversion rate of diisobutylene, and both too high and too low concentrations will lead to a decrease in the conversion rate, but the concentration has a smaller effect on the selectivity of linear aldehydes. Overall, the experimental results are better when the substrate concentration is 2 mmol / L.

[0123] Application Examples 20-22: Effect of Catalyst Amount

[0124] In a glove box, 20 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-2.5 prepared in Preparation Example 11, 8 mmol of diisobutylene and 2-16 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0125] The specific substrate conversion rate and aldehyde selectivity are shown in Table 6:

[0126] Table 6

[0127]

[0128]

[0129] Comparison of application examples 10 and 20-22 shows that the conversion rate of diisobutylene gradually increases with the increase of catalyst content, but the amount of catalyst has no significant effect on the selection of linear aldehyde. Overall, the experimental results are better when the catalyst amount is 0.1 mol%.

[0130] Application Examples 23-25: Comparison of No Ligand, Bidentate Ligand Monomer and Bidentate Ligand Polymer

[0131] In a glove box, commercial or prepared in Example 11, phospholipid phosphine ligand copolymer supported rhodium catalyst Rh@SPL-2.5, 8 mmol of diisobutylene and 4 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0132] The specific substrate conversion rate and aldehyde selectivity are shown in Table 7:

[0133] Table 7

[0134]

[0135] By comparing the application examples 10 and 23-25, it can be seen that the conversion rate of diisobutylene and the selectivity of linear aldehydes without ligand promotion are poor, and the proportion of branched aldehydes and olefin reduction products is relatively large. Therefore, the pure Rh4(CO) 12 The catalytic effect is not good. Compared with the bidentate ligand monomer and the bidentate ligand polymer, the conversion rate of diisobutylene and the selectivity of linear aldehyde are not much different. However, considering the separation of products and the recycling of catalysts and metals, we believe that the bidentate ligand polymer has a better effect.

[0136] Application Examples 17-21: Effect of Cycle Number

[0137] In a glove box, 20 mg of the phospholipid phosphine ligand copolymer-supported rhodium catalyst Rh@SPL-2.5 prepared in Preparation Example 11, 8 mmol of diisobutylene and 4 mL of toluene were added to an autoclave, the autoclave was sealed, the gas was replaced with synthesis gas (CO / H2) three times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the pressure was released, the reactor was opened, and the analysis was performed by gas chromatography.

[0138] The catalyst was separated by centrifugation, washed with a small amount of toluene, and the recovered catalyst was added to the reactor, 8 mmol of diisobutylene was added, the autoclave was sealed, the gas was replaced with hydrogen 3 times, and then 4 MPa of synthesis gas was introduced, and the reaction was stirred at 110°C for 12 hours. The temperature was lowered, the gas was released, and the reactor was opened for gas chromatography. The catalyst was used 5 times in a cycle.

[0139] The specific substrate conversion rate and aldehyde selectivity are shown in Table 8:

[0140] Table 8

[0141]

[0142] Comparison of application examples 10 and 17-20 shows that as the number of cycles increases, the conversion rate of diisobutylene gradually decreases, but the selectivity of linear aldehydes does not change significantly. The conversion rate of diisobutylene in 5 cycles is above 98% and the selectivity of linear aldehydes remains unchanged, which shows that this catalyst has good cycle performance.

[0143] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst, wherein the Rh loading is 0.01%-10%, preferably 0.11%-5%, of the total mass of the catalyst, calculated as the Rh element, and the structure of the monodentate phospholipid phosphine ligand copolymer can be represented by formula (I): The monodentate phospholipid phosphine ligand copolymer represented by formula (I) is polymerized from vinyl-functionalized phosphine-containing monomers and triphenylphosphine monomers, wherein m:n=1:0.1 to 1:20, preferably 1:0.2 to 1:15, for example, 1:0.5, 1:1, 1:2.5, 1:5, 1:10 or any range between the above values, and m:n represents the molar ratio of the phospholipid monomer to the triphenylphosphine monomer constituting the monodentate phospholipid phosphine ligand copolymer; The structure of formula (I) does not represent the linking order of each monomer. The linking order of each monomer is not fixed and is a random polymer. in, R 1 , R 2 , R 3 and R 4 The same as or different from each other, and each is independently selected from hydrogen, halogen, cyano, C1-C10 alkyl, C1-C10 alkoxy, C3-C10 cycloalkyl, C6-C14 aryl, an eight- to ten-membered heteroaryl containing 1 to 3 heteroatoms selected from O or N, C6-C14 aryloxy, C1-C3 alkyl C6-C14 aryloxy, C1-C3 alkoxy C6-C14 aryloxy.

2. The monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 1, It is characterized in that Preferably, R 1 , R 2 , R 3 and R 4 are the same as or different from each other, and are each independently selected from hydrogen, halogen, cyano, C1-C4 alkyl, C1-C4 alkoxy, C3-C6 cycloalkyl, C6-C10 aryl, an eight- to ten-membered heteroaryl containing 1 to 2 heteroatoms selected from O or N, C6-C10 aryloxy, C1-C3 alkyl C6-C10 aryloxy, C1-C3 alkoxy C6-C10 aryloxy; More preferably, R 1 , R 2 , R 3 and R 4 The same as or different from each other, each independently selected from hydrogen, methyl, ethyl, isopropyl, tert-butyl, cyclopentyl, cyclohexyl, 1-adamantyl, 2-furyl, phenyl, 1-naphthyl and other aromatic groups or hydrogen, fluorine, methyl, ethyl, cyano or methoxy, ethoxy, tert-butoxy, phenoxy, p-methoxyphenoxy, dimethylamino, cyano and the like.

3. The method for preparing a monodentate phosphine ligand copolymer-supported rhodium catalyst according to claim 1 or 2, wherein the method is carried out as follows: under argon protection, a certain amount of Rh precursor and monodentate phosphine ligand copolymer are taken, stirred at a certain temperature in a solvent for 4-8 hours, and the solvent is removed under reduced pressure to obtain the catalyst.

4. The method for preparing the monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 3, It is characterized in that Preferably, the Ru precursor can be selected from RhBr 3 , Rh 2 (SO 4 ) 3 、Rh(NO 3 ) 3 , Rh 2 (OAc) 4 , Rh 4 (CO) 12 、Rh(acac)(CO) 2 、Rh(acac) 3 、Rh(PPh 3 ) 3 Br, [Rh(COD) 2 ]BF 4 One or more of, preferably Rh 4 (CO) 12 ; Preferably, the loading mass fraction of Rh is 0.01%-10%, preferably 0.11%-5%; Preferably, the solvent is selected from n-hexane, dichloromethane, ethyl acetate, tetrahydrofuran, 1,4-dioxane, benzene, acetonitrile, methanol, ethanol, toluene, preferably 1,4-dioxane and toluene; Preferably, the temperature is 0°C-150°C, preferably 10°C-50°C.

5. The monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 1, It is characterized in that The preparation method of the monodentate phospholipid phosphine ligand copolymer is as follows: Under argon protection, a certain amount of vinyl functionalized phosphine-containing polymerization monomer is taken and a certain amount of triphenylphosphine comonomer Dissolve in 1,4-dioxane, add a certain amount of free radical initiator, and stir at a certain temperature for 24-48 hours; Among them, the substituent R 1 , R 2 , R 3 and R 4 The definition of is the same as in formula (I) of claim 1.

6. The monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 5, It is characterized in that Preferably, the molar ratio of the phosphine-containing polymer monomer to the triphenylphosphine comonomer is 1:0.1 to 1:20, preferably 1:0.2 to 1:15; Preferably, the amount of initiator used is 0.1% to 5% of the molar amount of vinyl in the raw material, preferably 1%; Preferably, the free radical initiator is selected from one or more of benzoyl peroxide, tert-butyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, cyclohexanone peroxide, diisopropyl peroxydicarbonate, azobisisobutyronitrile, potassium persulfate, ammonium persulfate, and hydrogen peroxide, preferably tert-butyl peroxide or cyclohexanone peroxide; Preferably, the reaction temperature is 50°C-150°C, preferably 80°C-100°C.

7. The monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 1, It is characterized in that The preparation method of the vinyl functionalized phosphine-containing polymerized monomer is as follows: Among them, R 1 , R 2 , R 3 and R 4 The definition is the same as that of formula (I) in claim 1; Step 1: Take compound A, Pd(PPh 3 ) 4 and R 1 The substituted boric acid was added to the reactor and DME / H 2 O was dissolved, refluxed and stirred for 24 hours, the solvent was removed under reduced pressure, and the obtained brown oily liquid was distilled to obtain a colorless oily compound B; Step 2: Take compound B and PCl 3 and TEA were added to a reaction flask, dissolved in THF, stirred at room temperature for 8 hours, the solvent was removed under reduced pressure, and the functionalized phosphine-containing polymer monomer (compound C) was separated by column chromatography; Step 3: Add compound D and n-butyl lithium to a reaction flask, add THF to dissolve, stir and react at -40°C for 3 hours, and add PCl 3 , react at 50°C with stirring for 2 h, add aqueous hydrochloric acid to adjust the pH to acidic, continue stirring for 30 minutes, filter, wash with water, and separate the filter cake by column chromatography to obtain a yellow solid compound E; Step 4: Add tert-butyl peroxide and compounds C and E to a dry Shrek tube, seal the tube under argon protection, react at 80°C for 48 hours, cool to room temperature, add methanol for precipitation, filter, wash with methanol, and vacuum dry to obtain a polymer represented by formula (I) as a white solid.

8. Use of the monodentate phospholipid phosphine ligand copolymer-supported rhodium catalyst according to claim 1 or 2 in catalyzing the isomerization hydroformylation of dimerized isobutylene to prepare isononanal.

9. A method for preparing isononanal by catalyzing the isomerization hydroformylation of dimerized isobutylene using the monodentate phospholipid phosphine ligand copolymer supported rhodium catalyst as claimed in claim 1 or 2, the method being carried out as follows: A certain amount of the monodentate phospholipid phosphine ligand copolymer supported rhodium catalyst and olefin compound according to claim 1 or 2 are added to the autoclave, and the reaction mixture is heated with synthesis gas (CO / H 2 =1:1) for 3 times, then introduce 2-8 MPa synthesis gas, stir the reaction at a certain temperature for a certain time, then cool down and release the gas.

10. The method according to claim 9, It is characterized in that The olefin compound is selected from diisobutylene; Preferably, the molar ratio of the olefin compound to Rh is 1000:1 to 30000:1, preferably 10000:1; Preferably, the pressure of the synthesis gas is 2 to 8 MPa, preferably 4 to 6 MPa; Preferably, the reaction temperature is 60 to 120°C, preferably 80 to 100°C; Preferably, the reaction time is 1 to 24 hours, preferably 5 to 12 hours.

Citation Information

Patent Citations

  • Organic molecular cage heterogeneous catalyst containing P skeleton structure unit as well as preparation method and application of organic molecular cage heterogeneous catalyst

    CN113976173A

  • Catalyst for preparing linear-chain aldehyde in high-selectivity manner as well as preparation and application thereof

    CN109806911A

  • Method for preparing aldehyde by hydroformylation of olefins

    CN109836318A

  • Hydroformylation reaction method for preparing isononaldehyde from diisobutylene and catalyst

    CN111909014A

  • Method for preparing isononanal through diisobutylene hydroformylation

    CN112794796A