Composite copper-cobalt-based catalyst as well as preparation method and application thereof

By combining alkali metal, copper-based COF catalyst and Co-based hydrotalcite, a composite copper-cobalt-based catalyst is prepared, and the synergistic effect of CoAl-LDH and Cu-MOF is used to solve the problems of high price, poor selectivity and low activity of existing catalysts. problem, achieving efficient and stable high-grade alcohol synthesis gas conversion, which is suitable for industrial applications.

CN118719151APending Publication Date: 2024-10-01KAILUAN (GROUP) CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410769307.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing catalysts used to directly produce higher alcohols from synthesis gas have problems such as high price, poor selectivity to higher alcohols, and low catalytic activity. In addition, the uneven dispersion of bimetallic catalysts results in limited reaction performance.

Method used

A composite copper-cobalt-based catalyst is used to combine alkali metal, copper-based COF catalyst and Co-based hydrotalcite, and precipitation method and in-situ growth method are used to prepare CoAl-LDH and Cu-MOF. The synergistic effect improves the catalytic activity, and through impregnation Alkali metals enhance the dispersion and stability of the catalyst.

Benefits of technology

It realizes the conversion of CO/H2 synthesis gas into higher alcohols with high efficiency and excellent selectivity, reduces the preparation cost, is suitable for industrial application, and improves the stability and reaction rate of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719151A_ABST
    Figure CN118719151A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of catalytic materials, and particularly discloses a composite copper-cobalt-based catalyst and a preparation method and application thereof. According to the preparation method of the composite copper-cobalt-based catalyst provided by the invention, CoAl-LDH is prepared by utilizing a precipitation method and is dispersed in an organic solvent, so that high aggregation or overlapping of an LDH material is prevented; the preparation method comprises the following steps: preparing a CoAl-LDH lamellar structure, enabling Cu-MOF to uniformly grow on the CoAl-LDH lamellar structure in a specific solvent by using an in-situ growth method, and dipping alkali metal to prepare the multi-component uniformly dispersed composite copper-cobalt-based catalyst, through the synergistic effect of multiple active centers of Mo, Cu and alkali metal, the activity of the catalyst is remarkably improved, and the catalyst is simple in preparation method and low in cost. The method is suitable for large-scale industrial preparation and application; when the catalyst is applied to a reaction for catalyzing synthesis gas to be converted into higher alcohols, higher alcohol selectivity is shown, and a catalytic material with excellent performance is provided for catalyzing synthesis gas to be converted into higher alcohols.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalytic material preparation, and in particular to a composite copper-cobalt based catalyst and a preparation method and application thereof. Background Art

[0002] Due to the rapid reduction of global petroleum energy and the gradual improvement of people's awareness of environmental protection, the development of sustainable energy and clean industrial production have received widespread attention. Vigorously promoting the clean and efficient utilization technology of coal resources and promoting the optimization of energy structure are important ways to ensure energy security and sustainable economic and social development. In recent years, C1 chemistry based on natural gas utilization has developed vigorously. In the process of syngas conversion, in addition to directly producing fuel oil, olefins, etc. through the Fischer-Tropsch synthesis reaction, higher alcohols (alcohols with two or more carbon numbers) can also be prepared through a one-step reaction. Higher alcohols have a wide range of applications in the fields of fuel additives, detergents, lubricants, and pharmaceutical intermediates. Therefore, vigorously developing syngas to produce higher alcohols in one step has broad prospects.

[0003] At present, there are four main types of catalysts used for direct production of higher alcohols from synthesis gas, namely modified Cu-based catalysts, modified Fischer-Tropsch catalysts, Mo-based catalysts, and Rh-based catalysts. Among them, Rh-based catalysts are difficult to industrialize due to their high prices, which hinders their further development; for Mo-based catalysts, the alcohol product is mainly methanol, and its water-gas shift activity is high and its CO2 selectivity is high. For modified Fischer-Tropsch Fe-based catalysts, there is also the problem of high water-gas shift activity. In order to reduce costs and improve the alcohol selectivity of the catalyst, researchers have selected suitable bimetallic catalysts as active centers to make bimetallic catalysts. However, due to the uneven dispersion of bimetallic catalysts, the bimetallic interaction effect is easily weakened, which affects the further improvement of the catalyst reaction performance. Summary of the invention

[0004] In view of the problems of high price, poor selectivity for higher alcohols, and low catalytic activity of existing catalysts for directly preparing higher alcohols from synthesis gas, the present invention provides a composite copper-cobalt-based catalyst and a preparation method and application thereof. By combining alkali metal, copper-based COF catalyst and Co-based hydrotalcite catalyst, the prepared catalyst has excellent activity, selectivity and stability for preparing higher alcohols from synthesis gas, low preparation cost, simple operation, and good practical application value.

[0005] To solve the above technical problems, the technical solution provided by the embodiment of the present invention is:

[0006] In a first aspect, the present invention provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0007] Step a, dissolving a cobalt source in water to obtain a cobalt source solution; adding an aluminum source and a precipitant to the cobalt source solution, reacting, adding the reaction product to a first organic solvent, dispersing, solid-liquid separation, and drying to obtain cobalt aluminum hydrotalcite;

[0008] Step b, dispersing the cobalt aluminum hydrotalcite and the copper source in a second organic solvent to obtain a dispersion; dissolving an organic ligand in a third organic solvent to obtain an organic linker solution; adding the organic linker solution to the dispersion, mixing evenly, reacting, solid-liquid separation, washing, and drying to obtain a Cu-COF / cobalt aluminum hydrotalcite composite catalyst;

[0009] Step c, impregnating the cobalt-aluminum hydrotalcite / Cu-COF composite catalyst into an alkali metal salt aqueous solution, drying, and calcining to obtain a composite copper-cobalt based catalyst.

[0010] Cobalt-based catalysts mainly catalyze the production of hydrocarbons in syngas conversion. Applying them in the reaction of converting syngas into alcohols requires adding other components to modify them. However, the dispersion of multiple components and the interaction between them have a significant impact on the improvement of catalyst performance.

[0011] Compared with the prior art, the preparation method of the composite copper-cobalt-based catalyst provided by the present invention uses a precipitation method to prepare CoAl-LDH, and disperses it in an organic solvent to prevent high aggregation or overlap of LDH materials, thereby facilitating the exposure of a large number of active sites of the LDH material; then, using an in-situ growth method in a specific solvent, Cu-MOF is uniformly grown on the CoAl-LDH sheet structure, and alkali metals are impregnated, and the catalytic activity of the catalyst is significantly improved through the synergistic effect of CoAl-LDH, Cu-MOF and alkali metal multi-active centers. At the same time, the composite of LDH and MOF materials, whose large specific surface area provides favorable conditions for the uniform dispersion of metal active sites, and the rich pore structure of the material is also conducive to the mass transfer process of raw materials and products, thereby facilitating the improvement of reaction rate; in addition, Cu and Co are introduced in the form of MOF materials and LDH materials, and alkali metals are subsequently introduced by impregnation, which not only improves the dispersibility of the metal, so that the interaction of multiple components is moderate, but also enables each active component to be uniformly and stably immobilized in the catalyst system, thereby improving the stability of the catalyst structure and performance.

[0012] By means of the preparation method provided by the present invention, a multi-component uniformly dispersed composite copper-cobalt-based catalyst can be prepared. The activity of the catalyst is significantly improved through the synergistic effect of multiple active centers of Mo, Cu, and alkali metals. The preparation method of the catalyst is simple and does not require conditions such as high temperature and high pressure, so the catalyst is suitable for large-scale industrial preparation and application. The catalyst is applied to the reaction of catalyzing the conversion of synthesis gas into higher alcohols, showing a high selectivity for alcohols, thereby providing a catalytic material with excellent performance for catalyzing the conversion of synthesis gas into higher alcohols.

[0013] Furthermore, in step a, the cobalt source is at least one of cobalt chloride, cobalt acetate, cobalt nitrate or cobalt sulfate.

[0014] Furthermore, in step a, the aluminum source is at least one of aluminum chloride, aluminum nitrate or aluminum sulfate.

[0015] Furthermore, in step a, the precipitant is at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium carbonate, sodium bicarbonate or urea.

[0016] Furthermore, in step a, the first organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide.

[0017] Furthermore, in step a, the concentration of the cobalt source solution is 0.01 mol / L-0.20 mol / L.

[0018] Furthermore, in step a, the molar ratio of Co in the cobalt source to Al in the aluminum source is 1:1-1:10.

[0019] Furthermore, in step a, the molar ratio of the precipitant to Co in the cobalt source is 1:1-10:1.

[0020] Furthermore, in step a, the reaction temperature is 50°C-100°C, and the reaction time is 24h-48h.

[0021] It should be noted that after the precipitation reaction in step a is completed, the mixture is cooled to room temperature, solid-liquid separation is performed, and the mixture is washed with deionized water until neutral, and then dispersed in the first organic solvent.

[0022] Furthermore, in step a, the ratio of the reaction product to the first organic solvent is 0.01 g:1 mL-0.05 g:1 mL.

[0023] Furthermore, in step a, the specific steps of dispersing are: first ultrasonic treatment for 5 min-60 min, and then stirring for 30 min-120 min.

[0024] The preferred first organic solvent and dispersion method can fully peel the cobalt aluminum hydrotalcite into a lamellar structure, avoid high aggregation or overlap of the cobalt aluminum hydrotalcite material, thereby avoiding the covering of a large number of chemical reaction sites and increasing the reaction active sites.

[0025] Exemplarily, in step a, the drying may be carried out by one of the following drying methods: forced air drying, vacuum drying, low temperature freeze drying, microwave drying or CO2 supercritical drying. Preferably, vacuum freeze drying is used.

[0026] Exemplarily, the vacuum freeze drying temperature is -90°C-0°C, the vacuum degree is below 10mTorr-100mTorr, and the drying time is 10h-48h.

[0027] The preferred drying method is beneficial to maintaining the structural integrity and valence stability of the multiple components in the catalyst.

[0028] Furthermore, in step b, the copper source is at least one of copper sulfate, copper nitrate, copper acetate or copper chloride.

[0029] Furthermore, in step b, the second organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide.

[0030] The preferred second organic solvent can make the Cu-MOF material uniformly formed during the in-situ growth process on the cobalt aluminum hydrotalcite sheet layer, avoid aggregation of the composite material, and increase the specific surface area of ​​the composite material.

[0031] Furthermore, in step b, the third organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide.

[0032] Furthermore, in step b, the organic linker is one or both of terephthalic acid and trimesic acid.

[0033] Furthermore, in step b, the molar ratio of Co in the cobalt-aluminum hydrotalcite to Cu in the copper source is 1:1-5:1.

[0034] Furthermore, in step b, the concentration of the copper source in the dispersion is 0.1 mol / L-1.0 mol / L.

[0035] Furthermore, in step b, the concentration of the organic linker solution is 1.0 mol / L-10 mol / L.

[0036] Furthermore, in step b, the molar ratio of Cu in the copper source to the organic linker is 1:1-1:4.

[0037] Furthermore, in step b, the specific steps of the reaction are: first react at 10°C-30°C for 10min-60min, and then react at 50°C-100°C for 5h-24h.

[0038] The preferred reaction conditions can make Cu-MOF grow evenly on the CoAl-LDH layer structure, thereby improving the stability of the composite material structure.

[0039] Exemplarily, in step b, the drying may be carried out by one of the following drying methods: forced air drying, vacuum drying, low temperature freeze drying, microwave drying or CO2 supercritical drying. CO2 supercritical drying is preferred.

[0040] Exemplarily, in step b, the washing agent used in the washing can be selected from at least one of methanol, ethanol, acetone or N,N-dimethylformamide.

[0041] Furthermore, in step c, the immersion temperature is 10°C-30°C, and the immersion time is 2h-3h.

[0042] Exemplarily, in step c, an equal volume impregnation method is adopted.

[0043] Exemplarily, in step c, the alkali metal salt solution is added dropwise to the cobalt aluminum hydrotalcite / Cu-COF composite catalyst, and the dropping process is stirred. The dropping time is 2h-3h.

[0044] Furthermore, in step c, the mass ratio of the metal element in the alkali metal salt to the cobalt aluminum hydrotalcite / Cu-COF composite catalyst is 0.01:1-0.1:1.

[0045] Furthermore, the alkali metal salt is a nitrate, sulfate, carbonate or acetate corresponding to Na, K or Cs. Preferably, the alkali metal is a nitrate, sulfate or the like corresponding to Cs.

[0046] The preferred impregnation conditions are conducive to uniformly loading the alkali metal on the cobalt-aluminum hydrotalcite / Cu-COF composite catalyst, and the selection of alkali metal in conjunction with Co and Cu can make the catalyst have excellent catalytic activity and selectivity for preparing higher alcohols from CO / H2 synthesis gas.

[0047] Furthermore, in step c, the calcination temperature is 300°C-500°C, the calcination time is 2h-8h, and the heating rate is 1°C / min-10°C / min.

[0048] The preferred calcination conditions are conducive to maintaining a high dispersion state of each active component, avoiding the loss of active components, and reducing the aggregation of the composite material, thereby helping to improve the catalytic activity of the prepared catalyst.

[0049] Exemplarily, in step c, the roasting equipment may be a muffle furnace or a tubular furnace, which is not particularly limited in the present invention.

[0050] In a second aspect, the present invention further provides a composite copper-cobalt-based catalyst prepared by any of the above-mentioned methods for preparing the composite copper-cobalt-based catalyst.

[0051] The composite copper-cobalt-based catalyst prepared by the present invention has excellent catalytic activity, selectivity and stability for preparing higher alcohols from CO / H2 synthesis gas, and has a simple preparation process, a wide source of raw materials, and low cost, and has broad application prospects in the field of preparing higher alcohols from synthesis gas.

[0052] In a third aspect, the present invention also provides the use of the above-mentioned composite copper-cobalt-based catalyst in the preparation of higher alcohols from synthesis gas.

[0053] The present invention combines a Cu-based MOF catalyst with a Co-based hydrotalcite and introduces an alkali metal to prepare a multi-metal catalyst. The composite structure of LDH and MOF can provide more active centers, reduce the aggregation of active centers, and make the active centers more evenly dispersed. Through the synergistic effect of Co, Cu and alkali metals, the low-temperature hydrogenation activity of the composite catalyst is effectively improved, the water-gas shift activity is low, and the CO2 selectivity in the product is low. At the same time, it has a significant promoting effect on the generation of higher alcohols, and shows great application potential in the industrial application of synthesizing gas to prepare higher alcohols.

[0054] In a fourth aspect, the present invention further provides a method for preparing higher alcohols from synthesis gas, comprising the following steps:

[0055] Quartz wool and silicon carbide are added to the bottom of the fixed bed reaction tube, and then mixed particles of the composite copper-cobalt-based catalyst and silicon carbide particles are filled, and synthesis gas is introduced to react to obtain higher alcohols.

[0056] Furthermore, the synthesis gas is H2 and CO in a molar ratio of 1:1-2:1, the reaction temperature is 200°C-300°C, the reaction pressure is 1.5MPa-6.0MPa, and the space velocity is 2000mL·g cat -1 ·h -1 -8000mL·g cat -1 ·h -1 .

[0057] Preferably, the synthesis gas is H2 and CO in a molar ratio of 2:1, the reaction temperature is 220-270°C, the reaction pressure is 3.0MPa-6.0MPa, and the space velocity is 2000mL·g cat -1 ·h -1 -6000mL·gcat -1 ·h -1 .

[0058] Furthermore, the particle size of the silicon carbide particles added to the bottom of the reaction tube is 10-30 meshes.

[0059] Furthermore, the particle size of the silicon carbide particles mixed with the composite copper-cobalt catalyst is 80-100 meshes.

[0060] Furthermore, the volume of the 80-100 mesh silicon carbide particles is three times the mass of the supported molybdenum carbide catalyst, wherein the unit of volume is milliliter and the unit of mass is gram.

[0061] The active components in the composite copper-cobalt-based catalyst provided by the present invention all maintain a high dispersion state, the interactions between the active components are moderate, and the binding force between the active components and the carrier is high. The active components are not easy to be lost during the catalytic process. Through the synergistic effect of multiple active components, the purpose of efficiently activating and converting synthesis gas to prepare higher alcohols under mild conditions is achieved. The industrial application prospect is high and the practical value is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is a scanning electron microscope image of CoAl-LDH prepared in Example 1;

[0063] Figure 2 This is a scanning electron microscope image of the Cu-MOF / CoAl-LDH catalyst prepared in Example 1;

[0064] Figure 3 The CO conversion rate and C content of the alcohol in the reaction of syngas to higher alcohols catalyzed by the K-Cu-MOF / CoAl-LDH catalyst prepared in Example 1 are 2+ Alcohol percentage chart. DETAILED DESCRIPTION

[0065] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0066] In order to better illustrate the present invention, further examples are given below.

[0067] Example 1

[0068] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0069] Step 1, weigh 0.005 mol of CoCl2·6H2O and 0.05 mol of AlCl3 and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.05 mol of urea and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 50°C for 48 hours; after the reaction is completed, after the solution is cooled to room temperature, centrifuge the product and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.03 g / mL, sonicate for 10 minutes, stir at room temperature for 120 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0070] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL of anhydrous ethanol, sonicate for 15 min, add 0.03 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0071] 0.03 mol of trimesic acid was dissolved in a mixed solution of 5 mL of anhydrous ethanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred at 50 ° C for 24 h, and after the reaction, centrifuged and washed three times with a mixed solution of ethanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0072] Step 3: Dissolve 0.08 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF / CoAl-LDH;

[0073] Step 4: calcine the above sample in a tube furnace at 300°C and a heating rate of 5°C / min for 8h to obtain K-CuO-MOF / CoAl-LDO.

[0074] The scanning electron microscopy image of CoAl-LDH prepared in step 1 of this example is as follows Figure 1 As shown in the figure, it can be seen that the sample is a nanosheet structure. The scanning electron microscope image of Cu-MOF / CoAl-LDH prepared in step 2 is shown in Figure 2 As shown in the figure, it can be seen that the surface of the sample becomes rough, which is caused by the in situ growth of Cu-MOF on the surface of LDH.

[0075] The BET test results of the K-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 1.

[0076] Table 1 BET test results of K-CuO-MOF / CoAl-LDO catalyst

[0077] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 437 0.58 5.3

[0078] The K-CuO-MOF / CoAl-LDO catalyst prepared in this example is used to prepare higher alcohols from syngas, and the specific steps are as follows:

[0079] 0.3 g of quartz wool was added to the bottom of the fixed bed reaction tube, and then 4 mL of 10-mesh silicon carbide particles were added on top. 1 g of K-CuO-MOF / CoAl-LDO catalyst was mixed with 3 mL of 100-mesh silicon carbide particles and then loaded into the reaction tube. The airtightness of the device was checked. If it was qualified, the synthesis gas was introduced. The reaction conditions were: H2 / CO=2, temperature 250°C, pressure 3.0 MPa, space velocity 4000 mL·g cat -1 ·h -1 The gas phase products were analyzed by online chromatography, and the liquid phase products were analyzed by offline gas chromatography.

[0080] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 67.3%, and the C 2+ The alcohol selectivity is 81.4%, such as Figure 3 shown.

[0081] Example 2

[0082] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0083] Step 1, weigh 0.013 mol of Co(NO3)2·6H2O and 0.052 mol of Al(NO3)3·9H2O and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of potassium hydroxide and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.04 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0084] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL acetone, sonicate for 15 min, add 0.01 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0085] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of acetone and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 20 min, stirred at 80 ° C for 8 h, and after the reaction, centrifuged and washed three times with a mixed solution of acetone and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0086] Step 3: Dissolve 0.4 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF / CoAl-LDH;

[0087] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain K-CuO-MOF / CoAl-LDO.

[0088] The BET test results of the K-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 2.

[0089] Table 2 BET test results of K-CuO-MOF / CoAl-LDO catalyst

[0090] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 529 0.63 4.0

[0091] The K-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0092] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 63.4%, and the C 2+ The alcohol selectivity was 85.1%.

[0093] Example 3

[0094] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0095] Step 1, weigh 0.04 mol of Co(SO4)2·7H2O and 0.04 mol of Al2(SO4)3 and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.04 mol of sodium carbonate and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 100°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.05 g / mL, sonicate for 40 minutes, stir at room temperature for 90 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0096] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL methanol, sonicate for 15 min, add 0.05 mol copper nitrate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0097] 0.1 mol of trimesic acid was dissolved in a mixed solution of 5 mL of methanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred at 100 ° C for 5 h, and after the reaction was completed, centrifuged and washed three times with a mixed solution of methanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0098] Step 3: Dissolve 0.75 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF / CoAl-LDH;

[0099] Step 4: calcine the above sample in a tube furnace at 500°C and a heating rate of 10°C / min for 2h to obtain K-CuO-MOF / CoAl-LDO.

[0100] The BET test results of the K-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 3.

[0101] Table 3 BET test results of K-CuO-MOF / CoAl-LDO catalyst

[0102] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Aperture D(nm) 491 0.60 4.7

[0103] The K-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0104] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 58.7%, and the C 2+ The alcohol selectivity was 89.5%.

[0105] Example 4

[0106] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0107] Step 1, weigh 0.1 mol of Co(SO4)2·7H2O and 0.15 mol of Al2(SO4)3 and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.2 mol of sodium carbonate and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 70°C for 35 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.01 g / mL, sonicate for 40 minutes, stir at room temperature for 90 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0108] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL methanol, sonicate for 15 min, add 0.04 mol copper nitrate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0109] 0.1 mol of trimesic acid was dissolved in a mixed solution of 5 mL of methanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred at 100 ° C for 5 h, and after the reaction was completed, centrifuged and washed three times with a mixed solution of methanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0110] Step 3: Dissolve 0.75 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF / CoAl-LDH;

[0111] Step 4: calcine the above sample in a tube furnace at 500°C and a heating rate of 10°C / min for 2h to obtain K-CuO-MOF / CoAl-LDO.

[0112] The BET test results of the K-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 4.

[0113] Table 4 BET test results of K-CuO-MOF / CoAl-LDO catalyst

[0114] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 459 0.68 5.1

[0115] The K-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0116] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 63.9%, and the C 2+ The alcohol selectivity was 78.4%.

[0117] Example 5

[0118] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0119] Step 1, weigh 0.013 mol of Co(NO3)2·6H2O and 0.052 mol of Al(NO3)3·9H2O and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of urea and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.03 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0120] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL of anhydrous ethanol, sonicate for 15 min, add 0.01 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0121] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of anhydrous ethanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred and reacted at 80 ° C for 8 h. After the reaction, centrifuged and washed three times with a mixed solution of ethanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0122] Step 3: Dissolve 0.4 g of cesium nitrate in 2.5 mL of deionized water to obtain a cesium nitrate solution; use an equal volume impregnation method to add the cesium nitrate solution dropwise to 3 g of the Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain Cs-Cu-MOF / CoAl-LDH;

[0123] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain Cs-CuO-MOF / CoAl-LDO.

[0124] The BET test results of the Cs-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 5.

[0125] Table 5 BET test results of Cs-CuO-MOF / CoAl-LDO catalyst

[0126] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 504 0.73 4.4

[0127] The Cs-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0128] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 55.4%, and the C 2+ The alcohol selectivity was 91.8%.

[0129] Example 6

[0130] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0131] Step 1, weigh 0.013 mol of Co(NO3)2·6H2O and 0.052 mol of Al(NO3)3·9H2O and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of urea and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.04 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid by supercritical CO2 for 20 hours to obtain CoAl-LDH;

[0132] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL of anhydrous ethanol, sonicate for 15 min, add 0.01 mol copper nitrate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0133] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of anhydrous ethanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred and reacted at 80 ° C for 8 h. After the reaction, centrifuged and washed three times with a mixed solution of ethanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0134] Step 3: Dissolve 0.4 g of cesium nitrate in 2.5 mL of deionized water to obtain a cesium nitrate solution; use an equal volume impregnation method to add the cesium nitrate solution dropwise to 3 g of the Cu-MOF / CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and then dry it with CO2 supercritical drying to obtain Cs-Cu-MOF / CoAl-LDH;

[0135] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain Cs-CuO-MOF / CoAl-LDO.

[0136] The BET test results of the Cs-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 6.

[0137] Table 6 BET test results of Cs-CuO-MOF / CoAl-LDO catalyst

[0138] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 543 0.76 3.2

[0139] The Cs-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0140] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 57.8%, and the C 2+ The alcohol selectivity was 92.9%.

[0141] Example 7

[0142] This embodiment provides a method for preparing a composite copper-cobalt-based catalyst, comprising the following steps:

[0143] Step 1, weigh 0.013 mol of Co(NO3)2·6H2O and 0.052 mol of Al(NO3)3·9H2O and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of urea and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.04 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0144] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL of anhydrous ethanol, sonicate for 15 min, add 0.01 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0145] 0.04 mol of terephthalic acid was dissolved in a mixed solution of 5 mL of anhydrous ethanol and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 10 min, stirred and reacted at 80 ° C for 8 h. After the reaction, centrifuged and washed three times with a mixed solution of ethanol and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0146] Step 3: Dissolve 0.4 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; add the potassium nitrate solution dropwise to 3 g Cu-MOF / CoAl-LDH sample using an equal volume impregnation method, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF / CoAl-LDH;

[0147] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain K-CuO-MOF / CoAl-LDO.

[0148] The BET test results of the K-CuO-MOF / CoAl-LDO catalyst prepared in this example are shown in Table 7.

[0149] Table 7 BET test results of K-CuO-MOF / CoAl-LDO catalyst

[0150] <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume V BJH (cm 3 ·g -1 )]]> Average pore size D(nm) 458 0.59 4.3

[0151] The K-CuO-MOF / CoAl-LDO catalyst prepared in this example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0152] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 58.6%, and the C 2+ The alcohol selectivity was 79.5%.

[0153] Comparative Example 1

[0154] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method thereof is different from that of Example 2 in that the step of dispersing in ethanol in step 1 is omitted. Specifically, step 1 is:

[0155] Step 1, weigh 0.013 mol of CoCl2·6H2O and 0.052 mol of AlCl3 and dissolve them in 500 mL of deionized water, dissolve them by ultrasound, weigh 0.104 mol of potassium hydroxide and add them to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, wait for the solution to cool to room temperature, centrifuge the product, wash it with deionized water until it is neutral, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0156] Steps 2 to 4 are exactly the same as those in Example 2 and will not be repeated here.

[0157] The K-CuO-MOF / CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0158] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 50.8%, and the C 2+ The alcohol selectivity was 58.6%.

[0159] Comparative Example 2

[0160] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method thereof is different from that of Example 2 in that step 2 is omitted. The specific steps are as follows:

[0161] Step 1, weigh 0.013 mol of CoCl2·6H2O and 0.052 mol of AlCl3 and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of potassium hydroxide and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, after the solution is cooled to room temperature, centrifuge the product and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.04 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0162] Step 3: Dissolve 0.4 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g CoAl-LDH sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 hours to obtain K-CoAl-LDH;

[0163] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain K-CoAl-LDO.

[0164] The K-CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0165] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 34.7%, and the C 2+ The alcohol selectivity was 41.4%.

[0166] Comparative Example 3

[0167] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method thereof is different from that of Example 2 in that step 3 is omitted. The specific steps are as follows:

[0168] Step 1, weigh 0.013 mol of CoCl2·6H2O and 0.052 mol of AlCl3 and dissolve them in 500 mL of deionized water, sonicate to dissolve them, weigh 0.104 mol of potassium hydroxide and add it to the above solution, transfer the solution to a three-necked flask after it is completely dissolved, and react at 80°C for 24 hours; after the reaction is completed, after the solution is cooled to room temperature, centrifuge the product and wash it with deionized water until it is neutral, then disperse the obtained solid in methanol at a ratio of 0.04 g / mL, sonicate for 60 minutes, stir at room temperature for 60 minutes, centrifuge, and dry the obtained solid at -80°C and a vacuum degree of 48 mTorr for 20 hours to obtain CoAl-LDH;

[0169] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL acetone, sonicate for 15 min, add 0.01 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0170] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of acetone and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 20 min, stirred at 80 ° C for 8 h, and after the reaction, centrifuged and washed three times with a mixed solution of acetone and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH;

[0171] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 h to obtain CuO-MOF / CoAl-LDO.

[0172] The CuO-MOF / CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0173] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 71.4%, and the C 2+ The alcohol selectivity was 53.2%.

[0174] Comparative Example 4

[0175] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method is different from that of Example 2 in that the cobalt nitrate in step 1 is replaced by ferrous nitrate, and the rest is exactly the same, to prepare K-CuO-MOF / FeAl-LDO.

[0176] The K-CuO-MOF / FeAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0177] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 82.4%, and the C 2+ The alcohol selectivity was 38.1%.

[0178] Comparative Example 5

[0179] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method is different from that of Example 2 in that the acetone in step 2 is replaced with deionized water. Specifically, step 2 is:

[0180] Step 2: Place the 0.01 mol CoAl-LDH sample obtained above in 60 mL of water, sonicate for 15 min, add 0.01 mol copper acetate, sonicate for 15 min to dissolve it, and obtain a dispersion;

[0181] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of water and 5 mL of N,N-dimethylformamide, and then added to the above dispersion, stirred at room temperature for 20 min, and stirred at 80 ° C for 8 h. After the reaction, centrifuged and washed 3 times with a mixed solution of water and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF / CoAl-LDH.

[0182] The remaining steps are exactly the same and will not be repeated here.

[0183] The K-CuO-MOF / CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0184] The reaction was carried out under this condition for 80 hours, and the evaluation data of the catalyst was obtained. The carbon monoxide conversion rate was 50.6%, and the C 2+ The alcohol selectivity was 71.3%.

[0185] Comparative Example 6

[0186] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method is different from that of Example 2 only in that the copper acetate in step 2 is replaced by cobalt acetate. The rest is exactly the same and will not be repeated here. K-CoO-MOF / CoAl-LDO is prepared.

[0187] The K-CoO-MOF / CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0188] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 45.8%, and the C 2+ The alcohol selectivity was 44.9%.

[0189] Comparative Example 7

[0190] This comparative example provides a method for preparing a composite copper-cobalt-based catalyst. The preparation method thereof is different from that of Example 2 in that step 1 is omitted. The specific steps are as follows:

[0191] Step 2: Place 0.01 mol of copper acetate in 60 mL of acetone and perform ultrasonic treatment for 15 min to obtain a copper acetate solution;

[0192] 0.04 mol of trimesic acid was dissolved in a mixed solution of 5 mL of acetone and 5 mL of N,N-dimethylformamide, and then added to the above copper acetate solution, stirred at room temperature for 20 min, stirred and reacted at 80 ° C for 8 h. After the reaction, centrifuged and washed 3 times with a mixed solution of acetone and N,N-dimethylformamide, and finally dried by supercritical CO2 to obtain Cu-MOF;

[0193] Step 3: Dissolve 0.4 g potassium nitrate in 2 mL deionized water to obtain a potassium nitrate solution; use an equal volume impregnation method to add the potassium nitrate solution dropwise to 3 g Cu-MOF sample with a pipette, and continue stirring until the impregnation is complete, and dry at -80 ° C and a vacuum degree of 48 mTorr for 20 h to obtain K-Cu-MOF;

[0194] Step 4: calcine the above sample in a tube furnace at 400°C and a heating rate of 2°C / min for 4 hours to obtain K-CuO-MOF.

[0195] The K-CoO-MOF / CoAl-LDO catalyst prepared in this comparative example was used to prepare higher alcohols from synthesis gas, and the synthesis conditions were exactly the same as those in Example 1.

[0196] The reaction was carried out under this condition for 80 hours to obtain the evaluation data of the catalyst. The carbon monoxide conversion rate was 52.1%, and the C 2+ The alcohol selectivity was 10.7%.

[0197] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite copper-cobalt based catalyst, characterized in that: The steps include: Step a, dissolving a cobalt source in water to obtain a cobalt source solution; adding an aluminum source and a precipitant to the cobalt source solution, reacting, adding the reaction product to a first organic solvent, dispersing, solid-liquid separation, and drying to obtain cobalt aluminum hydrotalcite; Step b, dispersing the cobalt aluminum hydrotalcite and the copper source in a second organic solvent to obtain a dispersion; dissolving an organic ligand in a third organic solvent to obtain an organic linker solution; adding the organic linker solution to the dispersion, mixing evenly, reacting, solid-liquid separation, washing, and drying to obtain a Cu-COF / cobalt aluminum hydrotalcite composite catalyst; Step c, impregnating the cobalt-aluminum hydrotalcite / Cu-COF composite catalyst into an alkali metal salt aqueous solution, drying, and calcining to obtain a composite copper-cobalt based catalyst.

2. The method for preparing a composite copper-cobalt based catalyst according to claim 1, characterized in that: In step a, the cobalt source is at least one of cobalt chloride, cobalt acetate, cobalt nitrate or cobalt sulfate; and / or In step a, the aluminum source is at least one of aluminum chloride, aluminum nitrate or aluminum sulfate; and / or In step a, the precipitant is at least one of potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium carbonate, sodium bicarbonate or urea; and / or In step a, the first organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide.

3. The method for preparing a composite copper-cobalt-based catalyst according to claim 1 or 2, characterized in that: In step a, the concentration of the cobalt source solution is 0.01 mol / L-0.20 mol / L; and / or In step a, the molar ratio of Co in the cobalt source to Al in the aluminum source is 1:1-1:10; and / or In step a, the molar ratio of the precipitant to Co in the cobalt source is 1:1-10:1; and / or In step a, the reaction temperature is 50°C-100°C, and the reaction time is 24h-48h; and / or In step a, the ratio of the reaction product to the first organic solvent is 0.01 g:1 mL-0.05 g:1 mL; and / or In step a, the specific steps of dispersing are: first ultrasonic treatment for 5 min to 60 min, and then stirring for 30 min to 120 min.

4. The method for preparing a composite copper-cobalt-based catalyst according to claim 1, characterized in that: In step b, the copper source is at least one of copper sulfate, copper nitrate, copper acetate or copper chloride; and / or In step b, the second organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide; and / or In step b, the third organic solvent is at least one of methanol, ethanol, acetone or N,N-dimethylformamide; and / or In step b, the organic linking agent is one or both of terephthalic acid and trimesic acid.

5. The method for preparing a composite copper-cobalt-based catalyst according to claim 1 or 4, characterized in that: In step b, the molar ratio of Co in the cobalt-aluminum hydrotalcite to Cu in the copper source is 1:1-5:1; and / or In step b, the concentration of the copper source in the dispersion is 0.1 mol / L-1.0 mol / L; and / or In step b, the concentration of the organic linker solution is 1.0 mol / L-10 mol / L; and / or In step b, the molar ratio of Cu in the copper source to the organic linker is 1:1-1:4; and / or In step b, the specific steps of the reaction are: first react at 10°C-30°C for 10min-60min, and then react at 50°C-100°C for 5h-24h.

6. The method for preparing a composite copper-cobalt based catalyst according to claim 1, characterized in that: In step c, the immersion temperature is 10°C-30°C, and the immersion time is 2h-3h; and / or In step c, the mass ratio of the metal element in the alkali metal salt to the cobalt aluminum hydrotalcite / Cu-COF composite catalyst is 0.01:1-0.1:1; and / or In step c, the calcination temperature is 300° C.-500° C., the calcination time is 2 h-8 h, and the heating rate is 1° C. / min-10° C. / min.

7. A composite copper-cobalt based catalyst, characterized in that: The composite copper-cobalt-based catalyst is prepared by the preparation method of any one of claims 1 to 6.

8. Use of the composite copper-cobalt-based catalyst according to claim 7 in the preparation of higher alcohols from synthesis gas.

9. A method for preparing higher alcohols from synthesis gas, characterized in that: The steps include: Add quartz wool and silicon carbide to the bottom of the reaction tube, then fill it with mixed particles of the composite copper-cobalt-based catalyst and silicon carbide particles as claimed in claim 7, and introduce synthesis gas to react to obtain higher alcohols.

10. The method for preparing higher alcohols from synthesis gas according to claim 9, characterized in that: The synthesis gas is H2 and CO in a molar ratio of 1:1-2:1, the reaction temperature is 200°C-300°C, the reaction pressure is 1.5MPa-6.0MPa, and the space velocity is 2000mL·g cat -1 ·h -1 -8000mL·g cat -1 ·h -1 .

Citation Information

Patent Citations

  • Structured copper-cobalt based catalyst and application of catalytic synthesis gas of structured copper-cobalt based catalyst in preparation of higher alcohols

    CN102489301A

  • Preparation method and application of cobalt-based catalyst for catalyzing carbon dioxide to prepare ethanol

    CN108380216A

  • Cobalt-copper bimetallic catalyst for directly preparing low-carbon alcohol from synthesis gas as well as preparation method and use method of cobalt-copper bimetallic catalyst

    CN114160137A

  • Catalyst for preparing higher alcohol through CO2 hydrogenation as well as preparation method and application of catalyst

    CN115999555A

  • Catalyst compositions for converting syngas to produce higher alcohols

    US20130245328A1