Lead-zinc oxide ore separation method

Through the multi-step lead-zinc oxide ore sorting method and high-concentration pulping and low-concentration flotation technology, the amine sulfide collector is optimized to solve the problems of low lead-zinc oxide ore flotation recovery rate and large desliming volume. More efficient zinc and lead recovery and a stable production process are achieved.

CN118719306AActive Publication Date: 2024-10-01CHINA ENFI ENG CORP +1

Patent Information

Application Number
CN202411043759.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-01
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The comprehensive flotation recovery rate of lead oxide zinc ore is low, and the desliming amount in the existing technology is large and unstable, resulting in a large loss of zinc metal, making it difficult to achieve the ideal separation effect.

Method used

A multi-step lead-zinc oxide separation method is adopted, including adding zinc sulfide inhibitors, lead collectors and frothers to the slurry for flotation, conducting multiple lead sweeps and beneficiations, and then selecting lead tailings. Add zinc sulfide activator and collector for flotation, combine high-concentration pulping and low-concentration flotation technology, and optimize the amine sulfide collector to increase the recovery rate.

Benefits of technology

It reduces the desliming amount of medium ore and zinc metal loss, improves the recovery rate of lead and zinc, achieves a more stable production process, reduces the impact of fine mud on the separation, and improves the concentrate grade and recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719306A_ABST
    Figure CN118719306A_ABST
Patent Text Reader

Abstract

The invention relates to a lead-zinc oxide ore separation method which comprises the following steps: step 1) adding a zinc sulfide inhibitor, a lead collecting agent and a foaming agent into lead-zinc oxide ore pulp for flotation, and performing lead scavenging on lead roughing tailing pulp for multiple times to obtain lead flotation tailings; the lead rough concentrate is subjected to multiple times of concentration to obtain lead concentrate, middling generated by each time of concentration is subjected to cyclone desliming, and settled sand obtained after middling desliming is sent to lead scavenging; secondly, a zinc sulfide activating agent, a zinc sulfide collecting agent and a foaming agent are added into the lead flotation tailings for flotation; performing multiple times of zinc sulfide scavenging on the zinc sulfide roughing tailing slurry to obtain zinc sulfide tailings; the zinc sulfide rough concentrate is subjected to multiple times of concentration to obtain concentrated zinc sulfide ore, middling generated by each time of concentration is subjected to cyclone desliming, and settled sand obtained after middling desliming is sent to zinc sulfide scavenging; and thirdly, zinc oxide flotation is conducted on the zinc sulfide tailings, and zinc oxide concentrate and tailings are obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral separation and processing, and in particular to a method for separating lead-zinc oxide ore. Background Art

[0002] The mineral composition of muddy oxidized lead-zinc ore is complex, with high content of fine mud and soluble salts, and the ore is extremely difficult to be separated, resulting in the unsatisfactory zinc recovery rate of conventional flotation of oxidized lead-zinc ore. At present, the most commonly used mineral processing technology for treating muddy oxidized lead-zinc ore is the sulfidation-amine process. The sulfidation-amine process is very sensitive to ore mud, and generally requires desludging flotation. The traditional process generally desludifies the zinc oxide flotation feed or raw ore, and the desludging amount is large and difficult to control, resulting in a large loss of zinc oxide metal content. At the same time, the separation index fluctuates greatly with the desludging effect, and the on-site production is generally not stable. In order to obtain better separation effects, mineral processing workers have tried a variety of mineral processing methods in recent years, such as flocculation flotation, carrier flotation, flotation using chelating collectors, sulfidation roasting-flotation, and multi-method combination processes. However, these processes have not yet made breakthrough progress, and the low flotation recovery rate of complex oxidized lead-zinc ore has always been a difficult problem in the mineral processing industry.

[0003] Therefore, it is necessary to develop a new method for separating lead-zinc oxide ores to solve the problem of low comprehensive recovery rate of lead-zinc oxide ore flotation in the prior art. Summary of the invention

[0004] The purpose of the present invention is to provide a method for separating lead-zinc oxide ores to solve the problem of low comprehensive recovery rate of lead-zinc oxide ores in flotation. The present invention is implemented by adopting the following technical solutions:

[0005] A method for separating lead-zinc oxide ore comprises the following steps:

[0006] Step 1) adding a zinc sulfide inhibitor, a lead collector and a frother to the oxidized lead-zinc ore pulp for flotation to obtain a lead roughing tailing pulp and a lead rough concentrate; performing lead scavenging on the lead roughing tailing pulp for multiple times to obtain lead tailings, and returning the scavenged concentrate obtained from each lead scavenging to the previous level; performing multiple concentrating on the lead rough concentrate to obtain a lead concentrate, and desludging the middlings produced from each concentrating in a cyclone, and sending the sediment after desludging the middlings to the lead scavenging;

[0007] Step 2) adding a zinc sulfide activator, a zinc sulfide collector and a frother to the lead tailings for flotation to obtain a zinc sulfide coarse concentrate and a zinc sulfide rougher tailings slurry; performing zinc sulfide scavenging on the zinc sulfide rougher tailings slurry for multiple times to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing multiple concentration on the zinc sulfide coarse concentrate to obtain a concentrated zinc sulfide ore, and performing a cyclone desludging on the middlings produced by each concentration, and the sediment after the desludging of the middlings is sent to the zinc sulfide scavenging;

[0008] Step 3) The zinc sulfide tailings are subjected to zinc oxide flotation to obtain zinc oxide concentrate and tailings.

[0009] Optionally, the zinc sulfide inhibitor is zinc sulfate and sodium sulfite, and the addition ratio of zinc sulfate to sodium sulfite is 1:0.5-1.

[0010] Optionally, the lead collector is at least one of No. 25 black medicine, butyl ammonium black medicine, isobutyl sodium black medicine and the like.

[0011] Optionally, in the step 1), the lead rough concentrate is beneficiated three times, and a zinc sulfide inhibitor is added during each beneficiation process;

[0012] In the step 1), the lead rough concentrate is subjected to secondary lead scavenging, and a lead collector is added in each lead scavenging.

[0013] Optionally, the zinc sulfide collector is at least one of butyl xanthate, pentyl xanthate, isobutyl xanthate, and isopentyl xanthate; and the zinc sulfide activator is copper sulfate.

[0014] Optionally, in the step 3), the zinc sulfide tailings are first desludged by a cyclone to remove overflow, so that the concentration of the zinc sulfide tailings is increased to 40-45%, and then a slurry conditioner, a zinc oxide activator, and a zinc oxide collector are added and mixed evenly, and then diluted with water to reduce the concentration of the zinc sulfide tailings to 15-25% before flotation.

[0015] Optionally, a pyrite inhibitor and a zinc sulfide collector are added to the concentrated zinc sulfide ore obtained in step 2) to carry out zinc-sulfur separation flotation to obtain a zinc sulfide concentrate and a sulfur concentrate.

[0016] Optionally, in the step 3), zinc oxide flotation is performed on the zinc sulfide flotation tailings, and the operation includes slurry adjustment after pulp concentration and two-stage roughing operations after pulp dilution. The pulp is concentrated to a concentration of 40-45%, and then sodium carbonate, sodium hexametaphosphate, sodium sulfide and zinc oxide collector are added for slurry adjustment. After the reagents are fully effective, the pulp concentration is diluted with water to 15-25% for flotation. This stage of operation obtains zinc oxide concentrate and final tailings.

[0017] Optionally, the zinc oxide collector is composed of an amine cationic collector and a chelating collector in a ratio of 10 to 20:1;

[0018] The amine cationic collector can be one or more amine collectors such as dodecylamine, octadecylamine, mixed amines, etc., and the chelating collector can be one or more hydroxamic acids such as benzohydroxamic acid, salicylic hydroxamic acid, octyl hydroxamic acid, etc.

[0019] Optionally, the foaming agent is one or more alcohols or ether alcohols such as No. 2 oil, MIBC, and diethylene glycol methyl ether.

[0020] Optionally, the oxidized lead-zinc ore slurry is prepared by the following method: the oxidized lead-zinc ore and sodium sulfide are ground in a mill, and the amount of sodium sulfide added is 500-1500 g / t; the final fineness of the ore is -0.074 mm particle size accounting for 75%-85%, and the final mass concentration of the floating slurry is 30%-35%.

[0021] Optionally, in the step 1), 600-800 g / t of zinc sulfate, 300-400 g / t of sodium sulfite, 60-80 g / t of lead collector and 25-30 g / t of frother are added to the oxidized lead-zinc ore pulp; 10-15 g / t of lead collector is added in the first lead scavenging, and 5-10 g / t of lead collector is added in the second scavenging to obtain lead tailings; the lead rough concentrate is subjected to three concentrations, 200-250 g / t of zinc sulfate and 100-150 g / t of sodium sulfite are added in the first concentration, 100-150 g / t of zinc sulfate and 50-100 g / t of sodium sulfite are added in the second concentration, and 50-60 g / t of zinc sulfate and 20-25 g / t of sodium sulfite are added in the third concentration to obtain lead concentrate.

[0022] In the step 2), 150-200 g / t of copper sulfate, 60-80 g / t of zinc sulfide collector and 25-30 g / t of No. 2 oil are added to the lead tailings for flotation to obtain zinc sulfide coarse concentrate and zinc sulfide roughing tailings slurry; the zinc sulfide roughing tailings slurry is subjected to two zinc sulfide scavengings, 20-30 g / t of zinc sulfide collector is added in the first scavenging, and 10-15 g / t of zinc sulfide collector is added in the second scavenging.

[0023] In the step 3), 2500-3000 g / t of sodium carbonate, 250-300 g / t of sodium hexametaphosphate, 7000-8000 g / t of sodium sulfide, 80-100 g / t of amine cation collector, and 20-30 g / t of chelating collector are added to the zinc sulfide tailings, and the mixture is evenly mixed, and then the zinc oxide is subjected to a first-stage roughing flotation. Then, 1500-2000 g / t of sodium sulfide and 60-100 g / t of dodecylamine are added to the tailings for a second-stage roughing to obtain zinc oxide concentrate and tailings.

[0024] Optionally, 2000-2500 g / t of calcium oxide and 10 g-15 g / t of collector are added to the selected zinc sulfide ore for zinc-sulfur separation and rough selection to obtain zinc sulfide and sulfur; the zinc sulfide is separated and selected twice, 400-500 g / t of calcium oxide is added for the first time, and 250-300 g / t of calcium oxide is added for the second time to obtain zinc sulfide concentrate; the sulfur is scavenged twice, 5-10 g / t of collector is added for the first scavenging, and 2-5 g / t of collector is added for the second scavenging to obtain sulfur concentrate, and the middlings from each separation and selection and separation scavenging are returned to the previous level.

[0025] The amount of reagents added in the above steps is based on the weight of the dry ore to be treated.

[0026] Compared with the prior art, the present invention has the following advantages and effects:

[0027] The present invention desludging the middlings of lead flotation and zinc sulfide flotation, not only the desludging operation processing volume is small. Moreover, because the fine mud contained in the middlings is fine mud with good floatability and great influence on zinc oxide flotation, selective desludging is achieved by processing the middlings, the desludging yield is below 10%, and the zinc metal amount is also controlled below 10% with the loss of fine mud, which greatly reduces the loss of zinc metal amount. The traditional process is mostly to desludging the raw ore or zinc oxide flotation feed, the desludging operation feed volume is large, all the fine mud in the ore is desludging, there is no selectivity and the desludging amount is large, the desludging yield is basically above 15%, and the zinc metal loss is also above 15%.

[0028] The zinc oxide flotation of the present invention adopts the method of high-concentration slurry adjustment and low-concentration flotation. First, the zinc oxide flotation feed slurry is densely packed and its concentration is increased to 40-45%. At this concentration, the beneficiation agent is added to improve the concentration and effect of the agent, especially the effect of sodium sulfide, and promote the zinc oxide collector to act on the surface of the zinc oxide mineral. After the agent acts at a high concentration, the pulp concentration is reduced to 20-25%, which can disperse the pulp and reduce the adverse effect of fine mud on the flotation of amine agents. At the same time, the viscosity of the flotation foam of the amine collector is reduced, and the concentrate grade and recovery rate are improved through high-concentration slurry adjustment and low-concentration flotation.

[0029] The invention optimizes the sulfidation amine collector, and adds a small amount of chelating collector on the basis of the amine collector of the traditional process, thereby improving the recovery rate of the difficult-to-select zinc oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is the process flow chart of Example 1.

[0031] Figure 2 It is a traditional process. DETAILED DESCRIPTION

[0032] In order to make the purpose and technical solution of the present invention more clear, the present invention is further described in detail. The experimental methods described in the following examples are all conventional methods unless otherwise specified: if no specific techniques or conditions are specified in the examples, they are carried out according to the techniques or conditions described in the literature in the field or according to the product instructions; the reagents and materials, unless otherwise specified, can be obtained from commercial channels.

[0033] Embodiment 1:

[0034] A certain oxidized lead-zinc ore contains 1.23% lead and 6.45% zinc, with oxidation rates of lead and zinc of 75% and 80% respectively. Figure 1 The process flow shown:

[0035] Step 1) First, grind the lead-zinc oxide ore and sodium sulfide in a mill, and add 1000g / t of sodium sulfide; the final fineness of the ore is -0.074mm, accounting for 80%, and the final mass concentration of the floating slurry is 30% to 35%. 800 g / t of zinc sulfate, 400 g / t of sodium sulfite, 80 g / t of butyl ammonium black powder and 30 g / t of frother No. 2 oil are added to the oxidized lead-zinc ore pulp for flotation to obtain lead roughing tailings pulp and lead rough concentrate; the lead roughing tailings pulp is subjected to lead scavenging twice, 20 g / t of butyl ammonium black powder is added in the first scavenging, and 10 g / t of butyl ammonium black powder is added in the second scavenging to obtain lead tailings, and the scavenged concentrate obtained by each lead scavenging is returned to the previous level; the lead rough concentrate is subjected to three concentrations, 200 g / t of zinc sulfate and 100 g / t of sodium sulfite are added in the first concentration, 100 g / t of zinc sulfate and 50 g / t of sodium sulfite are added in the second concentration, and 50 g / t of zinc sulfate and 25 g / t of sodium sulfite are added in the third concentration to obtain lead concentrate, and the middlings produced in each concentration are subjected to cyclone desliming, and the sediment after desliming of the middlings is sent to lead scavenging;

[0036] Step 2) adding 200 g / t of copper sulfate, 80 g / t of butyl xanthate and 30 g / t of No. 2 oil to the lead tailings for flotation to obtain zinc sulfide rough concentrate and zinc sulfide rougher tailings slurry; performing zinc sulfide scavenging on the zinc sulfide rougher tailings slurry twice, adding 20 g / t of butyl xanthate for the first scavenging, and adding 10 g / t of butyl xanthate for the second scavenging to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing three concentrations on the zinc sulfide rough concentrate to obtain concentrated zinc sulfide ore, and desludging the middlings produced by each concentration by a cyclone, and the sediment after desludging the middlings is sent to zinc sulfide scavenging;

[0037] The selected zinc sulfide ore is added with 2000g / t calcium oxide and 10g / t butyl xanthate for zinc-sulfur separation and rough selection to obtain zinc sulfide and sulfur; the zinc sulfide is separated and selected twice, 500g / t calcium oxide is added for the first time, and 250g / t calcium oxide is added for the second time to obtain zinc sulfide concentrate; the sulfur is scavenged twice, 5g / t butyl xanthate is added for the first scavenging, and 2g / t butyl xanthate is added for the second scavenging to obtain sulfur concentrate, and the middlings from each separation and separation are returned to the previous level.

[0038] Step 3) First, the zinc sulfide tailings are desludged by a cyclone to remove the overflow, so that the concentration of the zinc sulfide tailings is increased to 40%, and then 3000g / t of sodium carbonate, 300g / t of sodium hexametaphosphate, 8000g / t of sodium sulfide, 100g / t of dodecylamine, and 20g / t of benzohydroxamic acid are added and mixed evenly, and then diluted with water to reduce the concentration of the zinc sulfide tailings to 20%, and then the zinc oxide is subjected to a roughing flotation, and the tailings are then added with 2000g / t of sodium sulfide and 100g / t of dodecylamine for a second roughing to obtain zinc oxide concentrate and tailings. The amount of reagent added in each of the above steps is based on the weight of the dry ore to be treated.

[0039] Finally, lead concentrate with a lead grade of 45% and a lead recovery rate of 67%, zinc sulfide concentrate with a zinc grade of 49% and a zinc recovery rate of 15%, and zinc oxide concentrate with a zinc grade of 26% and a zinc recovery rate of 68% can be obtained.

[0040] Comparative Example 1

[0041] according to Figure 2 The conventional sulfurization-amine process shown includes the following steps:

[0042] Step 1) First, grind the lead-zinc oxide ore and sodium sulfide in a mill, and add 1000g / t of sodium sulfide; the final fineness of the ore is -0.074mm, accounting for 80%, and the final mass concentration of the floating slurry is 30% to 35%. 800 g / t of zinc sulfate, 400 g / t of sodium sulfite, 80 g / t of ammonium butyl black powder and 30 g / t of frother are added to the oxidized lead-zinc ore pulp for flotation to obtain lead roughing tailing pulp and lead rough concentrate; the lead roughing tailing pulp is subjected to lead scavenging twice, 20 g / t of ammonium butyl black powder is added in the first scavenging, and 10 g / t of ammonium butyl black powder is added in the second scavenging to obtain lead tailings, and the scavenging concentrate obtained by each lead scavenging is returned to the previous level; the lead rough concentrate is subjected to three concentrations, 200 g / t of zinc sulfate and 100 g / t of sodium sulfite are added in the first concentration, 100 g / t of zinc sulfate and 50 g / t of sodium sulfite are added in the second concentration, and 50 g / t of zinc sulfate and 25 g / t of sodium sulfite are added in the third concentration to obtain lead concentrate, and the middlings produced by each concentration are returned to the previous level;

[0043] Step 2) adding 200 g / t of copper sulfate, 80 g / t of butyl xanthate and 30 g / t of No. 2 oil to the lead tailings for flotation to obtain zinc sulfide rough concentrate and zinc sulfide rougher tailings slurry; performing zinc sulfide scavenging on the zinc sulfide rougher tailings slurry twice, adding 20 g / t of butyl xanthate for the first scavenging, and adding 10 g / t of butyl xanthate for the second scavenging to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing three concentrations on the zinc sulfide rough concentrate to obtain concentrated zinc sulfide ore, and returning the middling ore produced by each concentration to the previous level;

[0044] The selected zinc sulfide ore is added with 2000g / t calcium oxide and 10g / t butyl xanthate for zinc-sulfur separation and rough selection to obtain zinc sulfide and sulfur; the zinc sulfide is separated and selected twice, 500g / t calcium oxide is added for the first time, and 250g / t calcium oxide is added for the second time to obtain zinc sulfide concentrate; the sulfur is scavenged twice, 5g / t butyl xanthate is added for the first scavenging, and 2g / t butyl xanthate is added for the second scavenging to obtain sulfur concentrate, and the middlings from each separation and separation are returned to the previous level.

[0045] Step 3) The zinc sulfide tailings are desludged by a cyclone to remove the overflow. The concentration of the zinc sulfide tailings is 30%. Then, 3000g / t of sodium carbonate, 300g / t of sodium hexametaphosphate, 8000g / t of sodium sulfide, and 100g / t of dodecylamine are added and mixed evenly, and then diluted with water to reduce the concentration of the zinc sulfide tailings to 20%. Then, zinc oxide is subjected to a first-stage roughing flotation. The tailings are then added with 2000g / t of sodium sulfide and 100g / t of dodecylamine for a second-stage roughing to obtain zinc oxide concentrate and tailings. The amount of reagent added in each of the above steps is based on the weight of the dry ore to be treated.

[0046] Results The indicators of lead concentrate and zinc sulfide concentrate did not change much, but the zinc grade of zinc oxide concentrate was 24% and the zinc recovery rate was only 60%, which was greatly reduced.

[0047] Embodiment 2:

[0048] A certain oxidized lead-zinc ore contains 0.89% lead and 5.65% zinc, and the oxidation rates of lead and zinc are 70% and 75% respectively. The following method is used for treatment:

[0049] Step 1) First, grind the oxidized lead-zinc ore and sodium sulfide in a mill, and add 800g / t of sodium sulfide; the final fineness of the ore is -0.074mm, accounting for 80%, and the final mass concentration of the floating slurry is 30% to 35%. Add 600g / t of zinc sulfate, 300g / t of sodium sulfite, 60g / t of butyl ammonium black powder and 25g / t of frother No. 2 oil to the oxidized lead-zinc ore pulp for flotation to obtain lead roughing tailing pulp and lead rough concentrate; perform lead scavenging on the lead roughing tailing pulp twice, add 15g / t of butyl ammonium black powder in the first scavenging, and add 5g / t of butyl ammonium black powder in the second scavenging to obtain lead tailings, and return the scavenged concentrate obtained by each lead scavenging to the previous level; perform three concentrations on the lead rough concentrate, add 250g / t of zinc sulfate and 150g / t of sodium sulfite in the first concentration, add 150g / t of zinc sulfate and 50g / t of sodium sulfite in the second concentration, and add 50g / t of zinc sulfate and 25g / t of sodium sulfite in the third concentration to obtain lead concentrate, and desludging the middlings produced by each concentration by cyclone, and the sediment after desludging of the middlings is sent to lead scavenging;

[0050] Step 2) adding 150 g / t of copper sulfate, 60 g / t of butyl xanthate and 25 g / t of No. 2 oil to the lead tailings for flotation to obtain zinc sulfide rough concentrate and zinc sulfide rougher tailings slurry; performing zinc sulfide scavenging on the zinc sulfide rougher tailings slurry twice, adding 20 g / t of butyl xanthate for the first scavenging, and adding 10 g / t of butyl xanthate for the second scavenging to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing three concentrations on the zinc sulfide rough concentrate to obtain concentrated zinc sulfide ore, and performing cyclone desludging on the middlings produced by each concentration, and the sediment after desludging of the middlings is sent to zinc sulfide scavenging;

[0051] The selected zinc sulfide ore is added with 2500g / t calcium oxide and 10g / t butyl xanthate for zinc-sulfur separation and rough selection to obtain zinc sulfide and sulfur; the zinc sulfide is separated and selected twice, 500g / t calcium oxide is added for the first time, and 250g / t calcium oxide is added for the second time to obtain zinc sulfide concentrate; the sulfur is scavenged twice, 5g / t butyl xanthate is added for the first scavenging, and 2g / t butyl xanthate is added for the second scavenging to obtain sulfur concentrate, and the middlings from each separation and separation scavenging are returned to the previous level.

[0052] Step 3) First, the zinc sulfide tailings are desludged by a cyclone to remove the overflow, so that the concentration of the zinc sulfide tailings is increased to 40%, and then 2500g / t of sodium carbonate, 250g / t of sodium hexametaphosphate, 7000g / t of sodium sulfide, 80g / t of dodecylamine, and 20g / t of benzohydroxamic acid are added and mixed evenly, and then the zinc oxide is subjected to a roughing flotation, and the tailings are then added with 1500g / t of sodium sulfide and 60g / t of dodecylamine for a second roughing to obtain zinc oxide concentrate and tailings. The amount of reagent added in each of the above steps is based on the weight of the dry ore to be treated.

[0053] Finally, lead concentrate with a lead grade of 43% and a lead recovery rate of 64%, zinc sulfide concentrate with a zinc grade of 49% and a zinc recovery rate of 21%, and zinc oxide concentrate with a zinc grade of 25% and a zinc recovery rate of 61% can be obtained.

[0054] Comparative Example 2

[0055] according to Figure 2 The conventional amine sulfidation process shown includes the following steps:

[0056] Step 1) First, grind the oxidized lead-zinc ore and sodium sulfide in a mill, and add 800g / t of sodium sulfide; the final fineness of the ore is -0.074mm, accounting for 80%, and the final mass concentration of the floating slurry is 30% to 35%. Add 600g / t of zinc sulfate, 300g / t of sodium sulfite, 60g / t of butyl ammonium black powder and 25g / t of frother No. 2 oil to the oxidized lead-zinc ore pulp for flotation to obtain lead roughing tailing pulp and lead rough concentrate; perform lead scavenging on the lead roughing tailing pulp twice, add 15g / t of butyl ammonium black powder in the first scavenging, and add 5g / t of butyl ammonium black powder in the second scavenging to obtain lead tailings, and the scavenged concentrate obtained by each lead scavenging is returned to the previous level; perform three concentrations on the lead rough concentrate, add 250g / t of zinc sulfate and 150g / t of sodium sulfite in the first concentration, add 150g / t of zinc sulfate and 50g / t of sodium sulfite in the second concentration, and add 50g / t of zinc sulfate and 25g / t of sodium sulfite in the third concentration to obtain lead concentrate, and the middlings produced by each concentration are returned to the previous level;

[0057] Step 2) adding 150 g / t of copper sulfate, 60 g / t of butyl xanthate and 25 g / t of No. 2 oil to the lead tailings for flotation to obtain zinc sulfide rough concentrate and zinc sulfide rougher tailings slurry; performing zinc sulfide scavenging on the zinc sulfide rougher tailings slurry twice, adding 20 g / t of butyl xanthate for the first scavenging, and adding 10 g / t of butyl xanthate for the second scavenging to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing three concentrations on the zinc sulfide rough concentrate to obtain concentrated zinc sulfide ore, and returning the middling ore produced by each concentration to the previous level;

[0058] The selected zinc sulfide ore is added with 2500g / t calcium oxide and 10g / t butyl xanthate for zinc-sulfur separation and rough selection to obtain zinc sulfide and sulfur; the zinc sulfide is separated and selected twice, 500g / t calcium oxide is added for the first time, and 250g / t calcium oxide is added for the second time to obtain zinc sulfide concentrate; the sulfur is scavenged twice, 5g / t butyl xanthate is added for the first scavenging, and 2g / t butyl xanthate is added for the second scavenging to obtain sulfur concentrate, and the middlings from each separation and separation scavenging are returned to the previous level.

[0059] Step 3) The zinc sulfide tailings are desludged by a cyclone to remove the overflow, the concentration of the zinc sulfide tailings is 30%, and then 2500g / t of sodium carbonate, 250g / t of sodium hexametaphosphate, 7000g / t of sodium sulfide, and 80g / t of dodecylamine are added and mixed evenly, and then the zinc oxide is subjected to a roughing flotation, and the tailings are then added with 2000g / t of sodium sulfide and 100g / t of dodecylamine for a second roughing to obtain zinc oxide concentrate and tailings. The amount of reagent added in each of the above steps is based on the weight of the dry ore to be treated.

[0060] Results The indicators of lead concentrate and zinc sulfide concentrate did not change much, but the zinc grade of zinc oxide concentrate was 23% and the zinc recovery rate was only 55%, which was greatly reduced.

[0061] Example 3

[0062] Compared with Example 2, the lead flotation and zinc sulfide flotation processes are the same, but in step 3), the zinc oxide flotation does not perform high-concentration slurry adjustment and low-concentration flotation, and the zinc sulfide tailings are directly desludged by a cyclone to remove the overflow and the zinc sulfide tailings with a concentration of 30% are flotated, and the other steps are the same. As a result, the zinc oxide concentrate has a zinc grade of 25% and a recovery rate of 59%.

[0063] Comparative Example 3

[0064] Compared with Example 2, the other steps are the same, but in step 3), benzohydroxamic acid is not added for flotation, and the other steps are the same. Results The zinc grade of the zinc oxide concentrate is 24% and the recovery rate is 59%.

[0065] In addition, it should be noted that the above are only preferred embodiments of the present invention and are not limited to the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions recorded in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for separating lead-zinc oxide ore, characterized in that: The following steps are involved: Step 1) adding a zinc sulfide inhibitor, a lead collector, and a frother to the lead-zinc oxide ore pulp for flotation to obtain a lead rougher tailings pulp and a lead rough concentrate; performing multiple lead scavenging on the lead rougher tailings pulp to obtain lead tailings, and returning the scavenged concentrate obtained from each lead scavenging to the previous level; performing multiple beneficiation on the lead rougher concentrate to obtain a lead concentrate, and desludging the middlings produced from each beneficiation in a cyclone, and sending the sand after desludging the middlings to the lead scavenging; Step 2) adding a zinc sulfide activator, a zinc sulfide collector and a frother to the lead tailings for flotation to obtain a zinc sulfide coarse concentrate and a zinc sulfide rougher tailings slurry; performing multiple zinc sulfide scavenging on the zinc sulfide rougher tailings slurry to obtain zinc sulfide tailings, and returning the scavenged concentrate obtained by each zinc sulfide scavenging to the previous level; performing multiple concentration on the zinc sulfide rougher concentrate to obtain concentrated zinc sulfide ore, and performing a cyclone desludging on the middlings produced by each concentration, and sending the sediment after the desludging of the middlings to the zinc sulfide scavenging; Step 3) performing zinc oxide flotation on the zinc sulfide tailings to obtain a zinc oxide concentrate and tailings.

2. The method for separating lead-zinc oxide ore according to claim 1, wherein: The zinc sulfide inhibitor is zinc sulfate and sodium sulfite, and the addition ratio of zinc sulfate to sodium sulfite is 1:0.5-1.

3. The method for separating lead-zinc oxide ore according to claim 1, wherein: The lead collector is at least one of No. 25 lead scavenger, butyl ammonium lead scavenger, isobutyl sodium lead scavenger, and the like.

4. The method for separating lead-zinc oxide ore according to claim 1, wherein: In the step 1), the lead crude concentrate is subjected to three concentrations, and a zinc sulfide inhibitor is added during each concentration process; In the step 1), the lead concentrate is subjected to secondary lead scavenging, and a lead collector is added in each lead scavenging.

5. The method for separating lead-zinc oxide ore according to claim 1, wherein: The zinc sulfide collector is at least one of butyl xanthate, pentyl xanthate, isobutyl xanthate and isoamyl xanthate; and the zinc sulfide activator is copper sulfate.

6. The method for separating lead-zinc oxide ore according to claim 1, wherein: In the step 3), the zinc sulfide tailings are first desludged in a cyclone to remove overflow, so that the concentration of the zinc sulfide tailings is increased to 40-45%, and then a slurry conditioner, a zinc oxide activator, and a zinc oxide collector are added and mixed uniformly, and then diluted with water to reduce the concentration of the zinc sulfide tailings to 15-25% before flotation.

7. The method for separating lead-zinc oxide ore according to claim 1, wherein: Adding pyrite inhibitor and zinc sulfide collector to the concentrated zinc sulfide ore obtained in step 2) to carry out zinc-sulfur separation flotation to obtain zinc sulfide concentrate and sulfur concentrate.

8. The method for separating lead-zinc oxide ore according to claim 1, wherein: The zinc oxide collector is composed of an amine cationic collector and a chelating collector in a ratio of 10 to 20:1; The amine cationic collector is at least one of amine collectors such as dodecylamine, octadecylamine, and mixed amines, and the chelating collector is at least one of hydroxamic acids such as benzohydroxamic acid, salicylic hydroxamic acid, and octyl hydroxamic acid.

9. The method for separating lead-zinc oxide ore according to claim 1, wherein: The foaming agent is one or more alcohols or ether alcohols such as No. 2 oil, MIBC, and diethylene glycol methyl ether.

10. The method for separating lead-zinc oxide ore according to claim 1, wherein: The lead-zinc oxide ore slurry is prepared by the following method: the lead-zinc oxide ore and sodium sulfide are ground in a mill, and the amount of sodium sulfide added is 500-1500 g / t; the final fineness of the ore is -0.074 mm particle size accounting for 75%-85%, and the final mass concentration of the flotation slurry is 30%-35%.

Citation Information

Patent Citations

  • Beneficiation method of high-mud fine-grained copper oxide ore

    CN110216018A

  • Zinc oxide flotation recovery method based on combination of gravity and flotation selection and pre-desliming

    CN114054200A

  • Zinc oxide ore flotation method

    CN117960366A

  • Beneficiation method for zinc oxide mine

    CN1820853A

  • Process for increasing the selectivity of mineral flotation

    US4735783A

Cited By

  • Beneficiation method for lead-zinc separation of lead-zinc sulfide ore containing extremely low copper sulfide

    CN119702240A