Production method of high-strength low-cost HRB600 coiled snail
Through the multi-stage controlled rolling and controlled cooling process, the problems of high alloy cost and poor flowability in the production of HRB600 spiral snails are solved, high-strength and low-cost production is achieved, and the high quality and stability of the product are ensured.
Patent Information
- Application Number
- CN202410792583.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
AI Technical Summary
The existing HRB600 plate snail production process has high alloy costs, high production and operation costs, and poor product flowability, which cannot meet users' high-quality needs.
Adopting a multi-stage controlled rolling and controlled cooling process, including heating furnace, rough rolling mill, intermediate rolling mill, pre-finishing rolling mill, finishing rolling mill, reducing mill and air-cooling line cooling, by controlling the heating temperature, rolling parameters and cooling methods , reduce alloy costs, ensure structural uniformity and grain size, and achieve closed-loop control.
It reduces the cost of Mn and V alloys, avoids the generation of abnormal martensitic structures, improves the strength and toughness of the product, realizes the production of high-strength and low-cost HRB600 plate snails, and improves production stability and product competitiveness.
Smart Images

Figure CN118719796A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rolling of a steel wire rod coil production line, and in particular to a high-strength and low-cost HRB600 coil production method. Background Art
[0002] The production of coiled steel bars is mainly focused on improving product quality, production efficiency, reducing costs and meeting the needs of different fields for high-strength and high-toughness steel. Here are some key points:
[0003] 1. Development of hot rolling technology: As a type of hot-rolled ribbed steel bar, the production process of coil involves continuous plastic deformation of the billet heated to high temperature through a series of rotating rollers, and finally forms a finished product with a specific transverse rib shape. With the advancement of hot rolling technology, such as the application of controlled cooling technology and micro-alloying technology, coils with higher strength levels can be produced, such as HRB500, HRB600, etc., meeting the construction industry's demand for high-strength materials.
[0004] 2. Energy saving and consumption reduction: With the rising energy costs and the improvement of environmental protection requirements, the development of low-energy production methods has become a trend. For example, the production method of rolling 8mm coils with 24 passes can significantly improve economic benefits and reduce energy consumption compared to traditional methods.
[0005] 3. Production process optimization: In order to improve the performance and production efficiency of coil, a series of optimizations have been made to the production process, including the mismatched roller diameter method and the fine grain production process. The mismatched roller diameter method can be flexibly adjusted on the collectively driven high-speed wire mill to solve the problem of unadjustable rack speed in production, optimize the production process, and reduce production costs. The fine grain production process controls the cooling rate and heat treatment process to obtain a finer and more uniform grain structure, thereby improving the strength and toughness of the steel.
[0006] 4. Automation and intelligence: With the development of automation and intelligent technology, more and more automated equipment and intelligent control systems are used in the material handling, temperature control, quality inspection and other links in the production process of coils, which improves production efficiency and the stability of product quality.
[0007] 5. Environmental protection requirements: The increasingly stringent environmental protection laws and regulations have prompted more attention to energy conservation, emission reduction and waste treatment in the production process of coils, such as the use of environmentally friendly lubricants and the optimization of exhaust gas emission treatment systems.
[0008] 6. Standardization and certification: In order to ensure product quality and market competitiveness, the production of coils must comply with national or international standards, such as the Chinese national standard GB / T 1499 series for hot-rolled ribbed steel bars. Certification by authoritative organizations such as the Shanghai Stock Exchange Certification can improve market acceptance.
[0009] The existing HRB600 coil production process mainly has the following problems:
[0010] 1. Conventional or existing HRB600 uses high alloy components, such as Nb, V and Ti alloys, which require high heating temperature and long heat preservation time, increasing heating cost and high alloy cost. Some production processes adopt rapid cooling after rolling, which produces more abnormal martensitic low-temperature structures in the organization, and the organization and performance of the product are easily unqualified, which cannot meet the high-quality needs of users.
[0011] 2. Conventional HRB600 production has a low yield rate. In addition to the conventional flying shear after rough rolling, intermediate rolling and pre-finishing rolling, the coil needs to be cut and trimmed, and the length of the cut is generally greater than 3 turns, the weight is heavy, the yield rate is low, and the production and operation costs of the enterprise are increased.
[0012] 3. In the existing HRB600 production, the reduction of the final rolling unit is low, and the final rolling unit cannot be used for large reduction rolling, resulting in high alloy costs; the production process of rapid cooling after rolling is adopted, and abnormal martensitic low-temperature structure is produced in the organization, and the organization and performance of the product are unqualified.
[0013] 4. In the existing HRB600 production, the final rolling unit cannot achieve closed-loop control, the smoothness of the final product cannot be guaranteed, and stable negative deviation rolling cannot be achieved. The company's production cost is high and the product competitiveness is not strong.
[0014] Therefore, it is necessary to design a high-strength and low-cost HRB600 coil production method to solve the problems of high alloy cost, high production and operation cost, and poor product smoothness in the existing HRB600 coil production. Summary of the invention
[0015] In view of the problems existing in the prior art, the object of the present invention is to provide a high-strength and low-cost HRB600 coil production method.
[0016] The technical solution adopted by the present invention to solve the technical problem is: a high-strength and low-cost HRB600 spiral shell production method, comprising the following steps:
[0017] S1, heating furnace heating: the billet is heated three times and the rolling temperature is finally controlled;
[0018] S2, rough rolling unit rolling: control the average elongation coefficient of rough rolling passes, rough rolling entrance speed, rough rolling exit speed, and rough rolling exit material diameter;
[0019] S3, intermediate rolling unit rolling: After the rough rolling and flying shear head, it enters the intermediate rolling unit to control the average elongation coefficient of the intermediate rolling pass, the temperature entering the intermediate rolling, the intermediate rolling entrance speed, the intermediate rolling exit speed, and the intermediate rolling exit material diameter;
[0020] S4, pre-finishing rolling unit rolling: after intermediate rolling and shearing, the tail is sheared and enters the pre-finishing rolling unit, and the average elongation coefficient of the pre-finishing rolling pass, the pre-finishing rolling temperature, the pre-finishing rolling entrance speed, the pre-finishing rolling exit speed, and the pre-finishing rolling exit material diameter are controlled;
[0021] S5, finishing mill rolling: After the pre-finishing rolling and the flying shear head, it enters the finishing mill, controls the average elongation coefficient of the finishing pass, the finishing temperature, the finishing entrance speed, the finishing exit speed, and the finishing exit material diameter. Before finishing rolling, the 1# and 2# water tanks are used to reduce the temperature by 225℃ in total, and the temperature is returned to 850-950℃ before finishing rolling;
[0022] S6, reducing mill rolling: control the average elongation coefficient of the reducing pass, the temperature of the reducing mill, the inlet speed of the reducing mill, the outlet speed of the reducing mill, and the outlet material diameter of the reducing mill. Use 3# and 4# water tanks before the reducing mill. The 3# water tank is cooled by 120℃, and the 4# water tank is cooled by 40℃. The temperature is returned to 800-900℃ before the reducing mill.
[0023] S7, diameter measurement and closed-loop control with diameter gauge: The diameter gauge is set before the finishing mill, before the diameter reducing mill, and after the diameter reducing mill to detect the inlet size and outlet size of the diameter reducing mill in real time;
[0024] S8, Spinning machine: After the diameter reduction, the 5# and 6# water cooling boxes cool down by 190℃, and then return to the temperature of 750-920℃ after reaching the spinning machine;
[0025] S9, fan cooling: after spinning into a coil, the coil is cooled by air cooling line control;
[0026] S10, Rolling and Collection: After being cooled by the fan of the air cooling line, the coils are collected and transported and cooled on the PF line. Finally, they are weighed, collected and stored after being bundled.
[0027] Specifically, the composition of the HRB600 coiled snail includes, by mass percentage: C: 0.22-0.28%, Si: ≤0.65%, Mn: ≤1.45%, V: ≤0.050%, P: ≤0.040%, S: ≤0.040%, N: ≤0.010%, O: ≤28ppm, and the remainder is Fe and inevitable residual elements including but not limited to Ti, Nb, Cu, and Ni.
[0028] Specifically, the billet size in step S1 is a square billet of 165×165×12000 mm, the three heating temperatures are respectively controlled at 870°C-980°C, 980°C-1110°C, and 1070°C-1190°C, the uniform heating temperature of the billet in the heating furnace is controlled at 1100°C-1170°C, and the start rolling temperature is controlled at 980°C-1050°C.
[0029] Specifically, the average elongation coefficient of the rough rolling pass in step S2 is 1.373, the rough rolling entrance speed is 0.26 m / s, the rough rolling exit speed is 1.40 m / s, and the rough rolling exit material diameter is φ72 mm.
[0030] Specifically, the average elongation coefficient of the intermediate rolling pass in step S3 is 1.310, the intermediate rolling temperature is 950°C, the intermediate rolling entrance speed is 1.40m / s, the intermediate rolling exit speed is 7.11m / s, and the intermediate rolling exit material diameter is φ32mm.
[0031] Specifically, the average elongation coefficient of the pre-finishing rolling pass in step S4 is 1.290, the pre-finishing rolling temperature is 1050°C, the pre-finishing rolling entrance speed is 7.11m / s, the pre-finishing rolling exit speed is 18.88m / s, and the pre-finishing rolling exit material diameter is φ19.2mm.
[0032] Specifically, the average elongation coefficient of the finishing pass in step S5 is 1.255, the finishing temperature is 850-950°C, the finishing entrance speed is 18.88m / s, the finishing exit speed is 29.26m / s, and the finishing exit material diameter is φ12.4mm.
[0033] Specifically, the average elongation coefficient of the diameter reducing pass in step S6 is 1.248, the temperature of the diameter reducing unit is 800-900°C, the inlet speed of the diameter reducing unit is 29.26m / s, the outlet speed of the diameter reducing unit is 68m / s, and the outlet material diameter of the diameter reducing unit is φ10mm.
[0034] Specifically, the diameter gauge in step S7 provides real-time feedback on the changes in the pre-finishing rolling and finishing rolling material shapes. When the pre-finishing rolling and finishing rolling material shapes fluctuate greatly, the diameter gauge can measure it in the first place and issue an early warning.
[0035] Specifically, the fan in step S9 includes a first section, a second section, a third section and a fourth section, the opening degree of the four sections of the fan is set to 60-80%, and the cooling speed of the four sections of the fan is: 19°C / s for the first section, 15°C / s for the second section, 7°C / s for the third section, and 2°C / s for the fourth section.
[0036] The present invention has the following beneficial effects:
[0037] The high-strength and low-cost HRB600 coil production method designed by the present invention realizes HRB600 rolling production with reduced Mn alloy content and lower V alloy cost; and realizes structure control through controlled rolling and controlled cooling to ensure that the structure has no abnormal martensitic structure and has excellent performance.
[0038] The high-strength and low-cost HRB600 coil production method designed by the present invention realizes the preparation of the structure before phase change through large-pressure rolling with a reducing mill, and the structure is uniform and has a high grain size; it is realized by the diameter gauges before and after the reducing mill unit to detect and feedback the changes in the rolled material shape. When the rolled material shape fluctuates greatly, the diameter gauge can measure it in the first time and can give an early warning, thereby realizing closed-loop control and improving the uniformity of product dimensional accuracy and production stability.
[0039] The high-strength and low-cost HRB600 coil production method designed by the invention adopts high-speed flying shear to cut off the head and tail uncooled sections, and the length of the head and tail cut off without cooling is short, which is reduced by more than 50% compared with conventional shearing of the head and tail. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is the process flow chart for the production of high-strength and low-cost HRB600 coiled steel.
[0041] Figure 2 This is an actual picture of the high-strength and low-cost HRB600 coil.
[0042] Figure 3 It is the metallographic structure of high-strength and low-cost HRB600 coil Figure 1 .
[0043] Figure 4 It is the metallographic structure of high-strength and low-cost HRB600 coil Figure 2 .
[0044] Figure 5 It is the mechanical property curve of high-strength and low-cost HRB600 coil.
[0045] In the figure: 1-heating furnace; 2-roughing mill; 3-intermediate rolling mill; 4-pre-finishing mill; 5-finishing mill; 6-laying machine; 7-air cooling line; 8-coiling drum. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely further describe the technical solutions in the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0047] Embodiment 1:
[0048] like Figure 1-Figure 5 As shown, a high-strength and low-cost HRB600 coil production method comprises the following steps:
[0049] 1. Heating in heating furnace 1: The billet size is 165×165×12000mm. The billet is heated three times and the rolling temperature is finally controlled. The specific controlled temperature values are shown in Table 1 below:
[0050] Table 1 Billet heating temperature values
[0051]
[0052]
[0053] 2. Rolling of rough rolling unit 2: average elongation coefficient of rough rolling pass is 1.373, rough rolling inlet speed is 0.26m / s, rough rolling outlet speed is 1.40m / s, and rough rolling outlet material diameter is φ72mm.
[0054] 3. Intermediate rolling unit 3 rolling: After rough rolling and flying shear head, it enters the intermediate rolling unit, the average elongation coefficient of the intermediate rolling pass is 1.310, the intermediate rolling temperature is 950℃, the intermediate rolling entrance speed is 1.40m / s, the intermediate rolling exit speed is 7.11m / s, and the intermediate rolling exit material diameter is φ32mm.
[0055] 4. Pre-finishing mill group 4 rolling: After intermediate rolling and shearing, it enters the pre-finishing mill group, the average elongation coefficient of the pre-finishing pass is 1.290, the pre-finishing temperature is 1050℃, the pre-finishing entrance speed is 7.11m / s, the pre-finishing exit speed is 18.88m / s, and the pre-finishing exit material diameter is φ19.2mm.
[0056] 5. Finishing mill unit 5 rolling: After pre-finishing rolling and flying shear head, it enters the finishing mill unit, the average elongation coefficient of the finishing pass is 1.255, the finishing temperature is 850-950℃, 1# and 2# water tanks are used before finishing rolling, the temperature is reduced by 225℃ in total, and the temperature is returned to 850-950℃ before finishing rolling, the finishing entrance speed is 18.88m / s, the finishing exit speed is 29.26m / s, and the finishing exit material diameter is φ12.4mm.
[0057] 6. Rolling of the reducing mill: the average elongation coefficient per pass is 1.248, the temperature entering the reducing mill is 800-900℃, 3# and 4# water tanks are used before the reducing mill, the 3# water tank cools down by 120℃, the 4# water tank cools down by 40℃, and the temperature is returned to 800-900℃ before the reducing mill, the inlet speed of the reducing mill is 29.26m / s, the outlet speed of the reducing mill is 68m / s, and the outlet material diameter of the reducing mill is φ10mm.
[0058] 7. Diameter measurement and closed-loop control with diameter gauge: The diameter gauge is installed before the finishing mill, before the reducing mill, and after the reducing mill to detect the inlet size and outlet size of the reducing mill in real time; it provides real-time feedback on changes in pre-finishing and finishing material types. When the pre-finishing and finishing material types fluctuate greatly, the diameter gauge can measure it in the first time and issue an early warning.
[0059] 8. Spinning machine 6: After the diameter reduction, the 5# and 6# water cooling boxes cool down by 190℃ in total, and then return to the temperature of 750-920℃ after reaching the spinning machine;
[0060] 9. Fan cooling: After spinning into a circle, the coil is cooled by air cooling line control; the fan includes the first section, the second section, the third section and the fourth section, the opening degree of the four sections of the fan is set to 60-80%, and the cooling speed of the four sections of the fan is: 19℃ / s for the first section, 15℃ / s for the second section, 7℃ / s for the third section, and 2℃ / s for the fourth section.
[0061] 10. Coil collection: After cooling by the fan of the air cooling line, the coils are collected and transported and cooled on the PF line. Finally, they are weighed, collected and stored after being bundled.
[0062] The composition of HRB600 coiled snail includes, by mass percentage: C: 0.22-0.28%, Si: ≤0.65%, Mn: ≤1.45%, V: ≤0.050%, P: ≤0.040%, S: ≤0.040%, N: ≤0.010%, O: ≤28ppm, the remainder is Fe and unavoidable residual elements including but not limited to Ti, Nb, Cu, Ni. The addition amount in actual operation is shown in Table 2 below:
[0063] Table 2 Mass percentage of components of HRB600 coiled snail.
[0064]
[0065] The temperature control table in the HRB600 coil production process is shown in Table 3 below:
[0066] Table 3 Temperature values in the HRB600 coil production process.
[0067]
[0068] Temperature control case, taking 6mm rolling as an example:
[0069] 1) Case 1: Finishing rolling temperature 900℃ - diameter reduction temperature 850℃ - spinning temperature - 900℃ - high-speed fan cooling;
[0070] 2) Case 2: Finishing temperature 900℃ - diameter reduction temperature 800℃ - spinning temperature - 800℃ - high-speed fan cooling;
[0071] 3) Case 3: Finishing rolling temperature 850℃ - diameter reduction temperature 800℃ - spinning temperature - 800℃ - high-speed fan cooling;
[0072] 4) Case 4: Finishing rolling temperature 850℃ - diameter reducing temperature 800℃ - spinning temperature - 750℃ - high-speed fan cooling.
[0073] Temperature control case, taking rolling 8mm or 10mm as an example:
[0074] 5) Case 5: Finishing temperature 850℃ - diameter reduction temperature 800℃ - spinning temperature - 800℃ - high-speed fan cooling;
[0075] 6) Case 6: Change of composition, finishing temperature 850℃ - diameter reduction temperature 800℃ - spinning temperature -800℃ - high-speed fan cooling.
[0076] The matrix microstructure of high-strength and low-cost HRB600 coiled steel is evenly distributed ferrite + pearlite, and the grain size grade is ≥10.
[0077] The yield strength of high-strength and low-cost HRB600 coil screw is ≥630MPa, the tensile strength is ≥750MPa, the elongation after fracture is ≥16%, and the total elongation at maximum force is ≥9%.
[0078] In the high-strength and low-cost HRB600 coil production method, the average compression ratio of the two passes of the reducing unit is ≥1.25. The compression ratio of the reducing unit is detected and fed back in real time through the diameter gauges before and after the reducing unit. When the rolling material profile fluctuates greatly, the diameter gauge can measure it in the first time and give an early warning to achieve a stable compression ratio.
[0079] In the high-strength and low-cost HRB600 coil production method, the temperature of the rolled piece entering the finishing mill is 800-950°C, the temperature of the rolled piece entering the reducing mill is 780-880°C, and the temperature of the rolled piece entering the laying head is 700-900°C. The rolled piece is cooled by water cooling boxes before the finishing mill 5, after the finishing mill 5 and after the reducing mill, and the lowest cooling temperature of the rolled piece surface is ≥600°C.
[0080] After the reducing mill, a high-speed flying shear is used to cut off the uncooled sections at the head and tail. The length of the uncooled sections at the head and tail is ≤3m.
[0081] The nominal diameters of the final products are 6mm, 8mm, 10mm, and 12mm.
[0082] The mechanical properties data of HRB600 coiled coil are shown in Table 4 below:
[0083] Table 4 Mechanical properties data of HRB600 coil.
[0084]
[0085] The present invention is not limited to the above-mentioned implementation modes, and anyone should be aware of the structural changes made under the enlightenment of the present invention, and all those having the same or similar technical solutions as the present invention fall within the protection scope of the present invention.
[0086] The techniques, shapes, and structural parts not described in detail in the present invention are all well-known techniques.
Claims
1. A high-strength and low-cost HRB600 coil production method, It is characterized in that The following steps are involved: S1, heating furnace heating: the billet is heated three times and the rolling temperature is finally controlled; S2, rough rolling unit rolling: control the average elongation coefficient of rough rolling passes, rough rolling entrance speed, rough rolling exit speed, and rough rolling exit material diameter; S3, intermediate rolling unit rolling: After the rough rolling and flying shear head, it enters the intermediate rolling unit to control the average elongation coefficient of the intermediate rolling pass, the temperature entering the intermediate rolling, the intermediate rolling entrance speed, the intermediate rolling exit speed, and the intermediate rolling exit material diameter; S4, pre-finishing rolling unit rolling: after intermediate rolling and shearing, the tail is sheared and enters the pre-finishing rolling unit, and the average elongation coefficient of the pre-finishing rolling pass, the pre-finishing rolling temperature, the pre-finishing rolling entrance speed, the pre-finishing rolling exit speed, and the pre-finishing rolling exit material diameter are controlled; S5, finishing mill rolling: After the pre-finishing rolling and the flying shear head, it enters the finishing mill, controls the average elongation coefficient of the finishing pass, the finishing temperature, the finishing entrance speed, the finishing exit speed, and the finishing exit material diameter. Before finishing rolling, the 1# and 2# water tanks are used to reduce the temperature by 225℃ in total, and the temperature is returned to 850-950℃ before finishing rolling; S6, reducing mill rolling: control the average elongation coefficient of the reducing pass, the temperature of the reducing mill, the inlet speed of the reducing mill, the outlet speed of the reducing mill, and the outlet material diameter of the reducing mill. Use 3# and 4# water tanks before the reducing mill. The 3# water tank is cooled by 120℃, and the 4# water tank is cooled by 40℃. The temperature is returned to 800-900℃ before the reducing mill. S7, diameter measurement and closed-loop control with diameter gauge: The diameter gauge is set before the finishing mill, before the diameter reducing mill, and after the diameter reducing mill to detect the inlet size and outlet size of the diameter reducing mill in real time; S8, Spinning machine: After the diameter reduction, the 5# and 6# water cooling boxes cool down by 190℃, and then return to the temperature of 750-920℃ after reaching the spinning machine; S9, fan cooling: after spinning into a coil, the coil is cooled by air cooling line control; S10, Rolling and Collection: After being cooled by the fan of the air cooling line, the coils are collected and transported and cooled on the PF line. Finally, they are weighed, collected and stored after being bundled.
2. The high-strength and low-cost HRB600 spiral shell production method according to claim 1, It is characterized in that The components of the HRB600 coiled snail include, by mass percentage: C: 0.22-0.28%, Si: ≤0.65%, Mn: ≤1.45%, V: ≤0.050%, P: ≤0.040%, S: ≤0.040%, N: ≤0.010%, O: ≤28ppm, and the remainder is Fe and inevitable residual elements including but not limited to Ti, Nb, Cu, and Ni.
3. The high-strength and low-cost HRB600 spiral shell production method according to claim 1, It is characterized in that The billet size in step S1 is a square billet of 165×165×12000 mm, and the three heating temperatures are respectively controlled at 870°C-980°C, 980°C-1110°C, and 1070°C-1190°C, the uniform heating temperature of the billet in the heating furnace is controlled at 1100°C-1170°C, and the start rolling temperature is controlled at 980°C-1050°C.
4. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The average elongation coefficient of the rough rolling pass in step S2 is 1.373, the rough rolling entrance speed is 0.26 m / s, the rough rolling exit speed is 1.40 m / s, and the rough rolling exit material diameter is φ72 mm.
5. The high-strength and low-cost HRB600 spiral shell production method according to claim 1, It is characterized in that The average elongation coefficient of the intermediate rolling pass in step S3 is 1.310, the intermediate rolling temperature is 950°C, the intermediate rolling entrance speed is 1.40m / s, the intermediate rolling exit speed is 7.11m / s, and the intermediate rolling exit material diameter is φ32mm.
6. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The average elongation coefficient of the pre-finishing rolling pass in step S4 is 1.290, the pre-finishing rolling temperature is 1050°C, the pre-finishing rolling entrance speed is 7.11m / s, the pre-finishing rolling exit speed is 18.88m / s, and the pre-finishing rolling exit material diameter is φ19.2mm.
7. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The average elongation coefficient of the finishing pass in step S5 is 1.255, the finishing temperature is 850-950°C, the finishing entrance speed is 18.88m / s, the finishing exit speed is 29.26m / s, and the finishing exit material diameter is φ12.4mm.
8. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The average elongation coefficient of the diameter reducing pass in step S6 is 1.248, the temperature of the diameter reducing unit is 800-900°C, the inlet speed of the diameter reducing unit is 29.26m / s, the outlet speed of the diameter reducing unit is 68m / s, and the outlet material diameter of the diameter reducing unit is φ10mm.
9. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The diameter gauge in step S7 provides real-time feedback on the changes in the pre-finishing rolling and finishing rolling material shapes. When the pre-finishing rolling and finishing rolling material shapes fluctuate greatly, the diameter gauge can measure it in the first place and issue an early warning.
10. The high-strength and low-cost HRB600 Valve Snail production method according to claim 1, It is characterized in that The fan in step S9 includes a first section, a second section, a third section and a fourth section, the opening degree of the four sections of the fan is set to 60-80%, and the cooling speed of the four sections of the fan is: 19°C / s for the first section, 15°C / s for the second section, 7°C / s for the third section, and 2°C / s for the fourth section.
Citation Information
Patent Citations
HRB500 and HRB500E coiled reinforcing steel bar production process
CN103225043A
Coil production method and production line thereof
CN105665442A
Annular diameter measuring and temperature measuring instrument for bearing steel rolling control and cooling control
CN110404979A
Bar full-multiple-length system and control method
CN113000600A
High-efficiency low-cost 600MPa-grade high-strength anti-seismic coiled screw and production process thereof