Precoated sand precision casting waste sand recycling treatment method
Through the screening, pretreatment, drying and mixing of coated sand precision casting waste sand, the problem of low waste sand quality is solved, the reuse rate and production environmental protection are improved, and casting costs and energy consumption are reduced.
Patent Information
- Application Number
- CN202310796235.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-02
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing coating sand precision casting waste sand reuse technology, waste sand pretreatment is insufficient, resulting in low quality of recycled waste sand and affecting the quality of production products.
Using steps such as screening, pretreatment, drying, mixing and high-pressure water gun cleaning, treatment agents and degreasers are used to remove impurities and oil stains, and heat treatment is performed to improve the quality and reuse rate of waste sand.
It effectively improves the reuse rate of waste sand, reduces casting costs, reduces waste emissions and energy consumption, and improves the environmental benefits of the production process.
Smart Images

Figure BDA0004315195070000061 
Figure BDA0004315195070000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling foundry waste sand, and in particular to a method for recycling coated sand precision casting waste sand. Background Art
[0002] Coated sand is a new type of casting sand, commonly used in precision casting and foundry centers. Its sand surface is covered with a layer of white film, hence the name. This sand has good extrusion, pressure resistance and crack resistance, and can maintain good shape stability at high temperatures. The application of coated sand in the casting process is mainly in the production of high-precision, high-quality parts, such as automobile engine blocks, automobile steering gears, military equipment and other fields. However, due to its relatively high production cost, the waste generated by the sand needs to be reused to reduce costs and increase environmental benefits.
[0003] However, in the existing technology for recycling waste sand from coated sand precision casting, the pretreatment of waste sand from coated sand precision casting is poor. As a result, when the untreated waste sand from coated sand precision casting is recycled, the quality of the waste sand from coated sand precision casting is generally low. After mixing with new coated sand materials, the quality of the produced products is affected. Therefore, we proposed a method for recycling waste sand from coated sand precision casting. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a method for recycling waste sand from coated sand precision casting, which solves the problem of low quality of waste sand recovered from waste sand from coated sand precision casting in the prior art.
[0005] To achieve the above purpose, the present invention is implemented by the following technical scheme: a method for recycling waste sand from coated sand precision casting, comprising the following steps:
[0006] Step 1: Screening of waste sand
[0007] The waste sand is loaded into the screen side screening machine and screened;
[0008] Step 2: Pre-treat the screened waste sand
[0009] The waste sand is pre-treated by two treatment agents to remove its impurities;
[0010] Step 3: Sand drying
[0011] The screened coated sand is placed in a dryer and dried by the dryer;
[0012] Step 4: Sand mixing
[0013] Mix the dried waste sand, fresh quartz sand and resin together;
[0014] Step 5: Sand recovery and cleaning
[0015] Put the used coated sand into the high-pressure water gun for cleaning;
[0016] Step 6: Reuse sand.
[0017] Preferably, in step 2, the specific steps of pre-treating the waste sand are as follows:
[0018] S1, adding treatment agent 1 to the waste sand, stirring it by a stirring mechanism, and then standing it, and washing and draining the waste sand after pickling;
[0019] S2, adding treatment agent 2 to the waste sand after acid washing in step S1, stirring it by a stirring mechanism, and then standing it to wash and drain the waste sand after alkali washing;
[0020] S3, adding a degreasing agent to the waste sand treated in step S2 to remove oil stains in the waste sand;
[0021] S4, the waste sand treated in step S3 is transferred to the treated furnace for heat treatment, and the process is completed.
[0022] Preferably, in the step S1 and the step S2, the stirring speed of the stirring mechanism is 100 to 200 r / min, the stirring time is controlled at 5 to 10 min, and the standing time is 1 to 3 h.
[0023] Preferably, the treatment agent 1 includes the following raw materials in parts by weight: 20-30 parts of acidic substances, 50-80 parts of water, 2-3 parts of active agents, 2-5 parts of preservatives, 6-8 parts of surfactants, and 1-2 parts of auxiliary agents. The treatment agent 1 includes the following raw materials in parts by weight: 30-50 parts of alkaline substances, 40-70 parts of water, 2-3 parts of active agents, 1-4 parts of preservatives, 3-6 parts of surfactants, and 2-5 parts of auxiliary agents.
[0024] Preferably, the acidic substance is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid, and the mass ratio of the acidic substance to the treatment agent one is 1:3. In the step S2, the alkaline substance is selected from one or more of sodium hydroxide, sodium carbonate, potassium hydroxide and ethylenediaminetetraacetic acid, and the mass ratio of the alkaline substance to the treatment agent two is 1:4.
[0025] Preferably, in the step S4, the specific steps of the heat treatment are an annealing stage and a curing stage, the temperature of the annealing stage is controlled at 600° C. to 700° C., and the annealing time is controlled at 4 to 6 hours.
[0026] Preferably, in the curing stage, acetone resin is added to the waste sand, and the temperature in the curing stage is controlled at 130° C. to 180° C., and the curing time is controlled at 6 to 8 hours.
[0027] Preferably, in step three, the drying temperature of the dryer is 60° C. to 80° C., and the drying time is 40 to 80 min.
[0028] Preferably, in step 4, the specific steps of the sand material mixing process are as follows:
[0029] A. Place the dried sand and gravel in a mixer truck, add fresh quartz sand and resin into the mixer truck, and stir the mixture intermittently;
[0030] B. Carry out quality inspection on the sand mixed in step A.
[0031] Preferably, in step A, the stirring speed of the mixer truck is 80-150 r / min, the stirring time is controlled at 30-50 min, and the intermittent time is 5-8 min.
[0032] The present invention provides a method for recycling waste sand from coated sand precision casting, which has the following beneficial effects:
[0033] The present invention adds treatment agent 1, treatment agent 2 and degreasing agent to the waste sand of coated sand precision casting for cleaning, and heat-treats the waste sand of coated sand precision casting to effectively remove metal impurities, other non-metallic substances, grease, coating and thermosetting resin substances, thereby improving the reuse rate of waste sand and the quality of reused waste sand, reducing casting costs and saving the original cost of newly added casting sand, while reducing waste emissions in the casting production process, reducing pollution to the environment and reducing energy consumption required for casting production. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] Embodiment 1
[0036] The embodiment of the present invention provides a method for recycling waste sand from coated sand precision casting, comprising the following steps:
[0037] Step 1: Screening of waste sand
[0038] The waste sand is loaded into the screen side screening machine, and after screening, the waste sand is loaded into the screen side screening machine, and after screening, it is expanded, which can make full use of waste resources. In the process of waste sand screening, it is necessary to pay attention to the treatment method of waste sand raw materials to avoid waste sand impurities causing harm to equipment and workers' health;
[0039] Step 2: Pre-treat the screened waste sand
[0040] The waste sand is pretreated by two treatment agents to remove impurities. The specific steps of waste sand pretreatment are as follows:
[0041] S1. Add treatment agent 1 to the waste sand. The treatment agent 1 includes the following raw materials in parts by weight: 20 parts of acidic substance, 50 parts of water, 2 parts of active agent, 2 parts of preservative, 6 parts of surfactant, and 1 part of auxiliary agent. The acidic substance is hydrochloric acid. The mass ratio of the acidic substance to the treatment agent 1 is 1:3. Stir it through a stirring mechanism, then let it stand, and wash and drain the waste sand after pickling;
[0042] S2, adding treatment agent 2 to the waste sand after pickling in step S1, the treatment agent 2 comprises the following raw materials in parts by weight: 30 parts of alkaline substance, 40 parts of water, 2 parts of active agent, 1 part of preservative, 3 parts of surfactant, 2 parts of auxiliary agent, the alkaline substance is sodium hydroxide, the mass ratio of the alkaline substance to the treatment agent 2 is 1:4, stirring it by a stirring mechanism, and then standing it, and washing and draining the waste sand after alkali washing;
[0043] S3, adding a degreasing agent to the waste sand treated in step S2 to remove oil stains in the waste sand;
[0044] S4, the waste sand treated in step S3 is transferred to the treated furnace for heat treatment, that is, the specific steps of the heat treatment are annealing stage and curing stage, the temperature of the annealing stage is controlled at 600°C, the annealing time is controlled at 6h, in the curing stage, acetone resin is added to the waste sand, and the temperature of the curing stage is controlled at 180°C, and the curing time is controlled at 8h;
[0045] The stirring speed of the stirring mechanism is 200r / min, the stirring time is controlled at 10min, and the standing time is 3h;
[0046] Step 3: Sand drying
[0047] Put the screened coated sand into the dryer and dry it in the dryer. The drying temperature of the dryer is 80℃ and the drying time is 80min.
[0048] Step 4: Sand mixing
[0049] Mix the dried waste sand, fresh quartz sand and resin together. In step 4, the specific steps of sand mixing are as follows:
[0050] A. Place the dried sand and gravel in a mixer truck, add fresh quartz sand and resin into the mixer truck, and stir the mixture intermittently. The stirring speed of the mixer truck is 150r / min, the stirring time is controlled at 50min, and the intermittent time is 8min;
[0051] B. Conduct quality inspection on the sand mixed in step A;
[0052] Step 5: Sand recovery and cleaning
[0053] Put the used coated sand into the high-pressure water gun for cleaning;
[0054] Step 6: Reuse of sand. Reuse of sand can reduce the amount of original sand used, thereby effectively reducing production costs and reducing the impact of sand on the environment during the production process. It can give full play to its potential value, reduce resource waste, and reduce the energy consumed in the collection and processing of raw materials, thereby reducing energy consumption.
[0055] Embodiment 2:
[0056] This embodiment is different from the embodiment 1 in that the treatment agent and the treatment agent 2 have different weight parts, specifically: the treatment agent 1 includes the following raw materials in weight parts: 25 parts of acidic substance, 55 parts of water, 2.5 parts of active agent, 3 parts of preservative, 7 parts of surfactant, 2 parts of auxiliary agent, and the acidic substance is sulfuric acid;
[0057] The treatment agent 2 includes the following raw materials in parts by weight: 40 parts of alkaline substance, 60 parts of water, 3 parts of active agent, 4 parts of preservative, 5 parts of surfactant, and 4 parts of auxiliary agent. The alkaline substance is sodium carbonate.
[0058] Embodiment three:
[0059] This embodiment is different from the first embodiment in that the treatment agent and the second treatment agent have different weight parts, specifically: the first treatment agent includes the following raw materials in weight parts: 28 parts of acidic substance, 70 parts of water, 3 parts of active agent, 3 parts of preservative, 7 parts of surfactant, 1.5 parts of auxiliary agent, and the acidic substance is nitric acid;
[0060] Treatment agent 2 includes the following raw materials in parts by weight: 45 parts of alkaline substance, 65 parts of water, 2.5 parts of active agent, 3 parts of preservative, 5 parts of surfactant, 4 parts of auxiliary agent, and the alkaline substance is potassium hydroxide.
[0061] Embodiment 4:
[0062] This embodiment is different from the embodiment 1 in that the treatment agent and the treatment agent 2 have different weight parts, specifically: the treatment agent 1 includes the following raw materials in weight parts: 30 parts of acidic substance, 80 parts of water, 3 parts of active agent, 5 parts of preservative, 8 parts of surfactant, 2 parts of auxiliary agent, and the acidic substance is hydrofluoric acid;
[0063] The treatment agent 2 includes the following raw materials in parts by weight: 50 parts of alkaline substances, 70 parts of water, 3 parts of active agents, 4 parts of preservatives, 6 parts of surfactants, and 5 parts of auxiliary agents. The alkaline substance is ethylenediaminetetraacetic acid.
[0064] Experimental example:
[0065] The parameters of Example 1, Example 2, Example 3 and Example 4 were taken respectively, and the metal impurity residual rate, other non-metallic substance residual rate, grease residual rate, thermosetting resin residual rate, waste sand quality and energy consumption of the waste sand recycled by the coated sand precision casting were statistically analyzed. The results are shown in Table 1:
[0066]
[0067]
[0068] Table 1
[0069] As can be seen from Table 1, by adding treatment agent 1, treatment agent 2 and degreasing agent to the coated sand precision casting waste sand for cleaning, and by heat treating the coated sand precision casting waste sand, metal impurities, other non-metallic substances, grease, coating, thermosetting resin substances are effectively removed, the reuse rate of waste sand and the quality of recycled waste sand are improved, and on the other hand, the casting cost is reduced, the original cost of additional casting sand is saved, and at the same time, waste emissions in the casting production process are reduced, pollution to the environment is reduced, and the energy consumption required for casting production is reduced. At the same time, Example 3 is the optimal solution.
[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for recycling waste sand from coated sand precision casting, characterized in that: The following steps are involved: Step 1: Screening of waste sand The waste sand is loaded into the screen side screening machine and screened; Step 2: Pre-treat the screened waste sand The waste sand is pre-treated by two treatment agents to remove its impurities; Step 3: Sand drying The screened coated sand is placed in a dryer and dried by the dryer; Step 4: Sand mixing Mix the dried waste sand, fresh quartz sand and resin together; Step 5: Sand recovery and cleaning Put the used coated sand into the high-pressure water gun for cleaning; Step 6: Reuse sand.
2. The method for recycling waste sand from coated sand precision casting according to claim 1 is characterized in that: In the step 2, the specific steps of the waste sand pretreatment are as follows: S1, adding treatment agent 1 to the waste sand, stirring it by a stirring mechanism, and then standing it, and washing and draining the waste sand after pickling; S2, adding treatment agent 2 to the waste sand after acid washing in step S1, stirring it by a stirring mechanism, and then standing it to wash and drain the waste sand after alkali washing; S3, adding a degreasing agent to the waste sand treated in step S2 to remove oil stains in the waste sand; S4, the waste sand treated in step S3 is transferred to the treated furnace for heat treatment, and the process is completed.
3. The method for recycling waste sand from coated sand precision casting according to claim 2 is characterized in that: In the step S1 and the step S2, the stirring speed of the stirring mechanism is 100 to 200 r / min, the stirring time is controlled at 5 to 10 min, and the standing time is 1 to 3 h.
4. The method for recycling waste sand from coated sand precision casting according to claim 2 is characterized in that: The treatment agent 1 includes the following raw materials in parts by weight: 20-30 parts of acidic substances, 50-80 parts of water, 2-3 parts of active agents, 2-5 parts of preservatives, 6-8 parts of surfactants, and 1-2 parts of auxiliary agents. The treatment agent 2 includes the following raw materials in parts by weight: 30-50 parts of alkaline substances, 40-70 parts of water, 2-3 parts of active agents, 1-4 parts of preservatives, 3-6 parts of surfactants, and 2-5 parts of auxiliary agents.
5. The method for recycling waste sand from coated sand precision casting according to claim 4 is characterized in that: The acidic substance is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid, and the mass ratio of the acidic substance to the treatment agent one is 1:
3. In the step S2, the alkaline substance is selected from one or more of sodium hydroxide, sodium carbonate, potassium hydroxide and ethylenediaminetetraacetic acid, and the mass ratio of the alkaline substance to the treatment agent two is 1:
4.
6. The method for recycling waste sand from coated sand precision casting according to claim 2 is characterized in that: In the step S4, the specific steps of the heat treatment are an annealing stage and a curing stage. The temperature of the annealing stage is controlled at 600° C. to 700° C., and the annealing time is controlled at 4 to 6 hours.
7. The method for recycling waste sand from coated sand precision casting according to claim 3 is characterized in that: In the curing stage, acetone resin is added to the waste sand, and the temperature of the curing stage is controlled at 130° C. to 180° C., and the curing time is controlled at 6 to 8 hours.
8. The method for recycling waste sand from coated sand precision casting according to claim 1, characterized in that: In the step three, the drying temperature of the dryer is 60° C. to 80° C., and the drying time is 40 to 80 minutes.
9. The method for recycling waste sand from coated sand precision casting according to claim 1, characterized in that: In step 4, the specific steps of the sand material mixing process are as follows: A. Place the dried sand and gravel in a mixer truck, add fresh quartz sand and resin into the mixer truck, and stir the mixture intermittently; B. Carry out quality inspection on the sand mixed in step A.
10. The method for recycling waste sand from coated sand precision casting according to claim 9, characterized in that: In the step A, the stirring speed of the stirring truck is 80-150 r / min, the stirring time is controlled at 30-50 min, and the interval time is 5-8 min.